Method for treating scheelite heating cleaner tailings by using CO2-containing boiler tail gas
By reacting the boiler tailings containing CO2 and syringe tungsten warming selected tailings, co-precipitated granules were generated and flotation was flotation using sodium oleate and dwarf flotation columns, the wastewater in syringe tailings treatment was solved. It is difficult to reuse the wastewater in syringe tailings treatment. The problem of efficient wastewater treatment and carbon capture is achieved, reducing treatment costs and greenhouse gas emissions.
Patent Information
- Application Number
- CN202410974383.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
Smart Images

Figure CN118904888A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for treating flotation tailings with CO2, and in particular to a method for treating scheelite heated tailings by using boiler tail gas containing CO2. Background Art
[0002] Heating concentration is the most commonly used process for treating scheelite with high calcium gangue content. It uses the difference in the speed of water glass desorption of scheelite and collector on the surface of calcium gangue at high temperature to expand the floatability difference between different calcium-containing minerals, thereby obtaining high-quality scheelite concentrate. This process consumes a large amount of water glass, resulting in an increase in the pH value of scheelite tailings and a large amount of silicate, making it difficult for the tailings to settle and the wastewater to be reused.
[0003] At present, the main treatment methods for silicon-containing alkaline wastewater are: ① Chemical precipitation: by adding chemical reagents such as sulfuric acid, calcium chloride, quicklime, etc., the pH value of the wastewater is reduced to form silicate precipitation, and then separated by precipitation. ② Ion exchange: Use ion exchange resin to remove silicon and other impurities in wastewater. ③ Membrane separation technology: Use membrane separation technology such as nanofiltration or reverse osmosis to effectively remove silicon and other dissolved components in wastewater. ④ Biological treatment: For some organosilicon wastewater, biological treatment can be used to use microorganisms to decompose organosilicon. ⑤ Deep treatment: After preliminary treatment, deep treatment technologies such as activated carbon adsorption and ozone oxidation can be used to further purify the wastewater. Based on treatment cost and treatment effect, chemical precipitation is widely used in the treatment of industrial silicon-containing alkaline wastewater.
[0004] In industrial production, acid or lime is often used to treat heated tailings of scheelite. The large consumption of acid or lime has greatly increased the cost of recycling and processing, bringing pressure to enterprises. As an important measure for my country to cope with climate change, the "dual carbon" policy has always lacked an efficient and low-cost carbon capture process to reduce greenhouse gas emissions and mitigate the serious impact of global warming. Conventional carbon capture processes include afforestation, underground storage, seabed storage, carbon conversion technology, etc., which currently have problems such as low carbon capture efficiency and long distance from industrial application. Summary of the invention
[0005] In view of the above problems existing in the prior art, the purpose of the present invention is to provide a method for treating scheelite heating and concentrating tailings using boiler tail gas containing CO2. This method uses CO2 in industrial tail gas to treat scheelite heating and concentrating tailings, which can not only reduce the cost of wastewater treatment, but also achieve carbon capture, helping to achieve the "dual carbon" goal.
[0006] In order to achieve the above technical objectives, the present invention provides the following technical solutions:
[0007] The present invention provides a method for treating scheelite heated tailings by using boiler tail gas containing CO2, comprising the following steps:
[0008] 1) Pump the heated and concentrated tailings of scheelite into the primary sedimentation tank for sedimentation to obtain sediment and overflow; then discharge the sediment into the tailings pond and the overflow into the reaction container;
[0009] 2) The boiler tail gas containing CO2 is pressurized to make the tail gas pressure P ≥ 25psi, and then pumped into the reaction vessel to fully react with the overflow. During the reaction, the overflow water is stirred to generate co-precipitated particles;
[0010] 3) After the reaction is completed, sodium oleate is added to the reaction vessel to improve the hydrophobicity of the co-precipitated particles, and then the co-precipitated particles are pneumatically floated out and discharged into the tailings pond using a dwarf flotation column. The tailings discharged from the flotation column are the treated tailings water, which is returned to the heating and concentration system for recycling.
[0011] In step 1), the overflow has a high pH value and contains a large amount of suspended solids that are difficult to settle, silicate, calcium and magnesium ions, and other impurities.
[0012] Preferably, in step 2), the boiler tail gas containing CO2 is pressurized by a pressure pump to increase the pressure of the tail gas to 25-600 psi. Pressurizing the tail gas can increase the reaction rate of CO2 with silicate, hydroxide and calcium and magnesium ions in the overflow, increase the reaction depth, and make the wastewater treatment more efficient. However, too high a pressure has little effect on improving the reaction efficiency and increases the processing cost.
[0013] Preferably, in step 2), during the process of the CO2-containing boiler tail gas fully reacting with the overflow, the CO2 in the tail gas dissolves in water to form carbonic acid, and then gradually dissociates into hydrogen ions and carbonate ions, and the hydrogen ions react with the hydroxide ions in the overflow to neutralize, thereby reducing the pH value of the overflow; further, the hydrogen ions react with the silicate ions in the overflow to form silicate colloid; the carbonate ions react with the calcium ions and magnesium ions in the overflow to form carbonate precipitates; under the bridging effect of the silicate colloid, the silicate colloid and the carbonate precipitate as well as other suspended matter and metal ions in the overflow form co-precipitated particles.
[0014] Preferably, in step 2), the reaction time is 10 to 35 minutes.
[0015] Preferably, in step 2), the overflow water is stirred at a stirring speed of 30 to 90 r / min.
[0016] Preferably, in step 3), the amount of sodium oleate added is 600 to 2000 g / m 3 (g / m 3 The drug is relative to 1m 3 overflow addition amount).
[0017] Preferably, in step 3), the diameter-to-height ratio of the dwarfed flotation column is 1:3 to 1:7.5; the air inlet pressure range of the flotation column during the flotation process is 0.2 to 0.4 MPa. The use of air flotation can speed up the treatment efficiency of wastewater. The use of dwarfed flotation columns can avoid the formation of short-circuit flow in the column, which makes it difficult for some particles in the wastewater to float out, reduces the treatment effect, and affects reuse. The air inlet pressure of the flotation column is maintained within a reasonable range. If the air pressure is too low, the co-precipitated particles will be difficult to float, and if the air pressure is too high, the co-precipitated particles will easily be dispersed.
[0018] The present invention can process the tailings of scheelite by heating and concentration, and at the same time, realize carbon capture and rapid treatment and reuse of the concentrated wastewater. Its main principle is:
[0019] 1. pH value adjustment: After the primary sedimentation separates the easily settleable particles in the tailings, the pressurized CO2-containing boiler tail gas is introduced into the tailings overflow water containing a large amount of suspended matter, silicate and high alkalinity to form carbonic acid (H2CO3). Carbonic acid can react with the alkaline components in the wastewater to reduce the pH value of the water, thereby neutralizing the excessive alkalinity.
[0020] 2. Formation of carbonate precipitation: As the pH value decreases, the silicate dissolved in the water will react with the hydrogen ions dissociated from the carbonate to form silicate colloid. The dissociated carbonate reacts with the calcium ions and magnesium ions to form calcium carbonate (CaCO3) and magnesium carbonate (MgCO3) precipitation, removing the inevitable ions in the wastewater. This process can also help remove other harmful substances in the wastewater, such as heavy metal ions, because these substances can also precipitate with the generated carbonate; under the bridging effect of silicate colloid, silicate colloid forms co-precipitated particles with carbonate precipitate and other suspended matter and metal ions.
[0021] 3. Fast treatment cycle: The flotation method is used to overcome the problem of slow natural sedimentation of silicon-containing wastewater. Sodium oleate is added to enhance the hydrophobicity of the surface of the co-precipitated particles, and then the dwarf flotation column is used to quickly separate the co-precipitated particles under appropriate air pressure.
[0022] Compared with the prior art, the advantages of the present invention are:
[0023] In the present invention, the tail gas containing CO2 discharged from the boiler during the heating and selection process of scheelite is introduced into the reaction container through a pressure pump to interact with the tailings wastewater (mainly silicon-containing alkaline wastewater containing fine suspended matter) after primary precipitation. CO2 dissolves in water to form carbonic acid, consuming OH in the wastewater. - , reducing the alkalinity of wastewater; CO3 released by carbonic acid dissociation 2- With Ca in water 2+ Mg 2+ The reaction forms carbonate precipitation, which reduces the hardness of the tailings wastewater; the dissociated H +With SiO3 2- Combined to form silica colloid, silica colloid through bridging effect to make carbonate and fine suspended matter co-precipitate. Finally, the precipitate is quickly pneumatically floated out through the dwarf flotation column to reduce the hardness and alkalinity of the tailings wastewater, remove silicate ions and suspended matter, and achieve the purpose of continued reuse of the tailings wastewater; at the same time, CO2 fixation is achieved, greenhouse gas emissions are reduced, and conventional treatment processes such as lime method and acid addition method for silicon-containing alkaline wastewater are replaced, reducing wastewater treatment costs, and treating waste with waste, which is green and efficient. In addition, the operation process of this method is relatively simple, and it is also combined with the flotation method to accelerate the rapid separation of difficult-to-sediment substances in the tailings, thereby improving the treatment efficiency of scheelite tailings. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The process flow chart for treating scheelite tailings by heating and concentrating using boiler tail gas containing CO2;
[0025] Figure 2 Schematic diagram of dwarf flotation column. DETAILED DESCRIPTION
[0026] The present invention uses the CO2-containing tail gas generated by the boiler during the process of heating and concentrating scheelite to treat the tailings of heating and concentrating scheelite, and compares the implementation effects of the invention under different conditions. The CO2-containing tail gas generated by the boiler here refers to the tail gas emitted by burning natural gas.
[0027] Example 1
[0028] 1) Pump the heated and concentrated tailings of scheelite into the primary sedimentation tank for sedimentation to obtain sedimentation and overflow; after testing, the Si content in the overflow is 6450ppm, the Ca+Mg content is 590ppm, and the pH is 13.70;
[0029] The CO2-containing tail gas produced by the boiler during the heating and selection process of scheelite is introduced into the pressure pump to pressurize the tail gas and increase the pressure of the tail gas to 25psi.
[0030] 2) The pressurized tail gas is pumped into the reaction vessel to fully react with the overflow water of the heated and concentrated tailings of the scheelite after primary precipitation. The overflow water is stirred during the reaction at a stirring speed of 60 r / min and a reaction time of 30 min to generate co-precipitated particles;
[0031] 3) After the reaction is completed, add 2000g / m 3 The sodium oleate is added to improve the hydrophobicity of the coprecipitated particles, and then the coprecipitated particles are quickly pneumatically floated out and discharged into the tailings pond using a dwarf flotation column (diameter-height ratio D:H=1:3). The tailings discharged from the flotation column are the treated tailings water, which is returned to the heating and concentration system for recycling. During the flotation process, the air inlet pressure of the flotation column is 0.4MPa. The treatment results are shown in Table 1.
[0032] Table 1 Comparison of different treatment effects
[0033] Treatment process Si content / ppm Hardness (Ca+Mg) / ppm pH Overflow (raw water) 6450 590 13.70 Example 1 26 53 7.15 <![CDATA[Add H2SO4 (Comparative Example 1)]]> 25 552 6.04 Add quicklime (Comparative Example 2) 390 407 11.88
[0034] As shown in Table 1, Example 1 achieved the best treatment effect, not only removing most of the silicate, but also effectively reducing the hardness of the tailings water, and the pH of the slurry was close to the natural pH of water. However, the traditional treatment method, such as adding sulfuric acid, could not remove the inevitable ions, and the final pH was low; adding quicklime had the worst effect on the removal of silicate, and the return water still maintained a high pH.
[0035] Example 2
[0036] 1) Pump the heated tailings of scheelite into the primary sedimentation tank for sedimentation to obtain sedimentation and overflow; after testing, the Si content in the overflow is 4623ppm, the Ca+Mg content is 678ppm, and the pH is 12.97;
[0037] The CO2-containing tail gas produced by the boiler during the heating and selection process of scheelite is introduced into the pressure pump to pressurize the tail gas and increase the pressure of the tail gas to 100psi.
[0038] 2) The pressurized tail gas is pumped into the reaction vessel to fully react with the overflow water of the scheelite tailings after primary precipitation. During the reaction, the overflow water is stirred at a stirring speed of 30r / min and a reaction time of 10min to generate co-precipitated particles;
[0039] 3) After the reaction is completed, add 600g / m 3 The sodium oleate is added to improve the hydrophobicity of the coprecipitated particles, and then the coprecipitated particles are quickly pneumatically floated out and discharged into the tailings pond using a dwarf flotation column (diameter-to-height ratio D:H=1:7.5). The tailings discharged from the flotation column are the treated tailings water, which is returned to the heating and concentration system for recycling. During the flotation process, the air inlet pressure of the flotation column is 0.2MPa. The treatment results are shown in Table 2.
[0040] Example 3
[0041] This embodiment is basically the same as embodiment 2, except that the tail gas pressure is 300 psi. The treatment results are shown in Table 2.
[0042] Example 4
[0043] This embodiment is basically the same as embodiment 2, except that the tail gas pressure is 600 psi. The treatment results are shown in Table 2.
[0044] Table 2 Comparison of the effects of different exhaust pressures
[0045]
[0046] As shown in Table 2, if the exhaust gas discharged from the boiler is not pressurized, its treatment efficiency will be greatly reduced. If the exhaust pressure is further increased after reaching a certain pressure, the effect of improving the treatment effect is not obvious.
[0047] Example 5
[0048] 1) Pump the heated scheelite tailings into the primary sedimentation tank for sedimentation to obtain sedimentation and overflow; after testing, the Si content in the overflow was 5135ppm, the Ca+Mg content was 459ppm, and the pH was 13.02;
[0049] The CO2-containing tail gas generated by the boiler during the heating and selection of scheelite is introduced into the pressure pump to pressurize the tail gas to increase the pressure of the tail gas to 50psi;
[0050] 2) The pressurized tail gas is pumped into the reaction vessel to fully react with the overflow water of the scheelite tailings after primary precipitation. The overflow water is stirred during the reaction at a stirring speed of 30r / min and a reaction time of 15min to generate co-precipitated particles;
[0051] 3) After the reaction is completed, add 1200g / m 3 The sodium oleate is added to improve the hydrophobicity of the coprecipitated particles, and then the coprecipitated particles are quickly pneumatically floated out and discharged into the tailings pond using a dwarf flotation column (diameter-to-height ratio D:H=1:6). The tailings discharged from the flotation column are the treated tailings water, which is returned to the heating and concentration system for recycling. During the flotation process, the air inlet pressure of the flotation column is 0.3MPa. The treatment results are shown in Table 3.
[0052] Example 6
[0053] This embodiment is substantially the same as embodiment 5, except that the reaction time is 25 min. The treatment results are shown in Table 3.
[0054] Example 7
[0055] This embodiment is substantially the same as embodiment 5, except that the reaction time is 35 min. The treatment results are shown in Table 3.
[0056] Table 3 Comparison of effects of different reaction times
[0057]
[0058] It can be seen from Table 3 that when the reaction time is insufficient, a large amount of silicate and calcium and magnesium ions remain. When the reaction time of the exhaust gas exceeds 15 minutes, the reaction time of the exhaust gas and the overflow water is further extended, and the treatment effect is basically the same.
[0059] Example 8
[0060] 1) Pump the heated tailings of scheelite into the primary sedimentation tank for sedimentation to obtain sedimentation and overflow; after testing, the Si content in the overflow is 5043ppm, the Ca+Mg content is 705ppm, and the pH is 12.97;
[0061] The CO2-containing tail gas produced by the boiler during the heating and selection process of scheelite is introduced into the pressure pump to pressurize the tail gas and increase the pressure of the tail gas to 100psi.
[0062] 2) The pressurized tail gas is pumped into the reaction vessel to fully react with the overflow water of the scheelite tailings after primary precipitation. During the reaction, the overflow water is stirred at a stirring speed of 30r / min and a reaction time of 10min to generate co-precipitated particles;
[0063] 3) After the reaction is completed, add 1000g / m 3 The sodium oleate is added to improve the hydrophobicity of the coprecipitated particles, and then the coprecipitated particles are quickly pneumatically floated out and discharged into the tailings pond using a dwarf flotation column (diameter-to-height ratio D:H=1:7.5). The tailings discharged from the flotation column are the treated tailings water, which is returned to the heating and concentration system for recycling. During the flotation process, the air inlet pressure of the flotation column is 0.4MPa. The treatment results are shown in Table 4.
[0064] Example 9
[0065] This embodiment is basically the same as embodiment 8, the only difference being that the stirring speed is 60 r / min. The treatment results are shown in Table 4.
[0066] Example 10
[0067] This embodiment is basically the same as embodiment 8, the only difference being that the stirring speed is 90 r / min. The treatment results are shown in Table 4.
[0068] Table 4 Comparison of the effects of different stirring speeds
[0069]
[0070] It can be seen from Table 4 that when there is no stirring, the calcium ions, magnesium ions and silicate ions do not react thoroughly and there is still a lot of residue. When the stirring speed is increased to 30r / min, the effect of the treatment is not obvious if the stirring speed is further increased.
[0071] Embodiment 11
[0072] 1) Pump the heated tailings of scheelite into the primary sedimentation tank for sedimentation to obtain sedimentation and overflow; after testing, the Si content in the overflow is 5781ppm, the Ca+Mg content is 811ppm, and the pH is 13.74;
[0073] The CO2-containing tail gas generated by the boiler during the heating and selection of scheelite is introduced into the pressure pump to pressurize the tail gas to increase the pressure of the tail gas to 50psi;
[0074] 2) The pressurized tail gas is pumped into the reaction vessel to fully react with the overflow water of the scheelite tailings after primary precipitation. During the reaction, the overflow water is stirred at a stirring speed of 45r / min and a reaction time of 15min to generate co-precipitated particles;
[0075] 3) After the reaction is completed, add 800g / m 3 The sodium oleate is added to improve the hydrophobicity of the coprecipitated particles, and then the coprecipitated particles are quickly pneumatically floated out and discharged into the tailings pond using a dwarf flotation column (diameter-height ratio D:H=1:7.5). The tailings discharged from the flotation column are the treated tailings water, which is returned to the heating and concentration system for recycling. During the flotation process, the air inlet pressure of the flotation column is 0.3MPa. The treatment results are shown in Table 5.
[0076] Example 12
[0077] This embodiment is basically the same as embodiment 11, except that the amount of sodium oleate used is 1200 g / m 3 The processing results are shown in Table 5.
[0078] Table 5 Comparison of the effects of different sodium oleate dosages
[0079]
[0080] As shown in Table 5, when sodium oleate is not added, the coprecipitated particles are difficult to float effectively and are still dispersed in the overflow water; when the amount of sodium oleate is insufficient, some coprecipitated particles still remain in the overflow water, and the treatment effect is still not ideal. When the amount of sodium oleate exceeds the appropriate amount, the treatment effect is not further improved. Since sodium oleate is alkaline, the pH at the end of the flotation column is slightly increased.
[0081] Embodiment 13
[0082] 1) Pump the heated tailings of scheelite into the primary sedimentation tank for sedimentation to obtain sedimentation and overflow; after testing, the Si content in the overflow is 6081ppm, the Ca+Mg content is 676ppm, and the pH is 13.23;
[0083] The CO2-containing tail gas produced by the boiler during the heating and selection process of scheelite is introduced into the pressure pump to pressurize the tail gas and increase the pressure of the tail gas to 100psi.
[0084] 2) The pressurized tail gas is pumped into the reaction vessel to fully react with the overflow water of the scheelite tailings after primary precipitation. During the reaction, the overflow water is stirred at a stirring speed of 30r / min and a reaction time of 10min to generate co-precipitated particles;
[0085] 3) After the reaction is completed, add 1200g / m 3 The sodium oleate was added to improve the hydrophobicity of the coprecipitated particles, and then the coprecipitated particles were quickly pneumatically floated out and discharged into the tailings pond using a dwarf flotation column (diameter-height ratio D:H=1:7.5). The tailings discharged from the flotation column were the treated tailings water, which was returned to the heating and concentration system for recycling. During the flotation process, the air inlet pressure of the flotation column was 0.4MPa. The treatment results are shown in Table 6.
[0086] Table 6 Comparison of the effects of flotation columns with different diameter-to-height ratios
[0087]
[0088] It can be seen from Table 6 that when the diameter height of the flotation column is relatively small, a short-circuit flow is formed inside the column, and a small amount of co-precipitated particles will still remain in the flotation column and flow out with the tail when they accumulate to a certain extent; when the diameter height is relatively large, the flotation column loses its sorting effect, and a large amount of co-precipitated particles cannot flow out with the upwelling of the airflow in time, but remain in the flotation column and flow out with the tail.
[0089] Embodiment 14
[0090] 1) Pump the heated and concentrated tailings of scheelite into the primary sedimentation tank for sedimentation to obtain sedimentation and overflow; after testing, the Si content in the overflow was 4757ppm, the Ca+Mg content was 623ppm, and the pH was 13.19;
[0091] The CO2-containing tail gas produced by the boiler during the heating and selection process of scheelite is introduced into the pressure pump to pressurize the tail gas and increase the pressure of the tail gas to 80psi.
[0092] 2) The pressurized tail gas is pumped into the reaction vessel to fully react with the overflow water of the scheelite tailings after primary precipitation. The overflow water is stirred during the reaction at a stirring speed of 30r / min and a reaction time of 15min to generate co-precipitated particles;
[0093] 3) After the reaction is completed, add 800g / m 3 The sodium oleate is added to improve the hydrophobicity of the coprecipitated particles, and then the coprecipitated particles are quickly pneumatically floated out and discharged into the tailings pond using a dwarf flotation column (diameter-to-height ratio D:H=1:7.5). The tailings discharged from the flotation column are the treated tailings water, which is returned to the heating and concentration system for recycling. During the flotation process, the air inlet pressure of the flotation column is 0.4MPa. The treatment results are shown in Table 7.
[0094] Table 7 Comparison of the effects of different flotation column inlet pressures
[0095]
[0096] It can be seen from Table 7 that when the air inlet pressure of the flotation column is high, some co-precipitates that are not tightly bound are dispersed and remain in the flotation column, resulting in a decrease in the treatment effect; and when the air inlet pressure of the flotation column is insufficient, some large-sized co-precipitate particles will also remain in the flotation column.
Claims
1. A method for treating scheelite heated tailings using boiler tail gas containing CO2, comprising the following steps: 1) Pump the heated and concentrated tailings of scheelite into the primary sedimentation tank for sedimentation to obtain sediment and overflow; then discharge the sediment into the tailings pond and the overflow into the reaction container; 2) The boiler tail gas containing CO2 is pressurized to make the tail gas pressure P ≥ 25psi, and then pumped into the reaction vessel to fully react with the overflow. During the reaction, the overflow water is stirred to generate co-precipitated particles; 3) After the reaction is completed, sodium oleate is added to the reaction vessel to improve the hydrophobicity of the co-precipitated particles, and then the co-precipitated particles are pneumatically floated out and discharged into the tailings pond using a dwarf flotation column; the tailings discharged from the flotation column are the treated tailings water, which is returned to the heating and concentration system for recycling.
2. The method according to claim 1, characterized in that In step 2), the boiler tail gas containing CO2 is pressurized by a pressure pump to increase the pressure of the tail gas to 25-600 psi.
3. The method according to claim 1, characterized in that In step 2), the reaction time is 10 to 35 minutes.
4. The method according to claim 1, characterized in that: In step 2), the overflow water is stirred at a stirring speed of 30 to 90 r / min.
5. The method according to claim 1, characterized in that In step 2), during the process of the boiler tail gas containing CO2 fully reacting with the overflow, the CO2 in the tail gas dissolves in water to form carbonic acid, and then gradually dissociates into hydrogen ions and carbonate ions, and the hydrogen ions react with the hydroxide ions in the overflow to neutralize, thereby reducing the pH value of the overflow; further, the hydrogen ions react with the silicate ions in the overflow to form silicate colloid; the carbonate ions react with the calcium ions and magnesium ions in the overflow to form carbonate precipitates; under the bridging effect of the silicate colloid, the silicate colloid and the carbonate precipitate as well as other suspended matter and metal ions in the overflow form co-precipitated particles.
6. The method according to claim 1, characterized in that In step 3), the amount of sodium oleate added is 600-2000 g / m 3 .
7. The method according to claim 1, characterized in that In step 3), the diameter-to-height ratio of the dwarfed flotation column is 1:3 to 1:7.
5.
8. The method according to claim 1, characterized in that In step 3), the air inlet pressure range of the flotation column during the flotation process is 0.2-0.4 MPa.
Citation Information
Patent Citations
Oil sands tailings treatment process
CA2188064A1
Method for synergic oxidation treatment of wastewater containing organics and heavy metal generated in mining and mineral separation
CN104478160A
Wolframine beneficiation wastewater treatment process
CN105254069A
Aluminum bauxite flotation method
CN108452941A
Lead-zinc ore dressing wastewater treatment and recycling device and method thereof
CN109437448A
Cited By
Method and system for recovering tungsten from scheelite heating concentration tailings
CN121945311A
Method and system for recovering tungsten from scheelite warming cleaning tailings
CN121945311B