Graphene moisture-permeable heat-storage fabric and preparation method thereof
By combining a three-layer modified woven structure with antifouling finishing agents such as lithium nepheline powder and cesium tungsten bronze powder, the problem of insufficient waterproof and antifouling performance of graphene breathable and heat-storing fabrics is solved, achieving a balance between high waterproof, antifouling and breathable performance of the fabric.
Patent Information
- Application Number
- CN202410993565.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing graphene breathable and heat-retaining fabrics have shortcomings in terms of waterproof and stain-resistant properties, and directly adding a waterproof membrane will affect the breathability.
It adopts a three-layer modified fabric structure. The warp of the second layer of modified fabric forms a 40-50° angle with the warp of the first layer of modified fabric, and the warp of the third layer of modified fabric is parallel to the warp of the first layer of modified fabric. A stable nano-protective layer is formed by using an antifouling finishing agent made of lithium nepheline powder and cesium tungsten bronze powder.
It significantly improves the waterproof performance of the fabric while maintaining high moisture permeability, and enhances the anti-fouling effect through the UV shielding properties of cesium tungsten bronze powder and the surface activity of nepheline, thus maintaining its protective performance for a long time.
Smart Images

Figure BDA0004959516430000071 
Figure BDA0004959516430000081 
Figure BDA0004959516430000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fabric preparation, and in particular to a graphene moisture-permeable and heat-storage fabric and a preparation method thereof. Background Art
[0002] Graphene is an emerging material that has been widely studied in recent years. It is ultra-thin, has excellent conductivity, super hardness, and is light and soft. It has great application prospects in aerospace, weapons and equipment, major infrastructure, as well as new energy, new energy vehicles, energy conservation and environmental protection, and electronic information.
[0003] Research shows that graphene materials can be applied to textile fabrics because they also have excellent moisture permeability and thermal conductivity. The moisture permeability is reflected in the unique pore structure of graphene fabrics. These pores provide a good channel for water vapor, making the fabric have excellent air permeability and moisture permeability. This structure allows water vapor to pass through the fabric smoothly, thus keeping the human body dry and comfortable. The thermal conductivity is reflected in that on the one hand, graphene is a two-dimensional material composed of a single layer of carbon atoms, and its thermal conductivity is very high, which means that graphene can quickly transfer heat energy. On the other hand, graphene fabrics can absorb the radiant heat released by the human body and convert it to release heat accordingly. This far-infrared heat storage allows graphene fabrics to maintain a good warmth effect in cold environments.
[0004] However, although the existing graphene moisture-permeable heat-storage fabrics perform well in terms of warmth retention and moisture permeability, they have limitations in other functions. The two most critical disadvantages are poor waterproof and anti-fouling properties. Directly adding a waterproof film will affect the moisture permeability, which limits its application in specific occasions. Summary of the invention
[0005] The object of the present invention is to provide a graphene moisture permeable heat storage fabric and a preparation method thereof, which solves the problem of poor waterproof and antifouling performance of existing graphene moisture permeable heat storage fabrics.
[0006] The present invention achieves the above-mentioned purpose through the following technical solutions:
[0007] A method for preparing a graphene moisture-permeable heat-storage fabric, comprising:
[0008] S1, prepare graphene fiber, then take graphene fiber, cotton fiber and bamboo fiber as mixed fiber, make warp yarn and weft yarn of the mixed fiber through cotton opening, carding, drawing, roving, spun yarn and winding process, then vertically weave the warp yarn and the weft yarn to obtain woven cloth;
[0009] S2, taking the woven fabric, placing it in an antifouling finishing agent for soaking treatment, then taking out the woven fabric, washing and drying it, to obtain a modified woven fabric;
[0010] S3, taking three layers of the modified woven fabric and overlapping and bonding them in sequence to obtain a graphene moisture-permeable and heat-storage fabric;
[0011] The warp lines of the second layer of modified fabric form an angle of 40-50° with the warp lines of the first layer of modified fabric, and the warp lines of the third layer of modified fabric are parallel to the warp lines of the first layer of modified fabric.
[0012] A further improvement is that the specific operation of preparing graphene fibers is:
[0013] Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 6-10, and obtaining a spinning solution;
[0014] Preparing raw fibers: taking the spinning solution through a 0.5-1 mm spinneret and injecting it into a coagulation bath at a speed of 0.2-1 mL / min, and then drying to obtain raw fibers;
[0015] Stretching and shaping: placing the original fiber in a protective atmosphere furnace, controlling the temperature to 200-400° C., and applying tension to the original fiber to make the fiber length stretching rate 28-32%;
[0016] Reduction: Take the original fibers after stretching and shaping, place them in a reducing agent for reduction for 1-5 hours, wash and dry to obtain graphene oxide fibers.
[0017] A further improvement is that the reducing agent is selected from one of hydrazine hydrate, hydrobromic acid, sodium borohydride or hydroiodic acid.
[0018] A further improvement is that the mass ratio of the graphene fiber, the cotton fiber and the bamboo fiber is 1:1-4:1-2.
[0019] A further improvement is that in the cotton opening and cleaning process, the combing and beating speed is 420-520 r / min, and the comprehensive beating speed is 800-850 r / min;
[0020] In the carding process, the basis weight is 15-20 g / 5 m, the cylinder speed is 280-320 r / min, the doffer speed is 18-22 r / min, and the flat plate speed is 82-88 mm / min;
[0021] In the drawing process, 5-8 strands are combined in the first pass, the drafting ratio is 6-10 times, the sliver weight is 18-22g / 5m, and the sliver delivery speed is 200-250m / min; 5-10 strands are combined in the second pass, the drafting ratio is 5-10 times, the sliver weight is 16-20g / 5m, and the sliver delivery speed is 180-230m / min;
[0022] In the roving process, the dry weight is 2-4 g / 5 m, the spindle speed is 620-640 r / min, the front roller speed is 200-240 r / min, the back zone stretching multiple is 1-2 times, and the twist coefficient is 80-90;
[0023] In the spinning process, the dry weight is 1-2 g / 100 m, the spindle speed is 12000-14000 r / min, the front roller speed is 180-200 r / min, the back zone stretching multiple is 1-2 times, the total drafting multiple is 24-28 times, the twist coefficient is 300-340, and the jaw spacing is 2.5-2.8 mm;
[0024] In the winding process, the production tension is 180-220 and the machine speed is 1000-1300 m / min.
[0025] A further improvement is that, in terms of weight, the raw materials of the antifouling finishing agent include 10-20 parts of eucryptite powder, 1-5 parts of cesium tungsten bronze powder and 40-60 parts of deionized water.
[0026] A further improvement is that the soaking treatment refers to: controlling the temperature of the antifouling finishing agent to 55-65°C, soaking the fabric in the antifouling finishing agent for 10-15 hours, and applying ultrasonic oscillation treatment with a frequency of 20-25kHz and a power of 300-450W to the antifouling finishing agent during the soaking process.
[0027] A further improvement is that the bonding is performed by means of a mesh breathable hot melt adhesive.
[0028] The present invention also provides a graphene moisture-permeable heat-storage fabric, which is prepared by the preparation method.
[0029] The beneficial effects of the present invention are:
[0030] (1) The graphene moisture permeable heat storage fabric of the present invention is obtained by overlapping and bonding three layers of modified woven fabrics in sequence, and the warp of the second layer of modified woven fabric is at an angle of 40-45° with the warp of the first layer of modified woven fabric, and the warp of the third layer of modified woven fabric is parallel to the warp of the first layer of modified woven fabric, so that the layers are staggered, which is conducive to bonding and greatly reduces the through pores, so that the overall waterproof performance of the fabric is significantly improved, while still maintaining a high moisture permeability;
[0031] (2) The present invention adopts an antifouling finishing agent made of eucryptite powder and cesium tungsten bronze powder. The two are fused to form a stable nano protective layer, which has antifouling properties and further improves the waterproof effect. At the same time, the ultraviolet shielding performance of the cesium tungsten bronze powder can be used to improve the anti-aging performance of the protective layer, while improving the surface activity of eucryptite and enhancing the adhesion of eucryptite, so that the antifouling effect is maintained for a long time. DETAILED DESCRIPTION
[0032] The present application is further described in detail below in conjunction with specific embodiments. It is necessary to point out that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technical personnel in this field can make some non-essential improvements and adjustments to the present application based on the above application content.
[0033] 1. Main Materials
[0034] (1) Graphene oxide solution: 100 g of graphite powder and 50 g of sodium nitrate were placed in a glass container, and 2.3 L of concentrated sulfuric acid was slowly added to the container. The mixture was stirred in an ice bath for 2.5 h. 600 g of potassium permanganate was weighed and slowly added to the container. The temperature was maintained at no more than 20 °C and the mixture was stirred for 1 h. The ice bath was removed and the container was placed in a 35 °C water bath. The mixture was stirred for 2.5 h to obtain a dark brown paste. 4.8 L of hot water was added to the mixture and stirred. After the temperature reached 98 °C, the mixture was quickly transferred to a 98 °C hot water bath and stirred at a constant temperature for 5 min. The hot water bath was removed and the mixture was transferred to an ordinary water bath and stirred for 30 min. 1.4 L of 50 °C deionized water and 1 L of 20 °C deionized water were added to the mixture in sequence. 30% hydrogen peroxide, the reactant changes from brown to yellow, and after stirring for another 12 minutes, the reactant is taken out and filtered, and the filter cake is washed and centrifuged 3 times with 3% hydrochloric acid, and then redispersed in deionized water to obtain a brown suspension. After dialysis for 3 days, the graphene oxide solution is obtained.
[0035] (2) Eucryptite powder: β-eucryptite is used in this paper. The specific preparation method is as follows: Si(OC2H5)4 is pre-hydrolyzed in 75% ethanol water to obtain Si(OH)4 solution, LiNO3 and Al(NO3)3·9H2O are dissolved in anhydrous ethanol, and evenly mixed with the prepared Si(OH)4 solution. Then, it is added dropwise to a citric acid ethanol solution (the ratio of citric acid to metal ions is 2:1), and a small amount of polyethylene glycol is added as a dispersant. The pH value of the solution is 3. The solution is then placed in a constant temperature water bath at 75°C and heated to form a transparent gel after 100 minutes. Finally, the obtained gel is dried to obtain a loose brown-yellow dry gel powder, which is then calcined at 900°C for 3 hours to obtain β-eucryptite powder with a particle size of 20-25nm.
[0036] (3) Cesium tungsten bronze powder: Weigh tungstic acid and cesium hydroxide in a mass ratio of 3:1 and grind until the mixture is uniform; put the ground material into a sealed container and then put it into a muffle furnace for reaction at 800°C for 2 hours; thus, cesium tungsten bronze powder is obtained.
[0037] 2. Implementation of the experiment
[0038] Example 1
[0039] A method for preparing a graphene moisture-permeable heat-storage fabric, comprising:
[0040] S1. Prepare graphene fiber, and then take graphene fiber, cotton fiber and bamboo fiber as mixed fiber in a mass ratio of 1:1:1, and make the mixed fiber into warp yarn and weft yarn through cotton opening, carding, drawing, roving, spun yarn and winding processes, and then vertically weave the warp yarn and the weft yarn to obtain woven cloth.
[0041] Among them, the specific operation of preparing graphene fiber is:
[0042] Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 6, and obtaining a spinning solution;
[0043] Preparation of raw fibers: taking the spinning solution through a 0.5 mm spinneret and injecting it into a coagulation bath at a speed of 0.2 mL / min, and then drying to obtain raw fibers;
[0044] Stretching and shaping: placing the original fiber in a nitrogen protective atmosphere furnace, controlling the temperature to 200° C., and applying tension to the original fiber to make the fiber length stretching rate reach 28%;
[0045] Reduction: Take the original fiber after stretching and shaping, place it in a hydrazine hydrate reducing agent for reduction for 1 hour, wash and dry to obtain graphene oxide fiber.
[0046] Among them, in the cotton opening and cleaning process, the speed of the combing needle beater is 420r / min, and the comprehensive beater speed is 800r / min; in the cotton combing process, the basis weight is 15g / 5m, the cylinder speed is 280r / min, the doffer speed is 18r / min, and the cover speed is 82mm / min; in the drawing process, the first 5 strands are combined, the drafting multiple is 6 times, the drawing dry basis weight is 18g / 5m, and the sliver delivery speed is 200m / min; the second 5 strands are combined, the drafting multiple is 5 times, the drawing dry basis weight is 16g / 5m, and the sliver delivery speed is 18 0m / min; in the roving process, the dry weight is 2g / 5m, the spindle speed is 620r / min, the front roller speed is 200r / min, the stretching multiple of the back zone is 1.2 times, and the twist coefficient is 80; in the spun yarn process, the dry weight is 1g / 100m, the spindle speed is 12000r / min, the front roller speed is 180r / min, the stretching multiple of the back zone is 1.2 times, the total drafting multiple is 24 times, the twist coefficient is 300, and the jaw spacing is 2.5mm; in the winding process, the production tension is 180 and the machine speed is 1000m / min.
[0047] S2, take the fabric, place it in the antifouling finishing agent for soaking treatment, then take out the fabric, wash and dry it, and obtain the modified fabric; in terms of weight, the raw materials of the antifouling finishing agent include 10 parts of eucryptite powder, 1 part of cesium tungsten bronze powder and 40 parts of deionized water. The soaking treatment refers to: controlling the temperature of the antifouling finishing agent to 55°C, soaking the fabric in the antifouling finishing agent for 10 hours, and applying ultrasonic oscillation treatment with a frequency of 20kHz and a power of 30W to the antifouling finishing agent during the soaking process.
[0048] S3, taking three layers of the modified woven fabric and overlapping and bonding them in sequence (bonding them with a mesh breathable hot melt adhesive) to obtain a graphene moisture-permeable heat-storage fabric;
[0049] Among them, the warp of the second layer of modified fabric forms an angle of 40° with the warp of the first layer of modified fabric (measured by the acute angle after projection onto the same plane, the same below), and the warp of the third layer of modified fabric is parallel to the warp of the first layer of modified fabric.
[0050] Example 2
[0051] A method for preparing a graphene moisture-permeable heat-storage fabric, comprising:
[0052] S1. Prepare graphene fiber, and then take graphene fiber, cotton fiber and bamboo fiber as mixed fiber in a mass ratio of 1:2:1.5, and make the mixed fiber into warp yarn and weft yarn through cotton opening, carding, drawing, roving, spun yarn and winding steps, and then vertically weave the warp yarn and the weft yarn to obtain woven cloth.
[0053] Among them, the specific operation of preparing graphene fiber is:
[0054] Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 8, and obtaining a spinning solution;
[0055] Preparation of original fibers: taking the spinning solution through a 0.8 mm spinneret and injecting it into a coagulation bath at a speed of 0.6 mL / min, and then drying to obtain original fibers;
[0056] Stretching and shaping: placing the original fiber in a helium protective atmosphere furnace, controlling the temperature to 300° C., and applying tension to the original fiber to make the fiber length stretching rate 30%;
[0057] Reduction: Take the original fibers after stretching and shaping, place them in a hydrobromic acid reducing agent for reduction for 3 hours, wash and dry to obtain graphene oxide fibers.
[0058] Among them, in the cotton opening and cleaning process, the speed of the combing needle beater is 460r / min, and the comprehensive beater speed is 820r / min; in the cotton combing process, the basis weight is 18g / 5m, the cylinder speed is 300r / min, the doffer speed is 20r / min, and the cover speed is 85mm / min; in the drawing process, the first 6 strands are combined, the drafting multiple is 8 times, the drawing dry weight is 20g / 5m, and the sliver delivery speed is 220m / min; the second 8 strands are combined, the drafting multiple is 8 times, the drawing dry weight is 18g / 5m, and the sliver delivery speed is 200 m / min; in the roving process, the dry weight is 3g / 5m, the spindle speed is 630r / min, the front roller speed is 230r / min, the stretching multiple of the back zone is 1.6 times, and the twist coefficient is 85; in the spun yarn process, the dry weight is 1.6g / 100m, the spindle speed is 13000r / min, the front roller speed is 190r / min, the stretching multiple of the back zone is 1.6 times, the total drafting multiple is 26 times, the twist coefficient is 320, and the jaw spacing is 2.6mm; in the winding process, the production tension is 200 and the machine speed is 1200m / min.
[0059] S2, take the fabric, place it in the antifouling finishing agent for soaking treatment, then take out the fabric, wash and dry it, and obtain the modified fabric; according to the weight percentage, the raw materials of the antifouling finishing agent include 15 parts of eucryptite powder, 3 parts of cesium tungsten bronze powder and 50 parts of deionized water. The soaking treatment refers to: controlling the temperature of the antifouling finishing agent to 60°C, soaking the fabric in the antifouling finishing agent for 12 hours, and applying ultrasonic oscillation treatment with a frequency of 22kHz and a power of 350W to the antifouling finishing agent during the soaking process.
[0060] S3, taking three layers of the modified woven fabric and overlapping and bonding them in sequence (bonding them with a mesh breathable hot melt adhesive) to obtain a graphene moisture-permeable heat-storage fabric;
[0061] The warp lines of the second layer of modified fabric form an angle of 45° with the warp lines of the first layer of modified fabric, and the warp lines of the third layer of modified fabric are parallel to the warp lines of the first layer of modified fabric.
[0062] Example 3
[0063] A method for preparing a graphene moisture-permeable heat-storage fabric, comprising:
[0064] S1. Prepare graphene fiber, and then take graphene fiber, cotton fiber and bamboo fiber as mixed fiber in a mass ratio of 1:4:2, and make the mixed fiber into warp yarn and weft yarn through cotton opening, carding, drawing, roving, spun yarn and winding steps, and then vertically weave the warp yarn and the weft yarn to obtain woven cloth.
[0065] Among them, the specific operation of preparing graphene fiber is:
[0066] Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 10, and obtaining a spinning solution;
[0067] Preparation of raw fibers: taking the spinning solution through a 1 mm spinneret and injecting it into a coagulation bath at a speed of 1 mL / min, and then drying to obtain raw fibers;
[0068] Stretching and shaping: placing the original fiber in a nitrogen protective atmosphere furnace, controlling the temperature to 400° C., and applying tension to the original fiber to make the fiber length stretching rate 32%;
[0069] Reduction: Take the original fibers after stretching and shaping, place them in a hydroiodic acid reducing agent for reduction for 5 hours, wash and dry, and then obtain graphene oxide fibers.
[0070] Among them, in the cotton opening and cleaning process, the speed of the combing needle beater is 520r / min, and the comprehensive beater speed is 850r / min; in the cotton combing process, the basis weight is 20g / 5m, the cylinder speed is 320r / min, the doffer speed is 22r / min, and the cover speed is 88mm / min; in the drawing process, 8 strands are combined in the first pass, the drafting multiple is 10 times, the drawing dry basis weight is 22g / 5m, and the sliver output speed is 250m / min; 10 strands are combined in the second pass, the drafting multiple is 10 times, the drawing dry basis weight is 20g / 5m, and the sliver output speed is The dry weight is 4g / 5m, the spindle speed is 640r / min, the front roller speed is 240r / min, the stretching multiple of the rear zone is 2 times, and the twist coefficient is 90; in the spun yarn process, the dry weight is 2g / 100m, the spindle speed is 14000r / min, the front roller speed is 200r / min, the stretching multiple of the rear zone is 2 times, the total drafting multiple is 28 times, the twist coefficient is 340, and the jaw spacing is 2.8mm; in the winding process, the production tension is 220 and the machine speed is 1300m / min.
[0071] S2, take the fabric, place it in the antifouling finishing agent for soaking treatment, then take out the fabric, wash and dry it, and obtain the modified fabric; in terms of weight, the raw materials of the antifouling finishing agent include 20 parts of eucryptite powder, 5 parts of cesium tungsten bronze powder and 60 parts of deionized water. The soaking treatment refers to: controlling the temperature of the antifouling finishing agent to 65°C, soaking the fabric in the antifouling finishing agent for 15 hours, and applying ultrasonic oscillation treatment with a frequency of 25kHz and a power of 450W to the antifouling finishing agent during the soaking process.
[0072] S3, taking three layers of the modified woven fabric and overlapping and bonding them in sequence (bonding them with a mesh breathable hot melt adhesive) to obtain a graphene moisture-permeable heat-storage fabric;
[0073] The warp lines of the second layer of modified fabric form an angle of 50° with the warp lines of the first layer of modified fabric, and the warp lines of the third layer of modified fabric are parallel to the warp lines of the first layer of modified fabric.
[0074] Comparative Example 1
[0075] A method for preparing a graphene moisture-permeable heat-storage fabric, comprising:
[0076] S1. Same as Example 2.
[0077] S2, take the fabric, place it in the antifouling finishing agent for soaking treatment, then take out the fabric, wash and dry it, and obtain the modified fabric; according to the weight percentage, the raw materials of the antifouling finishing agent include 18 parts of eucryptite powder and 50 parts of deionized water. The soaking treatment refers to: controlling the temperature of the antifouling finishing agent to 60°C, soaking the fabric in the antifouling finishing agent for 12 hours, and applying ultrasonic oscillation treatment with a frequency of 22kHz and a power of 350W to the antifouling finishing agent during the soaking process.
[0078] S3. Same as Example 2.
[0079] Comparative Example 2
[0080] A method for preparing a graphene moisture-permeable heat-storage fabric, comprising:
[0081] S1. Same as Example 2.
[0082] S2. Take the fabric, place it in an antifouling finishing agent for soaking treatment, then take out the fabric, wash and dry it to obtain a modified fabric; the raw materials of the antifouling finishing agent include 18 parts of cesium tungsten bronze powder and 50 parts of deionized water by weight. The soaking treatment refers to: controlling the temperature of the antifouling finishing agent to 60°C, soaking the fabric in the antifouling finishing agent for 12 hours, and applying ultrasonic oscillation treatment with a frequency of 22kHz and a power of 350W to the antifouling finishing agent during the soaking process.
[0083] S3. Same as Example 2.
[0084] In addition, based on Example 2, only the angle between the warp of the second layer of modified woven fabric and the warp of the first layer of modified woven fabric in step S3 is adjusted, and the other components and parameters remain unchanged, thereby obtaining a comparative example as shown in Table 1 below.
[0085] Table 1: Angles between the warp of the second layer of modified woven fabric and the warp of the first layer of modified woven fabric in each comparative example
[0086]
[0087]
[0088] 3. Performance Test
[0089] The graphene moisture permeable heat storage fabric samples prepared in Examples 1-3 and Comparative Examples 1-12 were washed 20 times and then subjected to the following performance tests:
[0090] (1) Moisture permeability:
[0091] According to the national standard GB / T12704.1-2009(a), the samples were tested for moisture permeability using a FX3180 moisture permeability tester. During the test, the temperature was 38°C, the humidity was 90.0%, the air flow rate was 0.5m / s, and the test area was 28.3cm 2 Before the test, the test chamber needs to be pre-humidified. After the automatic humidity adjustment is completed, the instrument starts the moisture permeability test and automatically records the moisture permeability data once every hour, twice in total. After the experiment is completed, the moisture permeability data of the sample is manually recorded, and the average of 5 groups of experimental data for each group of samples is used as the final data.
[0092] (2) Waterproof performance:
[0093] Verified by hydrostatic pressure resistance test, the fabric is tested for hydrostatic pressure resistance in accordance with GB / T 4744-2013. Test method: Wipe off the experimental water on the clamping surface, clamp the sample, and make the front of the sample contact with water. Apply a continuously increasing water pressure to the sample at a water pressure increase rate of 60cm H20 / min, and observe the water seepage phenomenon. During the pressure increase process, stop increasing the pressure when the third water droplet appears on the sample, and record the hydrostatic pressure value at this time.
[0094] (3) Antifouling performance:
[0095] With reference to GB / T 30159.1-2013 "Testing and evaluation of antifouling properties of textiles Part 1: Stain resistance", the sample was tested using the liquid stain method. The specific process is: take 2 layers of filter paper and place them on a smooth horizontal surface, place the sample flatly with the front side facing up on the filter paper, and use a dropper to drop about 0.05mL of soy sauce liquid on each of the three parts of the sample. The distance between each drop is at least 50mm. When dropping, the dropper mouth is about 6mm away from the sample surface; after the sample is left to stand for 30s, observe each drop at a viewing angle of about 45° for rating. The rating standards refer to Table 2 below.
[0096] Table 2: Contamination levels
[0097]
[0098]
[0099] IV. Results Analysis
[0100] The test results of the above-mentioned moisture permeability, waterproof performance and antifouling performance are summarized in the following Table 3:
[0101] Table 3: Test results after the samples were washed 20 times
[0102] Group <![CDATA[Water vapor permeability g / (m 2 ·24h)]]> <![CDATA[Hydrostatic pressure resistance mmH2O]]> Contamination level Example 1 19642 14164 Level 4 Example 2 19963 14648 Level 4 Example 3 19479 13995 Level 4 Comparative Example 1 19531 11894 Level 2 Comparative Example 2 20046 12206 Level 2 Comparative Example 3 21135 8651 Level 4 Comparative Example 4 21029 9213 Level 4 Comparative Example 5 20864 10694 Level 4 Comparative Example 6 20561 11716 Level 4 Comparative Example 7 20269 14269 Level 4 Comparative Example 8 20252 14198 Level 4 Comparative Example 9 20493 11590 Level 4 Comparative Example 10 20790 10831 Level 4 Comparative Example 11 21034 9344 Level 4 Comparative Example 12 21167 8833 Level 4
[0103] As can be seen from Table 3 above, the graphene moisture permeable heat storage fabric samples prepared in Examples 1-3 of the present invention have outstanding waterproof and antifouling properties, while the moisture permeability can still maintain a high level. In Comparative Examples 1 and 2, the functional components of the antifouling finishing agent only use one component, eucryptite powder or cesium tungsten bronze powder, which significantly reduces the antifouling performance, and the waterproof performance also decreases to a certain extent. This shows that both are indispensable, and only the fusion of the two can form a stable nano protective layer and maintain high efficiency for a long time. Comparative Examples 3-12 adjust the angle between the warp of the second layer of modified fabric and the warp of the first layer of modified fabric, so that the waterproof performance changes significantly, especially when the angle is between 40-50°C, the water pressure resistance and hydrostatic pressure resistance reach more than 14000mmH2O.
[0104] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing a graphene moisture-permeable heat-storage fabric, characterized in that the steps include: S1, prepare graphene fiber, then take graphene fiber, cotton fiber and bamboo fiber as mixed fiber, make warp yarn and weft yarn of the mixed fiber through cotton opening, carding, drawing, roving, spun yarn and winding process, then vertically weave the warp yarn and the weft yarn to obtain woven cloth; S2, taking the woven fabric, placing it in an antifouling finishing agent for soaking treatment, then taking out the woven fabric, washing and drying it, to obtain a modified woven fabric; S3, taking three layers of the modified woven fabric and overlapping and bonding them in sequence to obtain a graphene moisture-permeable and heat-storage fabric; The warp lines of the second layer of modified fabric form an angle of 40-50° with the warp lines of the first layer of modified fabric, and the warp lines of the third layer of modified fabric are parallel to the warp lines of the first layer of modified fabric.
2. The method for preparing a graphene moisture-permeable heat-storage fabric according to claim 1, characterized in that: The specific operation of preparing graphene fiber is: Preparing a spinning solution: taking a graphene oxide solution, adjusting the pH to 6-10, and obtaining a spinning solution; Preparing raw fibers: taking the spinning solution through a 0.5-1 mm spinneret and injecting it into a coagulation bath at a speed of 0.2-1 mL / min, and then drying to obtain raw fibers; Stretching and shaping: placing the original fiber in a protective atmosphere furnace, controlling the temperature to 200-400° C., and applying tension to the original fiber to make the fiber length stretching rate 28-32%; Reduction: Take the original fibers after stretching and shaping, place them in a reducing agent for reduction for 1-5 hours, wash and dry to obtain graphene oxide fibers.
3. The method for preparing a graphene moisture-permeable heat-storage fabric according to claim 2, characterized in that: The reducing agent is selected from one of hydrazine hydrate, hydrobromic acid, sodium borohydride or hydroiodic acid.
4. The method for preparing a graphene moisture-permeable heat-storage fabric according to claim 1, characterized in that: The mass ratio of the graphene fiber, the cotton fiber and the bamboo fiber is 1:1-4:1-2.
5. The method for preparing a graphene moisture-permeable heat-storage fabric according to claim 1, characterized in that: In the cotton opening and cleaning process, the combing and beating speed is 420-520 r / min, and the comprehensive beating speed is 800-850 r / min; In the carding process, the basis weight is 15-20 g / 5 m, the cylinder speed is 280-320 r / min, the doffer speed is 18-22 r / min, and the flat plate speed is 82-88 mm / min; In the drawing process, 5-8 strands are combined in the first pass, the drafting ratio is 6-10 times, the sliver weight is 18-22g / 5m, and the sliver delivery speed is 200-250m / min; 5-10 strands are combined in the second pass, the drafting ratio is 5-10 times, the sliver weight is 16-20g / 5m, and the sliver delivery speed is 180-230m / min; In the roving process, the dry weight is 2-4 g / 5 m, the spindle speed is 620-640 r / min, the front roller speed is 200-240 r / min, the back zone stretching multiple is 1-2 times, and the twist coefficient is 80-90; In the spinning process, the dry weight is 1-2 g / 100 m, the spindle speed is 12000-14000 r / min, the front roller speed is 180-200 r / min, the back zone stretching multiple is 1-2 times, the total drafting multiple is 24-28 times, the twist coefficient is 300-340, and the jaw spacing is 2.5-2.8 mm; In the winding process, the production tension is 180-220 and the machine speed is 1000-1300 m / min.
6. The method for preparing a graphene moisture-permeable heat-storage fabric according to claim 1, characterized in that: In terms of weight, the raw materials of the antifouling finishing agent include 10-20 parts of eucryptite powder, 1-5 parts of cesium tungsten bronze powder and 40-60 parts of deionized water.
7. The method for preparing a graphene moisture-permeable heat-storage fabric according to claim 1, characterized in that: The soaking treatment refers to: controlling the temperature of the antifouling finishing agent to 55-65° C., soaking the fabric in the antifouling finishing agent for 10-15 hours, and applying ultrasonic oscillation treatment with a frequency of 20-25kHz and a power of 300-450W to the antifouling finishing agent during the soaking process.
8. The method for preparing a graphene moisture-permeable heat-storage fabric according to claim 1, characterized in that: The bonding is performed by mesh breathable hot melt adhesive.
9. A graphene moisture-permeable heat-storage fabric, characterized in that: The fabric is prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Production process of graphene fiber blended functional garment fabric
CN114517350A
Graphene blended yarn preparation process
CN115247297A
Breathable polyester elastic woven fabric
CN215551469U