Flux-cored wire containing rare earth metal slag and gas combined protection and application of flux-cored wire
By using flux-core welding wire containing rare earth metal slag gas combined protection in the welding of X80 pipeline steel, hydrogen embrittlement damage and fracture failure problems are solved, the hydrogen resistance and fracture toughness of the weld are improved, and the efficiency of welding is achieved. stability.
Patent Information
- Application Number
- CN202411005654.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
X80 pipeline steel is prone to hydrogen embrittlement damage and fracture failure problems in high pressure and corrosive environments, and existing welding wires have failed to effectively improve their hydrogen resistance and fracture toughness.
Flux-core welding wire with combined protection of rare earth metal slag gas is used to adjust the slag-forming agent formula and alloy element composition to form fluorite and rutile as the main slag system, Si-Mn-Mo-Ni as the main alloy element, and rare earth elements are added , realize joint protection of slag gas, and improve the hydrogen resistance and fracture toughness of the weld.
This welding wire achieves high strength, low diffusion hydrogen content and good process performance of weld metal in the welding of X80 pipeline steel. The weld surface is smooth and there is no large particle splash, and it is suitable for ring weld welding of X80 pipeline steel.
Smart Images

Figure CN118905496A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal material welding, and in particular relates to a rare earth metal-containing slag gas combined protection flux-cored welding wire and application thereof, and is particularly suitable for welding of X80 pipeline steel ring welds. Background Art
[0002] As the safest, most reliable and economical way to transport oil and natural gas over long distances, the construction and operation of oil and gas pipelines have achieved rapid development. In the construction of long-distance pipelines, in order to improve transportation efficiency and reduce construction costs, X80 pipeline steel with high strength and good toughness is usually used as the preferred pipe material for pipeline construction.
[0003] Oil and gas pipelines have been in service for a long time in high pressure and corrosive environments, and it is inevitable that the corrosive media in the environment will cause material corrosion failure. Among them, the hydrogen embrittlement damage and failure of materials caused by the introduction of hydrogen atoms are relatively more serious. On the one hand, the transportation environment of oil and gas pipelines contains a large amount of hydrogen-containing media. On the other hand, the extensive use of cathodic protection technology inevitably produces hydrogen evolution effect on the metal surface, which leads to the frequent occurrence of related damage and fracture failure caused by the introduction of hydrogen atoms in oil and gas pipeline steel, posing a serious threat to human life and property safety. At present, X80 pipeline steel often uses gas-shielded flux-cored wire without slag, but the slag can support the molten pool during welding, making it difficult for the molten pool to flow when welding in the vertical welding position, thereby optimizing the weld formation. At the same time, the deoxidation of the slag-forming components during the welding process can protect the alloy elements from smoothly transitioning into the weld, thereby improving the overall performance of the weld. The added rare earth elements can effectively refine the grains, improve the toughness and hydrogen resistance of the weld.
[0004] Therefore, the development of slag gas combined shielded flux-cored welding wire with added rare earth elements for X80 pipeline steel has important engineering practical significance and scientific research significance.
[0005] 202110105191.8 discloses a high-toughness gas-shielded flux-cored welding wire for X80 pipeline steel. The alloy system used in this patented welding wire is Si-Mn-Ni, and the trace elements are Cu, Ti, Mo, Nb, and V, but no slag-forming components are added, and the strength and fracture toughness are not mentioned.
[0006] 201410238443.4 discloses a seamless self-shielded flux-cored welding wire suitable for X80 pipeline steel. The patented welding wire uses fluorine, barium and lithium as the main slag-forming components, but no rutile is added. Zr, Mn and Ni are added as alloy elements, but Cr, Si and Nb are not added. Strength and fracture toughness are not mentioned. Summary of the invention
[0007] In order to solve the deficiencies of the prior art, the present invention provides a flux-cored welding wire containing rare earth metal and slag gas combined protection and its application. The flux-cored welding wire is suitable for full-position automatic welding of X80 pipeline steel. By adjusting the formula of the slag-forming agent and the composition range of the alloying elements, the weld is subjected to slag gas combined protection, so that the weld metal has a strength similar to that of the pipeline body, while improving the fracture toughness and corrosion resistance. In addition, the welding wire also has good process performance, and after welding, the slag coverage is uniform, the weld surface is smooth, and there is no large particle splash.
[0008] The technical solution provided by the present invention is as follows:
[0009] A flux-cored welding wire with rare earth metal slag gas combined protection consists of a carbon steel strip and a flux core. The flux core consists of the following raw materials in percentage by weight: 20-35% fluorite, 25-35% rutile, 15-25% potassium feldspar, 5-10% aluminum-magnesium alloy, 1-5% 75% ferrosilicon, 3-7% medium-carbon ferromanganese, 1-5% nickel powder, 0.4-2% ferromolybdenum, 0.5-2% cerium dioxide, 0.5-4% high-carbon ferrochrome, and the balance is iron powder. The mass of the flux core accounts for 13-18% of the total mass of the welding wire, that is, the filling rate is 13-18%.
[0010] In the above technical solution:
[0011] Fluorite: The main component of fluorite is CaF2, and its main functions are dehydrogenation and slag formation. It is non-toxic and inexpensive. In addition, BeF2, which is often used for slag formation, is beneficial to reduce spatter, but due to its toxicity, in line with the attitude of green welding, this welding wire uses CaF2 instead of BeF2 as the main slag forming agent.
[0012] Rutile: The main component of rutile is TiO2, which can reduce the basicity of slag as an acidic oxide and eventually transform into CaTiO3. It solidifies first at about 1900℃, forms a skeleton in the welding slag to support it, hinder the flow of slag, and make the slag evenly distributed. When slag is removed, it falls off in large pieces, and there is no sticky slag on the surface of the weld metal. In addition, the Ti element is transferred into the weld to form fine dispersed inclusions, which promotes the nucleation of acicular ferrite.
[0013] Potassium feldspar: The main components of potassium feldspar are K2O·Al2O3·6SiO2, in which K2O can provide K with low ionization potential. + , enhance arc stability, SiO2 can reduce the basicity and surface tension of the slag, refine the molten droplets, and promote the transition of rare earth elements.
[0014] Aluminum-magnesium alloy: It can deoxidize and denitrify. Aluminum also has the function of solid solution strengthening and promoting the transition of rare earth elements.
[0015] Nickel powder is mainly responsible for the transition of Ni element into the weld. The addition of Ni element can refine the structure and promote the formation of acicular ferrite. Ni element can also significantly reduce the ductile-brittle transition temperature of the weld. However, there is an interaction between Ni and Mn. When adding Ni, it should be added according to the amount of Mn element added.
[0016] 75 Ferrosilicon: Ferrosilicon is another important deoxidizer, and is also responsible for the transition of Si elements into the weld. Appropriate ferrosilicon can improve the processing performance of the welding wire, increase the strength of the weld metal, and Si / Mn has a great influence on the microstructure of the weld. Therefore, when considering the amount of ferrosilicon powder added, it is often necessary to consider the weight of the medium carbon ferromanganese powder.
[0017] Molybdenum iron can transition Mo into the weld and improve the weld strength.
[0018] Cerium oxide powder is used to transition the Ce element into the weld. Appropriate Ce elements can significantly reduce the diffusible hydrogen content of the weld. In addition, appropriate Ce elements can also improve the strength and toughness of the weld structure. However, excessive cerium oxide powder not only affects the process performance and produces large spatter, but is also prone to segregation, which reduces the mechanical properties of the weld.
[0019] Based on the above technical solution: the welding wire uses fluorite and rutile as the main slag system, potassium feldspar, magnesia and aluminum-magnesium alloy as auxiliary components, and the main alloy system of the metal powder is C-Si-Mn-Ni-Mo-Cr, supplemented by rare earth elements Ce. The introduction of the slag system forms a uniform slag on the surface of the weld metal, supporting the molten pool and promoting the transition of alloy elements. The addition of alloy elements effectively guarantees the strength and toughness of the weld, and rare earth elements can significantly improve the hydrogen resistance of the weld.
[0020] Specifically, the iron powder content may be zero.
[0021] Preferred:
[0022] The core is composed of the following raw materials in weight percentage: 29% fluorite, 32% rutile, 21% potassium feldspar, 9% aluminum-magnesium alloy, 1.7% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.3% nickel powder, 0.6% ferromolybdenum, 0.6% cerium dioxide, 0.6% high carbon ferrochrome, and the balance is iron powder;
[0023] The mass of the flux core accounts for 14.5% of the total mass of the welding wire.
[0024] Preferred:
[0025] The core is composed of the following raw materials in weight percentage: 34% fluorite, 27% rutile, 19.5% potassium feldspar, 9% aluminum-magnesium alloy, 1.7% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.8% nickel powder, 0.6% ferromolybdenum, 1.6% cerium dioxide, 1.2% high carbon ferrochrome, and the balance is iron powder;
[0026] The mass of the flux core accounts for 14.8% of the total mass of the welding wire.
[0027] Preferred:
[0028] The core is composed of the following raw materials in weight percentage: 34% fluorite, 29% rutile, 17.5% potassium feldspar, 9% aluminum-magnesium alloy, 1.7% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.8% nickel powder, 0.6% ferromolybdenum, 1.6% cerium dioxide, 1.2% high carbon ferrochrome, and the balance is iron powder;
[0029] The mass of the flux core accounts for 15.0% of the total mass of the welding wire.
[0030] Preferred:
[0031] The core is composed of the following raw materials in weight percentage: 32% fluorite, 25% rutile, 21% potassium feldspar, 5% aluminum-magnesium alloy, 3.0% 75 ferrosilicon, 5.0% medium carbon ferromanganese, 3.0% nickel powder, 1.6% ferromolybdenum, 2% cerium dioxide, and 2.4% high carbon ferrochrome;
[0032] The mass of the flux core accounts for 14.8% of the total mass of the welding wire.
[0033] Preferred:
[0034] The core is composed of the following raw materials in weight percentage: 25% fluorite, 25% rutile, 15% potassium feldspar, 7% aluminum-magnesium alloy, 1.2% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.8% nickel powder, 0.6% ferromolybdenum, 1.6% cerium dioxide, 1.2% high carbon ferrochrome, and the balance iron powder;
[0035] The mass of the flux core accounts for 15.8% of the total mass of the welding wire.
[0036] Preferred:
[0037] The core is composed of the following raw materials in weight percentage: 20% fluorite, 25% rutile, 18% potassium feldspar, 9% aluminum-magnesium alloy, 2.0% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.8% nickel powder, 0.4% ferromolybdenum, 1.6% cerium dioxide, 1.2% high carbon ferrochrome, and the balance is iron powder;
[0038] The mass of the flux core accounts for 15.8% of the total mass of the welding wire.
[0039] The rare earth metal-containing slag gas combined protection flux-cored welding wire can be prepared by a conventional method for preparing flux-cored welding wire.
[0040] The invention also provides the application of the rare earth metal slag gas combined protection flux-cored welding wire as the welding wire for X80 pipeline steel.
[0041] Specific:
[0042] The shielding gas is composed of 75-85% Ar and 15-25% CO2 by volume;
[0043] The interlayer temperature is 80-120°C;
[0044] The welding current is 200~220A, the welding voltage is 26V~28V, and the welding speed is 0.24m~0.25m / min.
[0045] Further:
[0046] No pre-weld heat treatment;
[0047] and / or, no post weld heat treatment.
[0048] The beneficial effects of the present invention are as follows:
[0049] Compared with other gas-shielded flux-cored welding wires for X80 pipeline steel, the present invention adopts a slag-gas combined protection method, comprehensively considers the process performance of the welding wire and the mechanical properties and hydrogen embrittlement resistance of the weld metal, and provides a welding wire with fluorite and rutile as the main slag system, Si-Mn-Mo-Ni as the main alloying elements, and rare earth elements added, which can be suitable for welding X80 steel. The girth weld has good forming, easy slag removal, good low-temperature toughness, and extremely low diffusible hydrogen content. At the same time, the slag-forming components are used to help the transition of rare earth elements, thereby improving the hydrogen embrittlement resistance of the weld. In addition, the welding wire has good process adaptability and is particularly suitable for welding the girth weld of X80 pipeline steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 This is the microstructure diagram of Example 1.
[0051] Figure 2 This is the microstructure diagram of Example 2.
[0052] Figure 3 This is the microstructure diagram of Example 3.
[0053] Figure 4 This is the microstructure diagram of Example 4.
[0054] Figure 5 This is the microstructure diagram of Example 5.
[0055] Figure 6This is a microstructure diagram of Example 6.
[0056] Figure 7 is another microstructure picture of Example 6. DETAILED DESCRIPTION
[0057] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0058] Unless otherwise specified, the test methods used in the embodiments of the present invention are conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0059] Rm (MPa) is the tensile strength.
[0060] ReL / Rp0.2 is the yield strength.
[0061] A (%) is the elongation after breaking.
[0062] KV2-30℃ is the impact absorption energy at -30℃.
[0063] Example 1
[0064] A rare earth metal-containing flux-cored welding wire for X80 pipeline steel, consisting of a carbon steel strip and a flux core, wherein the flux core is composed of the following raw materials in weight percentage: 29% fluorite, 32% rutile, 21% potassium feldspar, 9% aluminum-magnesium alloy, 1.7% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.3% nickel powder, 0.6% ferromolybdenum, 0.6% cerium dioxide, 0.6% high carbon ferrochrome, and the balance is iron powder. The mass of the flux core accounts for 14.5% of the total mass of the welding wire.
[0065] The welding conditions are as follows: the shielding gas is composed of 80% Ar and 20% CO2 by volume, no pre-weld and post-weld heat treatment is required, the interlayer temperature is about 100°C, the welding current is 200A, the welding voltage is 26V, and the welding speed is 0.25m / min.
[0066] The test shows that the welding wire has good process performance, stable welding arc, basically no spatter, beautiful weld bead, and no defects such as pores, slag inclusions, and lack of fusion in the weld. Figure 1 shown.
[0067] Mechanical properties of deposited metal
[0068]
[0069] Example 2
[0070] A rare earth metal-containing flux-cored welding wire for X80 pipeline steel, comprising a carbon steel strip and a flux core, wherein the flux core comprises the following raw materials in percentage by weight: 34% fluorite, 27% rutile, 19.5% potassium feldspar, 9% aluminum-magnesium alloy, 1.7% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.8% nickel powder, 0.6% ferromolybdenum, 1.6% cerium dioxide, and 1.2% high carbon ferrochrome. The mass of the flux core accounts for 14.8% of the total mass of the welding wire.
[0071] The welding conditions are as follows: the shielding gas is composed of 80% Ar and 20% CO2 by volume, no pre-weld and post-weld heat treatment is required, the interlayer temperature is about 100°C, the welding current is 220A, the welding voltage is 28V, and the welding speed is 0.25m / min.
[0072] The test shows that the welding wire has good process performance, stable welding arc, basically no spatter, beautiful weld bead, and no defects such as pores, slag inclusions, and lack of fusion in the weld. Figure 2 shown.
[0073] Mechanical properties of deposited metal
[0074]
[0075] Example 3
[0076] A rare earth metal-containing flux-cored welding wire for X80 pipeline steel, comprising a carbon steel strip and a flux core, wherein the flux core comprises the following raw materials in percentage by weight: 34% fluorite, 29% rutile, 17.5% potassium feldspar, 9% aluminum-magnesium alloy, 1.7% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.8% nickel powder, 0.6% ferromolybdenum, 1.6% cerium dioxide, and 1.2% high carbon ferrochrome. The mass of the flux core accounts for 15.0% of the total mass of the welding wire.
[0077] The welding conditions are as follows: the shielding gas is composed of 80% Ar and 20% CO2 by volume, no pre-weld and post-weld heat treatment is required, the interlayer temperature is about 100°C, the welding current is 220A, the welding voltage is 28V, and the welding speed is 0.25m / min.
[0078] The test shows that the welding wire has good process performance, stable welding arc, basically no spatter, beautiful weld bead, and no defects such as pores, slag inclusions, and lack of fusion in the weld. Figure 3 shown.
[0079] Mechanical properties of deposited metal
[0080]
[0081] Example 4
[0082] A rare earth metal-containing flux-cored welding wire for X80 pipeline steel, comprising a carbon steel strip and a flux core, wherein the flux core is composed of the following raw materials in weight percentage: 32% fluorite, 25% rutile, 21% potassium feldspar, 5% aluminum-magnesium alloy, 3.0% 75 ferrosilicon, 5.0% medium carbon ferromanganese, 3.0% nickel powder, 1.6% ferromolybdenum, 2% cerium dioxide, and 2.4% high carbon ferrochrome. The mass of the flux core accounts for 14.8% of the total mass of the welding wire.
[0083] The welding conditions are as follows: the shielding gas is composed of 80% Ar and 20% CO2 by volume, no pre-weld and post-weld heat treatment is required, the interlayer temperature is about 100°C, the welding current is 220A, the welding voltage is 28V, and the welding speed is 0.25m / min.
[0084] The test shows that the welding wire has good process performance, stable welding arc, basically no spatter, beautiful weld bead, and no defects such as pores, slag inclusions, and lack of fusion in the weld. Figure 4 shown.
[0085] Mechanical properties of deposited metal
[0086]
[0087] Example 5
[0088] A rare earth metal-containing flux-cored welding wire for X80 pipeline steel, consisting of a carbon steel strip and a flux core, wherein the flux core is composed of the following raw materials in weight percentage: 25% fluorite, 25% rutile, 15% potassium feldspar, 7% aluminum-magnesium alloy, 1.2% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.8% nickel powder, 0.6% ferromolybdenum, 1.6% cerium dioxide, 1.2% high carbon ferrochrome, and the remainder is iron powder. The mass of the flux core accounts for 15.8% of the total mass of the welding wire.
[0089] The welding conditions are as follows: the shielding gas is composed of 80% Ar and 20% CO2 by volume, no pre-weld and post-weld heat treatment is required, the interlayer temperature is about 100°C, the welding current is 220A, the welding voltage is 28V, and the welding speed is 0.25m / min.
[0090] The test shows that the welding wire has good process performance, stable welding arc, basically no spatter, beautiful weld bead, and no defects such as pores, slag inclusions, and lack of fusion in the weld. Figure 5 shown.
[0091] Mechanical properties of deposited metal
[0092]
[0093]
[0094] Example 6
[0095] This example compares two types of flux-cored welding wires for X80 pipeline steel, one with rare earth elements and the other without rare earth elements. The wires are composed of a carbon steel strip and a flux core. The welding conditions are set to be the same. The shielding gas is composed of 80% Ar and 20% CO2 by volume. No pre-weld and post-weld heat treatment is required. The interlayer temperature is about 100°C, the welding current is 220A, the welding voltage is 28V, and the welding speed is 0.25m / min.
[0096] The tests showed that both welding wires had good process performance, stable welding arc, basically no spatter, beautiful weld bead formation, and no defects such as porosity, slag inclusion, and lack of fusion in the weld.
[0097] The flux core with rare earth elements is composed of the following raw materials in weight percentage: fluorite 20%, rutile 25%, potassium feldspar 18%, aluminum-magnesium alloy 9%, 75 ferrosilicon 2.0%, medium carbon ferromanganese 3.6%, nickel powder 1.8%, ferromolybdenum 0.4%, cerium dioxide 1.6%, high carbon ferrochrome 1.2%, and iron powder as the balance. The mass of the flux core accounts for 15.8% of the total mass of the welding wire. The weld structure is fine ferrite with low diffusible hydrogen content. The microstructure is as follows: Figure 6 shown.
[0098] Mechanical properties of deposited metal
[0099]
[0100] The flux core without rare earth elements is composed of the following raw materials in weight percentage: fluorite 20%, rutile 25%, potassium feldspar 18%, aluminum-magnesium alloy 9%, 75 ferrosilicon 2.0%, medium carbon ferromanganese 3.6%, nickel powder 1.8%, ferromolybdenum 0.4%, high carbon ferrochrome 1.2%, and iron powder as the balance. The mass of the flux core accounts for 15.8% of the total mass of the welding wire. The weld structure is a relatively coarse ferrite structure with a high content of diffusible hydrogen. The microstructure is as follows: Figure 7 shown.
[0101] Mechanical properties of deposited metal
[0102]
[0103] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this description, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A rare earth metal slag gas combined protection flux-cored welding wire, consisting of a carbon steel strip and a flux core. It is characterized in that The flux core is composed of the following raw materials in weight percentage: 20-35% fluorite, 25-35% rutile, 15-25% potassium feldspar, 5-10% aluminum-magnesium alloy, 1-5% 75 ferrosilicon, 3-7% medium carbon ferromanganese, 1-5% nickel powder, 0.4-2% ferromolybdenum, 0.5-2% cerium dioxide, 0.5-4% high carbon ferrochrome, and the balance is iron powder. The mass of the flux core accounts for 13-18% of the total mass of the welding wire.
2. The rare earth metal-containing slag gas combined protection flux-cored welding wire according to claim 1, Features: The core is composed of the following raw materials in weight percentage: 29% fluorite, 32% rutile, 21% potassium feldspar, 9% aluminum-magnesium alloy, 1.7% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.3% nickel powder, 0.6% ferromolybdenum, 0.6% cerium dioxide, 0.6% high carbon ferrochrome, and the balance is iron powder; The mass of the flux core accounts for 14.5% of the total mass of the welding wire.
3. The rare earth metal-containing slag gas combined protection flux-cored welding wire according to claim 1, Features: The core is composed of the following raw materials in weight percentage: 34% fluorite, 27% rutile, 19.5% potassium feldspar, 9% aluminum-magnesium alloy, 1.7% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.8% nickel powder, 0.6% ferromolybdenum, 1.6% cerium dioxide, 1.2% high carbon ferrochrome, and the balance is iron powder; The mass of the flux core accounts for 14.8% of the total mass of the welding wire.
4. The rare earth metal-containing slag gas combined protection flux-cored welding wire according to claim 1, Features: The core is composed of the following raw materials in weight percentage: 34% fluorite, 29% rutile, 17.5% potassium feldspar, 9% aluminum-magnesium alloy, 1.7% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.8% nickel powder, 0.6% ferromolybdenum, 1.6% cerium dioxide, 1.2% high carbon ferrochrome, and the balance is iron powder; The mass of the flux core accounts for 15.0% of the total mass of the welding wire.
5. The rare earth metal-containing slag gas combined protection flux-cored welding wire according to claim 1, Features: The core is composed of the following raw materials in weight percentage: 32% fluorite, 25% rutile, 21% potassium feldspar, 5% aluminum-magnesium alloy, 3.0% 75 ferrosilicon, 5.0% medium carbon ferromanganese, 3.0% nickel powder, 1.6% ferromolybdenum, 2% cerium dioxide, and 2.4% high carbon ferrochrome; The mass of the flux core accounts for 14.8% of the total mass of the welding wire.
6. The rare earth metal-containing slag gas combined protection flux-cored welding wire according to claim 1, Features: The core is composed of the following raw materials in weight percentage: 25% fluorite, 25% rutile, 15% potassium feldspar, 7% aluminum-magnesium alloy, 1.2% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.8% nickel powder, 0.6% ferromolybdenum, 1.6% cerium dioxide, 1.2% high carbon ferrochrome, and the balance iron powder; The mass of the flux core accounts for 15.8% of the total mass of the welding wire.
7. The rare earth metal-containing slag gas combined protection flux-cored welding wire according to claim 1, Features: The core is composed of the following raw materials in weight percentage: 20% fluorite, 25% rutile, 18% potassium feldspar, 9% aluminum-magnesium alloy, 2.0% 75 ferrosilicon, 3.6% medium carbon ferromanganese, 1.8% nickel powder, 0.4% ferromolybdenum, 1.6% cerium dioxide, 1.2% high carbon ferrochrome, and the balance is iron powder; The mass of the flux core accounts for 15.8% of the total mass of the welding wire.
8. An application of a flux-cored welding wire with rare earth metal-containing slag gas combined protection according to any one of claims 1 to 7, Features: As welding wire for X80 pipeline steel.
9. The use according to claim 8, Features: The protective gas is composed of 75-85% Ar and 15-25% CO by volume. 2 composition; The interlayer temperature is 80-120°C; The welding current is 200~220A, the welding voltage is 26V~28V, and the welding speed is 0.24m~0.25m / min.
10. The use according to claim 8 or 9, Features: No pre-weld heat treatment; and / or, no post weld heat treatment.
Citation Information
Cited By
Stainless steel flux-cored wire and preparation method thereof
CN121245303A
A stainless steel flux-cored welding wire and its preparation method
CN121245303B