Multi-layer composite high-barrier PLA-based packaging film

Through the combination of multi-layer composite structure, homemade compatibilizer and modified barrier filler, the problem of insufficient strength and barrier properties of single-layer PLA film is solved, efficient water vapor and oxygen barriers are achieved, and the integration of PLA-based packaging film is improved. performance.

CN118909179APending Publication Date: 2024-11-08PUSIWEI (SHANGHAI) BIOMATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410944781.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The single-layer PLA film has problems such as poor strength, poor water vapor resistance and oxygen resistance, which limits its application range.

Method used

A multi-layer composite structure is adopted to prepare a PLA-based packaging film by making a self-made compatibilizer and modified barrier filler, combined with a coextrusion composite process. The compatibilizer forms a highly reactive macromolecular structure through UV curing. The modified barrier filler uses a mercaptosilane coupling agent and an olefin monomer for click reaction to form a "hyperbranched" structure, and is coextruded by three layers and bidirectional stretching. Process improves material performance.

Benefits of technology

It improves the mechanical properties and barrier properties of the PLA-based packaging film, enhances the adhesion between layers, achieves excellent water vapor and oxygen barrier effects, and ensures the degradability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004945305580000151
    Figure BDA0004945305580000151
  • Figure BDA0004945305580000161
    Figure BDA0004945305580000161
Patent Text Reader

Abstract

The invention belongs to the field of polymeric membranes. The invention relates to a multi-layer composite high-barrier PLA (polylactic acid)-based packaging film and a preparation method thereof, and the packaging film comprises three layers, namely an upper layer, a middle layer and a lower layer; the upper layer and the lower layer are PLA-based antibacterial layers, and the middle layer is a PLA-based barrier layer; raw materials of the PLA-based antibacterial layer and the PLA-based barrier layer are subjected to mixing, extrusion, plasticization, co-extrusion, vacuum sizing, cooling sizing, preheating, two-way stretching, heat treatment, traction, rolling and other processes according to a formula to prepare the PLA-based antibacterial barrier film. The defects that in the prior art, a single-layer polylactic acid film is poor in strength, and the barrier property cannot be achieved can be effectively overcome, meanwhile, the used main raw materials are all degradable materials, and great application potential is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a multi-layer composite high-barrier PLA-based packaging film and a preparation method thereof. The invention belongs to the field of polymer films. Background Art

[0002] High barrier packaging film materials have the function of blocking oxygen, water vapor, carbon dioxide, taste, etc., which can extend the shelf life of the contents, and have been widely used in the packaging fields of food, medicine, cosmetics, etc. Among them, food packaging is currently the most widely used field of high barrier materials. High barrier packaging films have the comprehensive properties of exquisite printing, excellent barrier properties, and outstanding heat sealing performance. Usually one material cannot meet all performance requirements. Therefore, the current high barrier packaging films are basically composite films of multiple materials, the most typical of which is PET / aluminum foil / PE structure, in addition to PA, EVOH, PP and other materials.

[0003] In view of this, multi-layer composite high barrier packaging materials have brought a lot of convenience to our lives. However, they have also caused a great burden on the environment and caused serious "white pollution". After several years of practice, the biodegradation route is considered to be the most fundamental way to solve the "white pollution" problem caused by discarded high barrier composite films.

[0004] Among biodegradable materials, polylactic acid (PLA) is an aliphatic polyester that naturally decomposes into CO2 and water under composting conditions. It is a green and environmentally friendly bio-sourced material. It is also the only transparent biodegradable polymer and is used in transparent packaging containers and daily necessities. Although PLA has good biodegradability, processability, and excellent mechanical properties, it is brittle and lacks elasticity and flexibility, which greatly limits the application of polylactic acid film. In addition, single-layer PLA film also has the problems of poor strength and poor water vapor and oxygen barrier properties.

[0005] In view of the above problems, modifying PLA and combining it with a multi-layer co-extrusion composite process has become a feasible solution. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a multi-layer composite high-barrier PLA-based packaging film in view of the defects of the prior art that the single-layer PLA film has poor strength and cannot achieve barrier properties. It uses a homemade compatibilizer in the outer layer and a homemade modified barrier filler in the middle barrier layer. After the formula is designed, it is added to the extruder for co-extrusion and biaxial stretching before preparation. The technical solution adopted by the present invention to solve its technical problems is:

[0007] The present invention provides a method for preparing a compatibilizer, comprising the following steps:

[0008] S11, UV curing aromatic acrylate, aliphatic acrylate and isocyanate acrylate under a photoinitiator to obtain a target product, i.e., a compatibilizer.

[0009] Furthermore, the usage ratio of the aromatic acrylate, aliphatic acrylate and isocyanate acrylate is 0.2-0.4 mol: 0.3-0.5 mol: 0.2-0.4 mol.

[0010] The invention provides a compatibilizer, which is prepared by the preparation method of the compatibilizer.

[0011] Another object of the present invention is to provide a method for preparing a modified barrier filler, comprising the following steps:

[0012] S21, placing the barrier filler and the mercaptosilane coupling agent in an alcohol solvent for silylation coupling reaction to obtain an intermediate product;

[0013] S22, click-reacting the intermediate product with an olefin monomer to obtain a target product, i.e., a modified barrier filler.

[0014] Further,

[0015] The usage ratio of the barrier filler, the mercaptosilane coupling agent and the alcohol solvent is 1g:3.3-5.5g:80mL; and

[0016] The barrier filler is a lamellar structure.

[0017] Further, the ratio of the intermediate product to the olefin monomer is 1 mol:1 mol; and

[0018] The vinyl monomer is a monomer containing an epoxy group or an isocyanate structure.

[0019] Another object of the present invention is to provide a modified barrier filler prepared by the above-mentioned preparation method of the modified barrier filler.

[0020] Another object of the present invention is to provide a multi-layer composite high-barrier PLA-based packaging film, the packaging film comprising three layers, namely an upper layer, a middle layer and a lower layer; the upper layer and the lower layer are both PLA-based antibacterial layers, the middle layer is a PLA-based barrier layer; the thickness ratio of the PLA-based antibacterial layer to the PLA-based barrier layer is 1:1.0-1.5;

[0021] The PLA-based antibacterial layer comprises the following raw materials in parts by weight:

[0022] PLA 60-80 parts;

[0023] PBAT 20-40 parts;

[0024] 1.0-2.0 parts of compatibilizer;

[0025] Chitosan 4.0-6.0 parts;

[0026] Antioxidant 0.1-0.5 parts;

[0027] Among them, the total mass of PLA and PBAT is 100 parts;

[0028] The PLA-based barrier layer comprises the following raw materials in parts by weight:

[0029] PLA 70-90 parts;

[0030] PPCP 10-30 parts;

[0031] 8-12 parts of plasticizer;

[0032] 1.0-3.0 parts of modified barrier filler;

[0033] Antioxidant 0.1-0.5 parts;

[0034] Among them, the total mass of PLA and PPCP is 100 parts.

[0035] Another object of the present invention is to provide a method for preparing a multi-layer composite high-barrier PLA-based packaging film, comprising the following steps:

[0036] S31, mixing and plasticizing, i.e.

[0037] Mix all the raw materials evenly according to the formula and put them in different extruders for plasticization;

[0038] S32, co-extrusion, vacuum sizing, cooling and shaping, preheating, biaxial stretching, i.e.

[0039] The plasticized melt in S31 is fed into a three-layer co-extrusion circular die head for melt forming, and subjected to vacuum sizing, cooling and shaping, preheating, and biaxial stretching to obtain a primary film material; and

[0040] S33, heat treatment, traction, winding, i.e.

[0041] The primary film material in S32 is heat treated and finally rolled up to obtain a multi-layer composite high-barrier PLA-based packaging film.

[0042] Further, the die temperature is 180-190°C;

[0043] The transverse stretching ratio is 2.5-3.0; the longitudinal stretching ratio is 2.5-3.0; and

[0044] The stretching temperature is 80-100° C.; the stretching rate is 50-60% / s.

[0045] Beneficial effects of the present invention:

[0046] (1) The present invention provides a multi-layer composite high-barrier PLA-based packaging film, which is mainly composed of PLA and supplemented with PBAT or PPCP as functional resins, and the resins in the system are all degradable materials; first, the PLA-based antibacterial layer is formulated to have good mechanical properties and toughness; the PLA-based barrier layer is formulated to have excellent barrier properties; and the three-layer co-extrusion structure is mainly composed of PLA structure, which has excellent interlayer adhesion.

[0047] (2) The present invention provides a multi-layer composite high barrier PLA-based packaging film, which contains a self-made compatibilizer in the PLA-based antibacterial layer, which is a linear macromolecular chain structure containing aromatic ring side groups, fatty structure side groups, isocyanate side groups and ester structures. First, the aromatic ring side groups, fatty structure side groups and ester groups have good compatibility with PBAT; the fatty structure side groups and ester structures have good compatibility with PLA, so the compatibilizer has a two-phase compatibilization effect with PLA and PBAT; second, the isocyanate structure in the compatibilizer can have a high reaction rate with the hydroxyl groups in PLA and PBAT, and has an excellent chain extension effect; at the same time, there is no migration problem of small molecule chain extenders; third, the compatibilizer also has a positive effect on the dispersion and chain extension of chitosan; fourth, the compatibilizer has good reactivity with the plasticizer in the intermediate barrier layer, further improving the adhesion between the layers.

[0048] (3) The present invention provides a multi-layer composite high-barrier PLA-based packaging film, which contains a self-made modified barrier filler in the PLA-based barrier layer, which is a two-dimensional lamellar filler structure modified with an organic chain that can react with active hydrogen, similar to a "hyperbranched" structure. First, the two-dimensional lamellar or lamellar structure has a good barrier effect on water vapor and oxygen; second, it can have good dispersibility in the polymer system after being modified with an organic chain; third, the reactive structure with active hydrogen has a cross-linking and chain extension effect in the PLA / PPCP system and the plasticizer structure, which can effectively improve the mechanical properties of the material; fourth, the organic chain structure has a certain molecular chain length, which is conducive to the directional arrangement of the filler during the biaxial stretching orientation process, further improving the barrier properties.

[0049] (4) The present invention provides a method for preparing a multi-layer composite high-barrier PLA-based packaging film, which is prepared by co-extruding three layers using different extruders and then biaxially stretching. After the biaxially stretching process, the comprehensive performance can be effectively improved, and the directional arrangement of the modified barrier filler can be promoted, thereby further improving the barrier properties. DETAILED DESCRIPTION

[0050] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.

[0051] The purpose of the present invention is to develop a multi-layer composite high barrier PLA-based packaging film. The design idea is: in view of the brittleness and fragility of existing PLA, it is blended with PBAT; at the same time, PPCP material is introduced as the middle layer to carry out three-layer co-extrusion material. The problems arising from this are as follows: 1. The raw materials of the upper and lower layers of co-extrusion are PLA and PBAT materials, and the compatibility problem needs to be solved; 2. The middle layer is blended with PLA and PPCP. PLA and PPCP have certain compatibility. In addition, a suitable plasticizer needs to be added, and at the same time, a two-dimensional lamellar barrier filler needs to be added to achieve synergistic barrier properties. There is a modification problem of the two-dimensional lamellar barrier filler. The solution is: first, a self-made compatibilizer is made, and at the same time, it can solve the problem of delamination caused by the migration of the plasticizer in the middle layer to the interlayer. The isocyanate structure is used as the chain extension reaction structure in the compatibilizer. Compared with the epoxy structure, the isocyanate has a high reactivity and can effectively improve the mechanical properties; and it is a macromolecular structure without migration and toxicity problems. Second, after the two-dimensional lamellar filler is modified with an organic chain of a certain chain length, there will be a certain movement during stretching and orientation, forming a better shielding layer, further improving the barrier properties. The theoretical basis for this is: first, through low-temperature UV curing, the macromolecular structure of the compatibilizer is efficiently formed; second, for the modified barrier filler, it is modified with a mercaptosilane coupling agent, and then a "mercapto-ene" click reaction is carried out with the carbon-carbon double bond to form a "hyperbranched" structure containing epoxy or isocyanate at the end group. The above-mentioned homemade ingredients are added to different extruders for co-extrusion and biaxial stretching process treatment to obtain a three-layer composite high-barrier PLA packaging film material with improved performance in all aspects. The components work synergistically with each other to effectively improve the barrier properties, mechanical properties, etc. The embodiments of the present invention are as follows:

[0052] The present invention provides a method for preparing a compatibilizer, comprising the following steps:

[0053] S11, N2 protection, aromatic acrylate, aliphatic acrylate, isocyanate acrylate, photoinitiator A are dissolved in anhydrous N,N-dimethylformamide A, stirred, placed under UV device for UV curing for 5-30 minutes; after the reaction is completed, the reaction device is removed, reduced pressure distillation is carried out, and vacuum drying is carried out at 40°C for 12 hours to obtain the target product, i.e., the compatibilizer.

[0054] The usage ratio of the aromatic acrylate, aliphatic acrylate, isocyanate acrylate and anhydrous N,N-dimethylformamide A is 0.2-0.4 mol: 0.3-0.5 mol: 0.2-0.4 mol: 500 mL.

[0055] The aromatic acrylate may be phenyl methacrylate, 2-phenoxyethyl acrylate, benzyl methacrylate, 4-(6-(acryloyloxy)hexyloxy)benzoic acid, etc.; and preferably phenyl methacrylate;

[0056] The aliphatic acrylate may be methyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, etc.; and preferably methyl methacrylate;

[0057] The isocyanate acrylate can be methacrylate-2-isocyanate ethyl ester, etc.

[0058] The amount of the photoinitiator A is 1.0-4.0% of the total mass of the reactants;

[0059] The photoinitiator A can be photoinitiator 184, photoinitiator 1173, photoinitiator 2959, photoinitiator TPO, etc.;

[0060] The radiation energy intensity of the UV device can be 300-500 mW / cm 2 ; Specifically, it can be 300mW / cm 2 、350mW / cm 2 , 400mW / cm 2 、450mW / cm 2 , 500mW / cm 2 , or a range of any two values.

[0061] The embodiment of the present invention provides a method for preparing a modified barrier filler, comprising the following steps:

[0062] S21, adding the barrier filler and the mercaptosilane coupling agent to an alcohol solvent, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 50-70° C. for 4-10 h, filtering, taking the insoluble matter, and drying at 60° C. for 12 h to obtain an intermediate product;

[0063] The usage ratio of the barrier filler, the mercaptosilane coupling agent and the alcohol solvent is 1g: 0.8-1.5g: 80mL; and

[0064] The barrier filler is a lamellar structure; it may be graphene oxide, montmorillonite, mica flakes, talcum powder, etc.; and graphene oxide is preferred;

[0065] The graphene oxide is graphene oxide prepared by an improved Hummer's method; and the hydroxyl content of the graphene oxide is 3.0-8.0 mmol / g.

[0066] The mercaptosilane coupling agent may be KH580, KH590, etc.; and KH580 is preferred;

[0067] The alcohol solvent may be anhydrous methanol, anhydrous ethanol, anhydrous isopropanol, etc., and anhydrous ethanol is preferred.

[0068] S22, adding the intermediate product, olefin monomer and photoinitiator B to anhydrous N,N-dimethylformamide B, stirring, and placing under a UV device for UV curing for 5-120 minutes; removing the reaction device, continuing to stir for 1 hour, distilling under reduced pressure, and vacuum drying at 40°C for 12 hours to obtain the target product, i.e., the modified barrier filler.

[0069] The ratio of the intermediate product to the olefin monomer is 1 mol:1 mol;

[0070] The usage ratio of the intermediate product to anhydrous N,N-dimethylformamide B is 1 g:50 mL;

[0071] The vinyl monomer is a monomer containing an epoxy group or an isocyanate structure; it may be allyl glycidyl ether, glycidyl methacrylate, isocyanoethyl methacrylate, etc.; and allyl glycidyl ether is preferred.

[0072] The amount of the photoinitiator B is 0-2.0% of the total mass of the reactants; when the amount of the photoinitiator B is 0, that is, no photoinitiator B is added;

[0073] The photoinitiator B can be photoinitiator 184, photoinitiator 1173, photoinitiator 2959, photoinitiator TPO, etc.;

[0074] The radiation energy intensity of the UV device can be 300-500 mW / cm 2 ; Specifically, it can be 300mW / cm 2 、350mW / cm 2 , 400mW / cm 2 、450mW / cm 2 , 500mW / cm 2 , or a range of any two values.

[0075] The photoinitiator B and the photoinitiator A may be the same photoinitiator or different photoinitiators. In the embodiment of the present invention, the same photoinitiator is selected. Similarly, the radiation energy intensity of the UV device is also selected to be the same light intensity. In the following embodiments of the present invention, the radiation energy intensity of the UV device is 400 mW / cm 2 .

[0076] The embodiment of the present invention further provides a multi-layer composite high-barrier PLA-based packaging film, the packaging film comprising three layers, namely an upper layer, a middle layer and a lower layer; the upper layer and the lower layer are both PLA-based antibacterial layers, the middle layer is a PLA-based barrier layer; the thickness ratio of the PLA-based antibacterial layer to the PLA-based barrier layer is 1:1.0-1.5;

[0077] The PLA-based antibacterial layer comprises the following raw materials in parts by weight:

[0078] PLA 60-80 parts;

[0079] PBAT 20-40 parts;

[0080] 1.0-2.0 parts of compatibilizer;

[0081] Chitosan 4.0-6.0 parts;

[0082] Antioxidant 0.1-0.5 parts;

[0083] Among them, the total mass of PLA and PBAT is 100 parts;

[0084] The PLA-based barrier layer comprises the following raw materials in parts by weight:

[0085] PLA 70-90 parts;

[0086] PPCP 10-30 parts;

[0087] 8-12 parts of plasticizer;

[0088] 1.0-3.0 parts of modified barrier filler;

[0089] Antioxidant 0.1-0.5 parts;

[0090] Among them, the total mass of PLA and PPCP is 100 parts.

[0091] The melt index of the PLA is 2.5-3.5 g / 10 min (190° C., 2.16 kg); the model of the PLA described in the following embodiments of the present invention is PT102, purchased from Pulisi Biotechnology Co., Ltd. PT102 PLA has self-nucleation ability and can crystallize quickly.

[0092] The brand of PBAT described in the following embodiments of the present invention is TH801T, which was purchased from Xinjiang Blue Mountain Tunhe Polyester Co., Ltd.

[0093] The PPCP, with a molecular weight of 52.5 kg / mol and a glass transition temperature (Tg) of 47° C., was purchased from Guangdong Tianxin New Materials Technology Co., Ltd.

[0094] The plasticizer can be glycerol, trimethylolpropane, pentaerythritol, triethyl citrate, low molecular weight polyester diol, polyether diol, etc.; a small molecule and a certain molecular weight plasticizer are selected for compounding and use, while achieving a certain plasticizing effect and having low migration; and the plasticizer described in the following embodiments of the present invention is glycerol, triethyl citrate, and PCL400 mixed in a mass ratio of 2:2:1.

[0095] The antioxidant is a hindered phenol; it can be antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant 2246, etc.; and the antioxidant described in the following embodiments of the present invention is antioxidant 1010.

[0096] The embodiment of the present invention also provides a method for preparing a multi-layer composite high-barrier PLA-based packaging film, comprising the following steps:

[0097] S31, mixing and plasticizing, i.e.

[0098] According to the formula, the raw materials are placed in a mixer at 40°C and mixed evenly, and then placed in different extruders for plasticization;

[0099] The PLA-based antibacterial layer raw materials were placed in a single-screw extruder, and the temperature zones were set to 150-190°C;

[0100] The PLA-based barrier layer raw material is placed in a single-screw extruder, and the temperature zones are set to 155-195°C;

[0101] The single screw extruder is a general screw with a length-to-diameter ratio of 32:1.

[0102] S32, co-extrusion, vacuum sizing, cooling and shaping, preheating, biaxial stretching, i.e.

[0103] The plasticized melt in S31 is fed into a three-layer co-extrusion circular die head for melt forming, and is subjected to vacuum sizing, cooling and shaping, hot water tank preheating, and biaxial stretching to obtain a primary film material;

[0104] The die temperature is 180-190°C;

[0105] The transverse stretching ratio is 2.5-3.0; the longitudinal stretching ratio is 2.5-3.0; and

[0106] The stretching temperature is 80-100° C.; the stretching rate is 50-60% / s.

[0107] S33, heat treatment, traction, winding, i.e.

[0108] The primary film material in S32 is heat treated at 90-100° C. for 10-20 min, and finally rolled up to obtain a multi-layer composite high-barrier PLA-based packaging film.

[0109] In order to further understand the present invention, a multi-layer composite high-barrier PLA-based packaging film provided by the present invention is described in detail below in conjunction with specific embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0110] Example 1

[0111] A method for preparing a compatibilizer comprises the following steps:

[0112] S11, N2 protection, phenyl methacrylate, methyl methacrylate, 2-isocyanatoethyl methacrylate, photoinitiator 184 were dissolved in anhydrous N,N-dimethylformamide A, stirred, and placed under UV device for UV curing for 10 minutes; after the reaction, the reaction device was removed, vacuum distilled, and vacuum dried at 40°C for 12 hours to obtain the target product, i.e., the compatibilizer ( PDI = 1.83).

[0113] The dosage ratio of the phenyl methacrylate, methyl methacrylate, 2-isocyanatoethyl methacrylate and anhydrous N,N-dimethylformamide A is 0.3 mol: 0.4 mol: 0.3 mol: 500 mL.

[0114] The amount of the photoinitiator 184 used is 2.0% of the total mass of the reactants.

[0115] Its infrared data are as follows: 2275cm -1 :-NCO exists; 1735cm -1 :-C=O exists; 3011cm -1 、1595cm -1 、1498cm -1 : Benzene ring exists; 1606cm -1 、811cm -1 :-C=C- does not exist.

[0116] A method for preparing a modified barrier filler comprises the following steps:

[0117] S21, adding graphene oxide and mercaptosilane coupling agent KH580 to anhydrous ethanol solvent, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain an intermediate product;

[0118] The usage ratio of the graphene oxide (hydroxyl content 5.0 mmol / g), mercaptosilane coupling agent KH580 and anhydrous ethanol solvent is 1 g:1.0 g:80 mL.

[0119] Its infrared data is as follows: 3445cm -1、1734cm -1 :-COOH exists (weak peak); 2953cm -1 :-CH exists; 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak); 1109cm -1 、801cm -1 :-Si-O- exists; 2550cm -1 :-SH exists.

[0120] S22, add the intermediate product, allyl glycidyl ether and photoinitiator 184 to anhydrous N,N-dimethylformamide B, stir, and place under UV device for UV curing for 10 minutes; remove the reaction device, continue stirring for 1 hour, distill under reduced pressure, and vacuum dry at 40°C for 12 hours to obtain the target product, i.e., the modified barrier filler.

[0121] The ratio of the intermediate product to allyl glycidyl ether is 1 mol:1 mol;

[0122] The usage ratio of the intermediate product to anhydrous N,N-dimethylformamide B is 1 g:50 mL;

[0123] The amount of the photoinitiator 184 used is 1.5% of the total mass of the reactants.

[0124] Its infrared data is as follows: 3445cm -1 、1734cm -1 :-COOH exists (weak peak); 2953cm -1 :-CH exists; 1218cm -1 、1104cm -1 : Epoxy groups exist and are enhanced; 1109cm -1 、801cm -1 :-Si-O- exists; 2550cm -1 :-SH does not exist; 1623cm -1 :-C=C- does not exist.

[0125] A multi-layer composite high-barrier PLA-based packaging film, the packaging film comprising three layers, namely an upper layer, a middle layer and a lower layer; the upper layer and the lower layer are both PLA-based antibacterial layers, the middle layer is a PLA-based barrier layer; the thickness ratio of the PLA-based antibacterial layer to the PLA-based barrier layer is 1:1.2;

[0126] The PLA-based antibacterial layer comprises the following raw materials in parts by weight:

[0127] PLA 70 parts;

[0128] PBAT 30 copies;

[0129] 1.5 parts of expander;

[0130] Chitosan 5.0 parts;

[0131] 0.3 parts of antioxidant;

[0132] The PLA-based barrier layer comprises the following raw materials in parts by weight:

[0133] PLA 80 parts;

[0134] PPCP 20 parts;

[0135] 10 parts of plasticizer;

[0136] 2.0 parts of modified barrier filler;

[0137] 0.4 parts of antioxidant.

[0138] A method for preparing a multi-layer composite high-barrier PLA-based packaging film comprises the following steps:

[0139] S31, mixing and plasticizing, i.e.

[0140] According to the formula, the raw materials are placed in a mixer at 40°C and mixed evenly, and then placed in different extruders for plasticization;

[0141] The PLA-based antibacterial layer raw material is placed in a single-screw extruder, and the temperature of zone 1 is set to 150°C, zone 2 is set to 170°C, zone 3 is set to 180°C, zone 4 is set to 180°C, and zone 5 is set to 175°C.

[0142] The PLA-based barrier layer raw material was placed in a single-screw extruder, and the temperature was set at 160°C in zone 1, 175°C in zone 2, 185°C in zone 3, 185°C in zone 4, and 180°C in zone 5;

[0143] S32, co-extrusion, vacuum sizing, cooling and shaping, preheating, biaxial stretching, i.e.

[0144] The plasticized melt in S31 is fed into a three-layer co-extrusion circular die head for melt forming, and is subjected to vacuum sizing, cooling and shaping, hot water tank preheating, and biaxial stretching to obtain a primary film material;

[0145] The die temperature is 185°C;

[0146] The transverse stretching ratio is 2.8; the longitudinal stretching ratio is 2.8; and

[0147] The stretching temperature is 90° C. and the stretching rate is 60% / s.

[0148] S33, heat treatment, traction, winding, i.e.

[0149] The primary film material in S32 was heat treated at 100°C for 10 min and finally rolled up to obtain a multi-layer composite high-barrier PLA-based packaging film.

[0150] Example 2

[0151] The rest is the same as in Example 1, except that:

[0152] A method for preparing a compatibilizer comprises the following steps:

[0153] S11, N2 protection, phenyl methacrylate, methyl methacrylate, 2-isocyanatoethyl methacrylate, photoinitiator 184 were dissolved in anhydrous N,N-dimethylformamide A, stirred, and placed under UV device for UV curing for 5 minutes; after the reaction was completed, the reaction device was removed, vacuum distilled, and vacuum dried at 40°C for 12 hours to obtain the target product, i.e., the compatibilizer ( PDI = 2.31).

[0154] The usage ratio of phenyl methacrylate, methyl methacrylate, 2-isocyanatoethyl methacrylate and anhydrous N,N-dimethylformamide A is 0.4 mol: 0.4 mol: 0.2 mol: 500 mL.

[0155] The amount of the photoinitiator 184 used is 4.0% of the total mass of the reactants.

[0156] Its infrared data are as follows: 2275cm -1 :-NCO exists; 1735cm -1 :-C=O exists; 3011cm -1 、1595cm -1 、1498cm -1 : Benzene ring exists; 1606cm -1 、811cm -1 :-C=C- does not exist.

[0157] A method for preparing a modified barrier filler comprises the following steps:

[0158] S21, adding graphene oxide and mercaptosilane coupling agent KH580 to anhydrous ethanol solvent, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 50° C. for 10 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain an intermediate product;

[0159] The usage ratio of the graphene oxide (hydroxyl content: 3.0 mmol / g), mercaptosilane coupling agent KH580 and anhydrous ethanol solvent is 1 g:0.8 g:80 mL.

[0160] Its infrared data is as follows: 3445cm-1 、1734cm -1 :-COOH exists (weak peak); 2953cm -1 :-CH exists; 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak); 1109cm -1 、801cm -1 :-Si-O- exists; 2550cm -1 :-SH exists.

[0161] S22, add the intermediate product and allyl glycidyl ether to anhydrous N,N-dimethylformamide B, stir, and place under a UV device for UV curing for 120 minutes; remove the reaction device, continue stirring for 1 hour, distill under reduced pressure, and vacuum dry at 40°C for 12 hours to obtain the target product, i.e., the modified barrier filler.

[0162] The ratio of the intermediate product to allyl glycidyl ether is 1 mol:1 mol;

[0163] The usage ratio of the intermediate product to anhydrous N,N-dimethylformamide B is 1 g:50 mL.

[0164] Its infrared data is as follows: 3445cm -1 、1734cm -1 :-COOH exists (weak peak); 2953cm -1 :-CH exists; 1218cm -1 、1104cm -1 : Epoxy groups exist and are enhanced; 1109cm -1 、801cm -1 :-Si-O- exists; 2550cm -1 :-SH does not exist; 1623cm -1 :-C=C- does not exist.

[0165] Example 3

[0166] The rest is the same as in Example 1, except that:

[0167] A method for preparing a compatibilizer comprises the following steps:

[0168] S11, N2 protection, phenyl methacrylate, methyl methacrylate, 2-isocyanatoethyl methacrylate, photoinitiator 184 were dissolved in anhydrous N,N-dimethylformamide A, stirred, and placed under UV device for UV curing for 30 minutes; after the reaction, the reaction device was removed, vacuum distilled, and vacuum dried at 40°C for 12 hours to obtain the target product, i.e., the compatibilizer ( PDI = 1.76).

[0169] The dosage ratio of the phenyl methacrylate, methyl methacrylate, 2-isocyanatoethyl methacrylate and anhydrous N,N-dimethylformamide A is 0.2 mol: 0.5 mol: 0.3 mol: 500 mL.

[0170] The amount of the photoinitiator 184 used is 1.0% of the total mass of the reactants.

[0171] Its infrared data are as follows: 2275cm -1 :-NCO exists; 1735cm -1 :-C=O exists; 3011cm -1 、1595cm -1 、1498cm -1 : Benzene ring exists; 1606cm -1 、811cm -1 :-C=C- does not exist.

[0172] A method for preparing a modified barrier filler comprises the following steps:

[0173] S21, adding graphene oxide and mercaptosilane coupling agent KH580 to anhydrous ethanol solvent, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 70° C. for 4 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain an intermediate product;

[0174] The usage ratio of the graphene oxide (hydroxyl content 8.0 mmol / g), mercaptosilane coupling agent KH580 and anhydrous ethanol solvent is 1 g:1.5 g:80 mL.

[0175] Its infrared data is as follows: 3445cm -1 、1734cm -1 :-COOH exists (weak peak); 2953cm -1 :-CH exists; 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak); 1109cm -1 、801cm -1 :-Si-O- exists; 2550cm -1 :-SH exists.

[0176] S22, add the intermediate product, allyl glycidyl ether and photoinitiator 184 to anhydrous N,N-dimethylformamide B, stir, and place under UV device for UV curing for 5 minutes; remove the reaction device, continue stirring for 1 hour, distill under reduced pressure, and vacuum dry at 40°C for 12 hours to obtain the target product, i.e., the modified barrier filler.

[0177] The ratio of the intermediate product to allyl glycidyl ether is 1 mol:1 mol;

[0178] The usage ratio of the intermediate product to anhydrous N,N-dimethylformamide B is 1 g:50 mL;

[0179] The amount of the photoinitiator 184 used is 2.0% of the total mass of the reactants.

[0180] Its infrared data is as follows: 3445cm -1 、1734cm -1 :-COOH exists (weak peak); 2953cm -1 :-CH exists; 1218cm -1 、1104cm -1 : Epoxy groups exist and are enhanced; 1109cm -1 、801cm -1 :-Si-O- exists; 2550cm -1 :-SH does not exist; 1623cm -1 :-C=C- does not exist.

[0181] Example 4

[0182] The rest is the same as in Example 1, except that:

[0183] A method for preparing a compatibilizer comprises the following steps:

[0184] S11, N2 protection, phenyl methacrylate, methyl methacrylate, 2-isocyanatoethyl methacrylate, photoinitiator 184 were dissolved in anhydrous N,N-dimethylformamide A, stirred, and placed under UV device for UV curing for 10 minutes; after the reaction, the reaction device was removed, vacuum distilled, and vacuum dried at 40°C for 12 hours to obtain the target product, i.e., the compatibilizer ( PDI = 2.22).

[0185] The dosage ratio of the phenyl methacrylate, methyl methacrylate, 2-isocyanatoethyl methacrylate and anhydrous N,N-dimethylformamide A is 0.3 mol: 0.3 mol: 0.4 mol: 500 mL.

[0186] The amount of the photoinitiator 184 used is 3.0% of the total mass of the reactants.

[0187] Its infrared data are as follows: 2275cm -1 :-NCO exists; 1735cm -1 :-C=O exists; 3011cm -1 、1595cm -1、1498cm -1 : Benzene ring exists; 1606cm -1 、811cm -1 :-C=C- does not exist.

[0188] A method for preparing a modified barrier filler comprises the following steps:

[0189] S21, adding graphene oxide and mercaptosilane coupling agent KH580 to anhydrous ethanol solvent, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain an intermediate product;

[0190] The usage ratio of the graphene oxide (hydroxyl content 5.0 mmol / g), mercaptosilane coupling agent KH580 and anhydrous ethanol solvent is 1 g:1.0 g:80 mL.

[0191] Its infrared data is as follows: 3445cm -1 、1734cm -1 :-COOH exists (weak peak); 2953cm -1 :-CH exists; 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak); 1109cm -1 、801cm -1 :-Si-O- exists; 2550cm -1 :-SH exists.

[0192] S22, add the intermediate product, allyl glycidyl ether and photoinitiator 184 to anhydrous N,N-dimethylformamide B, stir, and place under UV device for UV curing for 40 minutes; remove the reaction device, continue stirring for 1 hour, distill under reduced pressure, and vacuum dry at 40°C for 12 hours to obtain the target product, i.e., the modified barrier filler.

[0193] The ratio of the intermediate product to allyl glycidyl ether is 1 mol:1 mol;

[0194] The usage ratio of the intermediate product to anhydrous N,N-dimethylformamide B is 1 g:50 mL;

[0195] The amount of the photoinitiator 184 used is 1.0% of the total mass of the reactants.

[0196] Its infrared data is as follows: 3445cm -1 、1734cm -1 :-COOH exists (weak peak); 2953cm -1 :-CH exists; 1218cm -1 、1104cm-1 : Epoxy groups exist and are enhanced; 1109cm -1 、801cm -1 :-Si-O- exists; 2550cm -1 :-SH does not exist; 1623cm -1 :-C=C- does not exist.

[0197] Example 5

[0198] The rest is the same as in Example 1, except that:

[0199] The thickness ratio of the PLA-based antibacterial layer to the PLA-based barrier layer is 1:1.0.

[0200] Example 6

[0201] The rest is the same as in Example 1, except that:

[0202] The thickness ratio of the PLA-based antibacterial layer to the PLA-based barrier layer is 1:1.5.

[0203] Example 7

[0204] The rest is the same as in Example 1, except that:

[0205] A multi-layer composite high barrier PLA-based packaging film,

[0206] The PLA-based antibacterial layer comprises the following raw materials in parts by weight:

[0207] PLA 60 parts;

[0208] PBAT 40 parts;

[0209] 2.0 parts of compatibilizer;

[0210] Chitosan 4.0 parts;

[0211] Antioxidant 0.1 part;

[0212] The PLA-based barrier layer comprises the following raw materials in parts by weight:

[0213] PLA 90 parts;

[0214] PPCP 10 parts;

[0215] 8 parts of plasticizer;

[0216] 3.0 parts of modified barrier filler;

[0217] 0.5 parts of antioxidant.

[0218] A method for preparing a multi-layer composite high-barrier PLA-based packaging film comprises the following steps:

[0219] S31, mixing and plasticizing, i.e.

[0220] According to the formula, the raw materials are placed in a mixer at 40°C and mixed evenly, and then placed in different extruders for plasticization;

[0221] The PLA-based antibacterial layer raw material is placed in a single-screw extruder, and the temperature of zone 1 is set to 160°C, zone 2 is set to 170°C, zone 3 is set to 170°C; zone 4 is set to 180°C; zone 5 is set to 170°C;

[0222] The PLA-based barrier layer raw material was placed in a single-screw extruder, and the temperature of zone 1 was set to 175°C, zone 2 to 185°C, zone 3 to 185°C, zone 4 to 195°C, and zone 5 to 185°C.

[0223] S32, co-extrusion, vacuum sizing, cooling and shaping, preheating, biaxial stretching, i.e.

[0224] The plasticized melt in S31 is fed into a three-layer co-extrusion circular die head for melt forming, and is subjected to vacuum sizing, cooling and shaping, hot water tank preheating, and biaxial stretching to obtain a primary film material;

[0225] The die temperature is 190°C;

[0226] The transverse stretching ratio is 2.5; the longitudinal stretching ratio is 2.5; and

[0227] The stretching temperature is 80° C. and the stretching rate is 50% / s.

[0228] S33, heat treatment, traction, winding, i.e.

[0229] The primary film material in S32 was heat treated at 90°C for 20 min and finally rolled up to obtain a multi-layer composite high-barrier PLA-based packaging film.

[0230] Example 8

[0231] The rest is the same as in Example 1, except that:

[0232] A multi-layer composite high barrier PLA-based packaging film,

[0233] The PLA-based antibacterial layer comprises the following raw materials in parts by weight:

[0234] PLA 80 parts;

[0235] PBAT 20 copies;

[0236] 1.0 part of compatibilizer;

[0237] Chitosan 6.0 parts;

[0238] 0.5 parts of antioxidant;

[0239] The PLA-based barrier layer comprises the following raw materials in parts by weight:

[0240] PLA 70 parts;

[0241] PPCP 30 parts;

[0242] 12 parts of plasticizer;

[0243] 1.0 part of modified barrier filler;

[0244] Antioxidant 0.1 part.

[0245] A method for preparing a multi-layer composite high-barrier PLA-based packaging film comprises the following steps:

[0246] S31, mixing and plasticizing, i.e.

[0247] According to the formula, the raw materials are placed in a mixer at 40°C and mixed evenly, and then placed in different extruders for plasticization;

[0248] The PLA-based antibacterial layer raw material is placed in a single-screw extruder, and the temperature of zone 1 is set to 170°C, zone 2 is set to 190°C, zone 3 is set to 190°C, zone 4 is set to 190°C, and zone 5 is set to 180°C.

[0249] The PLA-based barrier layer raw material was placed in a single-screw extruder, and the temperature of zone 1 was set to 155°C, zone 2 to 175°C, zone 3 to 185°C; zone 4 to 180°C; and zone 5 to 175°C.

[0250] S32, co-extrusion, vacuum sizing, cooling and shaping, preheating, biaxial stretching, i.e.

[0251] The plasticized melt in S31 is fed into a three-layer co-extrusion circular die head for melt forming, and is subjected to vacuum sizing, cooling and shaping, hot water tank preheating, and biaxial stretching to obtain a primary film material;

[0252] The die temperature is 180°C;

[0253] The transverse stretching ratio is 3.0; the longitudinal stretching ratio is 3.0; and

[0254] The stretching temperature is 100° C. and the stretching rate is 60% / s.

[0255] S33, heat treatment, traction, winding, i.e.

[0256] The primary film material in S32 was heat treated at 90°C for 20 min and finally rolled up to obtain a multi-layer composite high-barrier PLA-based packaging film.

[0257] The following comparative examples are compared with specific embodiment 1:

[0258] Comparative Example 1

[0259] The rest is the same as in Example 1, except that:

[0260] No compatibilizer is added to the raw material formula of the PLA-based antibacterial layer.

[0261] Comparative Example 2

[0262] The rest is the same as in Example 1, except that:

[0263] The 2-isocyanatoethyl methacrylate was replaced with glycidyl methacrylate.

[0264] Comparative Example 3

[0265] The rest is the same as in Example 1, except that:

[0266] No modified barrier filler is added to the raw material formula of the PLA-based barrier layer.

[0267] Comparative Example 4

[0268] The rest is the same as in Example 1, except that:

[0269] The modified barrier filler is replaced with the corresponding graphene oxide.

[0270] Comparative Example 5

[0271] The rest is the same as in Example 1, except that:

[0272] A method for preparing a modified barrier filler comprises the following steps:

[0273] S21, adding graphene oxide and silane coupling agent KH560 to anhydrous ethanol solvent, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain an intermediate product;

[0274] The usage ratio of the graphene oxide (hydroxyl content 5.0 mmol / g), the silane coupling agent KH560 and the anhydrous ethanol solvent is 1 g:1.0 g:80 mL.

[0275] Its infrared data is as follows: 3445cm -1 、1734cm -1 :-COOH exists (weak peak); 2953cm -1 :-CH exists; 1218cm -1 、1104cm -1 : Epoxy group exists; 1109cm -1 、801cm -1 :-Si-O- exists.

[0276] Comparative Example 6

[0277] The rest is the same as in Example 1, except that:

[0278] No PPCP is added to the PLA-based barrier layer raw material formula.

[0279] Comparative Example 7

[0280] The rest is the same as in Example 1, except that:

[0281] In the preparation method of the multi-layer composite high-barrier PLA-based packaging film, no biaxial stretching process is performed.

[0282] Comparative Example 8

[0283] The rest is the same as in Example 1, except that:

[0284] The high-barrier PLA-based packaging film is a single-layer film with a PLA-based antibacterial layer.

[0285] Comparative Example 9

[0286] The rest is the same as in Example 1, except that:

[0287] The high-barrier PLA-based packaging film is a single-layer film of a PLA-based barrier layer.

[0288] The physical properties of the multi-layer composite high barrier PLA-based packaging films in the embodiments of the present invention and the comparative examples are respectively measured and the results are shown in Table 1.

[0289] Table 1 Physical test performance of each embodiment

[0290]

[0291]

[0292] First, it can be concluded from Examples 1-8 in Table 1 that the multi-layer composite high-barrier PLA-based packaging film of the present invention has excellent mechanical properties and water vapor and oxygen barrier properties.

[0293] Second, it can be observed from Example 1 and Comparative Examples 1-2 that the multi-layer composite high barrier PLA-based packaging film of the present invention uses a homemade compatibilizer, which has a significant effect on improving mechanical properties, etc.; at the same time, the homemade compatibilizer has a higher reactivity and has a more significant effect than the conventional epoxy-based compatibilizer, which is reflected in mechanical properties, interlayer adhesion, etc.;

[0294] It can be observed from Example 1 and Comparative Examples 3-6 that in the multi-layer composite high-barrier PLA-based packaging film of the present invention, the self-made modified barrier filler has excellent barrier effects on both water vapor and oxygen; at the same time, it can be found that the modified filler has better compatibility and better effect; there are also certain requirements for the modified organic chain used, and the barrier effect of organic chains with a certain chain length is better. The possible reason is that in the later biaxial stretching process, the long chain structure helps the filler to move in the orientation direction, thereby achieving a better barrier effect; in addition, PPCP resin has a good barrier effect on water vapor, and has a synergistic barrier effect when used in combination with the modified barrier filler;

[0295] It can be observed from Example 1 and Comparative Example 7 that the multi-layer composite high-barrier PLA-based packaging film of the present invention has better barrier properties after biaxial stretching, and the mechanical properties are significantly improved;

[0296] It can be observed from Example 1 and Comparative Examples 8-9 that the multi-layer composite high barrier PLA-based packaging film of the present invention and the three-layer co-extruded composite material have better comprehensive properties such as mechanical properties and barrier properties than single-layer materials.

[0297] In summary, the multi-layer composite high-barrier PLA-based packaging film provided by the present invention, on the one hand, has a self-made high-reactivity compatibilizer and a modified barrier filler through molecular design; on the other hand, a three-layer structure is designed through a formula; and it is prepared by a three-layer co-extrusion and biaxial stretching process, and has excellent mechanical properties, barrier properties and other comprehensive properties; and the subject raw materials used have the advantage of being completely degradable and widely used.

[0298] The test method is as follows:

[0299] (1) Mechanical properties: Tested according to the method described in GB / T 1040.3-2006.

[0300] (2) Water vapor permeability: tested in accordance with the method described in GB / T 1037-2021; the average thickness of the film to be tested is 50 μm.

[0301] (3) Oxygen permeability: tested in accordance with the method described in GB / T 1038.1-2022. The test conditions are 1 atm. The average thickness of the film to be tested is 50 μm.

[0302] (4) Antibacterial rate: The test was conducted according to the method described in ASTM E2180-07 (2012). The test bacteria species was Staphylococcus aureus.

[0303] (5) Whether there is splitting: observe whether there is splitting after the mechanical properties test. If there is obvious splitting, the interlayer adhesion is poor; if there is no obvious splitting, the interlayer adhesion is good. The marking method for splitting is: no obvious splitting, marked as "○"; slight splitting, marked as "◎"; obvious splitting, marked as "●".

[0304] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a compatibilizer, characterized in that: The following steps are involved: S11, UV curing aromatic acrylate, aliphatic acrylate and isocyanate acrylate under a photoinitiator to obtain a target product, i.e., a compatibilizer.

2. The method for preparing the compatibilizer according to claim 1, characterized in that: The usage ratio of the aromatic acrylate, the aliphatic acrylate and the isocyanate acrylate is 0.2-0.4 mol: 0.3-0.5 mol: 0.2-0.4 mol.

3. A compatibilizer, characterized in that The compatibilizer is prepared by the method for preparing the compatibilizer as claimed in claim 1 or 2.

4. A method for preparing a modified barrier filler, characterized in that: The following steps are involved: S21, placing the barrier filler and the mercaptosilane coupling agent in an alcohol solvent for silylation coupling reaction to obtain an intermediate product; S22, click-reacting the intermediate product with an olefin monomer to obtain a target product, i.e., a modified barrier filler.

5. The method for preparing the modified barrier filler according to claim 4, characterized in that: The usage ratio of the barrier filler, the mercaptosilane coupling agent and the alcohol solvent is 1g: 0.8-1.5g: 80mL; and The barrier filler is a lamellar structure.

6. The method for preparing the modified barrier filler according to claim 4, characterized in that: The ratio of the intermediate product to the olefin monomer is 1 mol:1 mol; and The vinyl monomer is a monomer containing an epoxy group or an isocyanate structure.

7. A modified barrier filler, characterized in that: The modified barrier filler is prepared by the preparation method of any one of claims 4 to 6.

8. A multi-layer composite high barrier PLA-based packaging film, characterized in that: The packaging film comprises three layers, namely an upper layer, a middle layer and a lower layer; the upper layer and the lower layer are both PLA-based antibacterial layers, and the middle layer is a PLA-based barrier layer; the thickness ratio of the PLA-based antibacterial layer to the PLA-based barrier layer is 1:1.0-1.5; The PLA-based antibacterial layer comprises the following raw materials in parts by weight: PLA 60-80 parts; PBAT 20-40 parts; 1.0-2.0 parts of compatibilizer; Chitosan 4.0-6.0 parts; Antioxidant 0.1-0.5 parts; Among them, the total mass of PLA and PBAT is 100 parts; The PLA-based barrier layer comprises the following raw materials in parts by weight: PLA 70-90 parts; PPCP 10-30 parts; 8-12 parts of plasticizer; 1.0-3.0 parts of modified barrier filler; Antioxidant 0.1-0.5 parts; Among them, the total mass of PLA and PPCP is 100 parts.

9. A method for preparing a multi-layer composite high barrier PLA-based packaging film, characterized in that: The steps include: S31, mixing and plasticizing, i.e. Mix all the raw materials evenly according to the formula and put them in different extruders for plasticization; S32, co-extrusion, vacuum sizing, cooling and shaping, preheating, biaxial stretching, i.e. The plasticized melt in S31 is fed into a three-layer co-extrusion circular die head for melt forming, and is subjected to vacuum sizing, cooling and shaping, preheating, and biaxial stretching to obtain a primary film material; as well as S33, heat treatment, traction, winding, i.e. The primary film material in S32 is heat treated and finally rolled up to obtain a multi-layer composite high-barrier PLA-based packaging film.

10. The method for preparing the multi-layer composite high barrier PLA-based packaging film according to claim 9, characterized in that: The die temperature is 180-190°C; The transverse stretching ratio is 2.5-3.0; the longitudinal stretching ratio is 2.5-3.0; and The stretching temperature is 80-100° C.; the stretching rate is 50-60% / s.