Conductive wear-resistant nitrile rubber material and preparation method thereof
By scientifically matching carbon nanotube graphene nitrile rubber masterbatch with nitrile rubber, and combining it with additives such as high wear-resistant carbon black, a two-step process is used to prepare conductive and wear-resistant nitrile rubber. This solves the problems of complex processes and high costs in existing technologies, and achieves improved material conductivity and wear resistance, as well as ease of industrialization.
Patent Information
- Application Number
- CN202411172662.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-08
AI Technical Summary
The existing conductive and wear-resistant nitrile rubber materials have complex manufacturing processes, high manufacturing costs, and are difficult to mass-produce.
A conductive and wear-resistant nitrile rubber material is prepared by scientifically matching carbon nanotube graphene nitrile rubber masterbatch with nitrile rubber, and with the help of high wear-resistant carbon black, zinc oxide, stearic acid, antioxidant, dispersant, plasticizer, vulcanization accelerator and sulfur, through a two-step process, including liquid phase wet mixing and internal mixing, and open milling.
It improves the electrical conductivity and wear resistance of nitrile rubber materials, simplifies the process, and facilitates industrial production.
Smart Images

Figure BDA0005010417810000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber preparation, and in particular to a conductive wear-resistant nitrile rubber material and a preparation method thereof. Background Art
[0002] Nitrile rubber (NBR) is a copolymer formed by the polymerization of acrylonitrile and butadiene monomers, and is mainly produced by low-temperature emulsion polymerization. NBR has excellent oil resistance and is mainly used to make oil-resistant rubber products. The acrylonitrile content (%) in NBR is 42-46%, 36-41%, 31-35%, 25-30%, and 18-24%. The higher the acrylonitrile content, the better the oil resistance. NBR can be used for a long time in hot air at 120°C or oil at 150°C. In addition, it also has good water resistance, air tightness and excellent bonding properties. However, the strength of nitrile rubber materials is not high, it is prone to wear, and its electrical properties are poor.
[0003] Existing publication number is the Chinese patent of CN107501656B, discloses a preparation method of a conductive wear-resistant nitrile rubber material, by subjecting graphite to microwave treatment to obtain expanded graphite, and ultrasonic treatment, the expanded graphite is dispersed into nano graphite flakes by vibration, the nano graphite flakes and acrylonitrile and butadiene are copolymerized, under emulsion blending, the nano graphite flakes active points and rubber molecules are self-vulcanized to form a conductive network, thereby achieving the effect of improving poor electrical conductivity. Due to the polar interaction between the groups, the activity of the nitrile rubber segment is greatly reduced. Modified bentonite is added in the plasticizing process, which can produce larger hysteresis loss during friction, and the rubber material on the friction surface is destroyed to form abrasive particles, which can improve the adhesion of the rubber material to the friction surface, thereby achieving the purpose of improving wear resistance.
[0004] However, the manufacturing process of the above conductive wear-resistant nitrile rubber material is complicated, the manufacturing cost is high, and it is difficult to produce on a large scale. Summary of the invention
[0005] The purpose of the present invention is to provide a conductive wear-resistant nitrile rubber material and a preparation method thereof, aiming to solve the problems of complex manufacturing process, high manufacturing cost and difficulty in large-scale production of conductive wear-resistant nitrile rubber materials in the prior art.
[0006] In order to solve the above technical problems, the present invention is mainly implemented through the following technical solutions:
[0007] In a first aspect, the present invention provides a conductive wear-resistant nitrile rubber material, comprising the following components in parts by weight:
[0008] 70-80 parts of nitrile rubber, 20-30 parts of carbon nanotube graphene nitrile masterbatch, 30-45 parts of high wear-resistant carbon black, 5-8 parts of zinc oxide, 2-5 parts of stearic acid, 3-5 parts of antioxidant, 2-5 parts of dispersant, 5-20 parts of plasticizer, 1-3 parts of vulcanization accelerator, and 1-3 parts of sulfur.
[0009] In the present invention, the nitrile rubber has excellent oil resistance, chemical stability and water resistance, and the general heat resistance temperature is as high as 120°C. Since the nitrile rubber is a polymer material, there are very few movable ions or free electrons in the structure to conduct electricity, so it is basically not conductive and belongs to an insulator. In the carbon nanotube graphene nitrile masterbatch, the carbon nanotube and the graphene are both composed of pure carbon atoms, but the arrangement and combination of carbon atoms are different, forming spiral carbon nanotubes and sheet graphene, so they all have some common characteristics, such as conductivity; the present invention scientifically matches the nitrile rubber and the carbon nanotube graphene nitrile masterbatch, and under the action of high wear-resistant carbon black, zinc oxide, stearic acid, antioxidant, dispersant, plasticizer, vulcanization accelerator and sulfur, the conductive performance of the nitrile rubber material is greatly improved; this nitrile rubber material also greatly improves wear resistance and mechanical properties.
[0010] As a preferred embodiment, the carbon nanotube content in the carbon nanotube graphene nitrile masterbatch is 5% to 15%, and the graphene content in the carbon nanotube graphene nitrile masterbatch is 5% to 15%. The carbon nanotubes and graphene in the carbon nanotube graphene nitrile masterbatch of the present invention improve the conductivity of the nitrile rubber material.
[0011] As a preferred embodiment, the antioxidant includes any one or a combination of N-cyclohexyl-N'-phenyl-p-phenylenediamine (anti-aging agent 4010), N-phenyl-N'-isopropyl-p-phenylenediamine (anti-aging agent 4010NA), N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (anti-aging agent 4020), 2,2,4-trimethyl-1,2-dihydroquinoline polymer (anti-aging agent RD) or 2-thiol benzimidazole (anti-aging agent MB). The addition of the antioxidant in the present invention further increases the aging resistance of the nitrile rubber material, and the antioxidant has many types, a wide source, and is easy to use.
[0012] As a preferred embodiment, the dispersant includes any one or a combination of microcrystalline wax or paraffin wax. The dispersant selected in the present invention can promote the movement and interaction of rubber molecules, make the dispersion of fillers in rubber more uniform, and improve the performance and stability of nitrile rubber materials.
[0013] As a preferred embodiment, the vulcanization accelerator includes any one or a combination of N-cyclohexyl-2-benzothiazole sulfenamide (accelerator CZ), 2-thiol benzothiazole (accelerator M), benzothiazole disulfide (accelerator DM) or tetramethylthiuram disulfide (accelerator TMTD). The vulcanization accelerator of the present invention can promote the vulcanization reaction, improve the scorching performance of the rubber material, and improve the physical and mechanical properties of the rubber material; it can reduce the amount of sulfur, avoid the sulfur spraying phenomenon, and at the same time reduce the vulcanization temperature and shorten the vulcanization time; accelerator CZ belongs to the sulfenamide class, has a long scorching time and high vulcanization activity; M and DM belong to the thiazole class, have high vulcanization activity, and can give the vulcanized rubber good aging resistance and fatigue resistance; vulcanization accelerator TMTD can improve the heat resistance and aging resistance of the nitrile rubber material.
[0014] As a preferred embodiment, the plasticizer comprises any one or a combination of liquid nitrile rubber, dioctyl phthalate, tributyl acetyl citrate, di(butoxyethoxyethyl) adipate, mixed ether ester, dioctyl trimellitate, dioctyl terephthalate or diisononyl phthalate. The plasticizer of the present invention can increase the distance between polymer molecular chains, weaken the interaction force between polymer molecules, play a role in blocking crystallization and increasing polymer processing plasticity, flexibility and processability.
[0015] In a second aspect, the present invention provides a method for preparing a conductive wear-resistant nitrile rubber material as described in any one of the embodiments of the first aspect above, comprising the following steps:
[0016] Step (1) firstly uses a coupling agent to modify graphene and carbon nanotubes respectively, and set them aside; then takes deionized water in a beaker, adds a water-soluble dispersant into the beaker, stirs, then adds the modified graphene and carbon nanotubes, continues to stir, and obtains a mixed solution of graphene and carbon nanotubes; takes nitrile latex and slowly adds it to the mixed solution of graphene and carbon nanotubes, stirs, then adds a flocculant to flocculate, collects the flocculated solid mixture with a filter, washes it with deionized water for 3 to 5 times, and then puts it into an oven for drying, and obtains a carbon nanotube graphene nitrile masterbatch for standby use;
[0017] Step (2) setting the initial temperature of the internal mixer to 60-80°C and the rotation speed to 60-80rpm, then putting the nitrile rubber and the carbon nanotube graphene nitrile masterbatch into the internal mixer, first plasticizing for 1-3min, then sequentially putting zinc oxide, stearic acid, antioxidant and dispersant into the internal mixer, continuing to internally mix for 1-3min, then putting high wear-resistant carbon black and plasticizer into the internal mixer, continuing to internally mix for 2-5min, lifting the top bolt of the internal mixer for cleaning, and then continuing to internally mix until the temperature is about 120-150°C to discharge the glue to obtain a film;
[0018] Step (3) adjusting the roller spacing of the open mill to 1.5 mm, adding the rubber sheet obtained in step (2) into the open mill for plasticizing 2 to 3 times, then adding sulfur and vulcanization accelerator, turning the rubber sheet left and right three times each, then adjusting the roller spacing of the open mill to 0.2 mm, performing thin passes 6 to 8 times, discharging the material, and leaving it at room temperature for 12 hours to obtain a rubber mix; finally, vulcanizing and performing performance tests on the rubber mix.
[0019] The preparation method of the conductive wear-resistant nitrile rubber material of the present invention is mainly completed by a two-step method. First, a carbon nanotube graphene nitrile masterbatch is prepared by a liquid phase wet mixing process, thereby improving the dispersion of carbon nanotubes and graphene in rubber, making the carbon nanotubes, graphene and rubber molecular chains fully combined, and improving the conductive network; then, the nitrile rubber, the carbon nanotube graphene nitrile masterbatch and various processing aids are evenly mixed by internal mixing and open mixing; the process is simple, the operation is convenient, and it is easy to realize industrialization.
[0020] As a preferred embodiment, the water-soluble dispersant in step (1) includes any one or a combination of sodium dodecylbenzene sulfonate, polyethylene glycol, acrylic resin or hydroxymethyl cellulose. The present invention can reduce the surface tension of water by adding a water-soluble dispersant, improve the dispersibility of graphene and carbon nanotubes in water, avoid agglomeration, and improve the conductivity, mechanical strength and chemical stability of the nitrile rubber material.
[0021] As a preferred embodiment, the flocculant comprises any one or a combination of calcium chloride, sodium chloride, dilute sulfuric acid, acetic acid or formic acid. In the present invention, by adding a flocculant to the nitrile latex, the flocculant plays a bridging role between the nitrile latex particles, promotes the aggregation of the nitrile latex particles, thereby making the suspended particles in the latex aggregate larger or form flocs, accelerating the coagulation of the particles, and achieving the purpose of solid-liquid separation.
[0022] As a preferred embodiment, the drying temperature in step (1) is 50-80° C. and the drying time is 24-40 hours. By drying the flocculated nitrile latex, the residual solvent can be removed to obtain the product.
[0023] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention scientifically matches nitrile rubber and carbon nanotube graphene nitrile masterbatch, and greatly improves the conductive properties of nitrile rubber materials under the action of high wear-resistant carbon black, zinc oxide, stearic acid, antioxidant, dispersant, plasticizer, vulcanization accelerator and sulfur; the nitrile rubber material also greatly improves wear resistance and mechanical properties. The preparation method mainly adopts two steps, firstly, the carbon nanotube graphene nitrile masterbatch is prepared by adopting a liquid phase wet mixing process, the dispersion of carbon nanotubes and graphene in rubber is improved, the carbon nanotubes, graphene and rubber molecular chains are fully combined, and the conductive network is improved; then, the nitrile rubber, carbon nanotube graphene nitrile masterbatch and various processing aids are evenly mixed by internal mixing and open mixing; the process is simple, the operation is convenient, and it is easy to realize industrialization. DETAILED DESCRIPTION
[0024] The technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Carbon nanotubes (CNTs) are one-dimensional quantum materials with a special structure (radial dimensions are nanometers, axial dimensions are micrometers, and both ends of the tube are basically sealed). Carbon nanotubes are mainly composed of several to dozens of layers of coaxial circular tubes composed of carbon atoms arranged in hexagons. The distance between layers is fixed, about 0.34nm, and the diameter is generally 2-20nm. And according to the different orientations of carbon hexagons along the axial direction, they can be divided into three types: zigzag, armchair, and spiral. Carbon nanotubes have good electrical conductivity. Since the structure of carbon nanotubes is the same as the lamellar structure of graphite, they have good electrical properties. Theoretical predictions show that their electrical conductivity depends on their tube diameter and the spiral angle of the tube wall. When the diameter of CNTs is greater than 6nm, the electrical conductivity decreases; when the diameter is less than 6nm, CNTs can be regarded as one-dimensional quantum wires with good electrical conductivity.
[0026] Graphene is a two-dimensional carbon nanomaterial composed of carbon atoms in a hexagonal honeycomb lattice with sp2 hybrid orbitals. Graphene has excellent optical, electrical and mechanical properties, and has important application prospects in materials science, energy, biomedicine and drug delivery, and is considered to be a revolutionary material of the future.
[0027] The conductive wear-resistant nitrile rubber material of the present invention comprises the following components in parts by weight: 70-80 parts of nitrile rubber, 20-30 parts of carbon nanotube graphene nitrile masterbatch, 30-45 parts of high wear-resistant carbon black, 5-8 parts of zinc oxide, 2-5 parts of stearic acid, 3-5 parts of antioxidant, 2-5 parts of dispersant, 5-20 parts of plasticizer, 1-3 parts of vulcanization accelerator and 1-3 parts of sulfur.
[0028] Furthermore, the carbon nanotube content in the carbon nanotube-graphene nitrile masterbatch is 5% to 15%, and the graphene content is 5% to 15%.
[0029] Furthermore, the antioxidant includes any one or a combination of N-cyclohexyl-N'-phenyl-p-phenylenediamine (antioxidant 4010), N-phenyl-N'-isopropyl-p-phenylenediamine (antioxidant 4010NA), N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (antioxidant 4020), 2,2,4-trimethyl-1,2-dihydroquinoline polymer (antioxidant RD), and 2-thiol benzimidazole (antioxidant MB).
[0030] Furthermore, the dispersant includes any one of microcrystalline wax and paraffin wax, or a combination of both.
[0031] Furthermore, the vulcanization accelerator includes any one or a combination of N-cyclohexyl-2-benzothiazole sulfenamide (accelerator CZ), 2-thiolbenzothiazole (accelerator M), benzothiazole disulfide (accelerator DM) or tetramethylthiuram disulfide (accelerator TMTD).
[0032] Furthermore, the plasticizer includes any one or a combination of liquid nitrile rubber, dioctyl phthalate, tributyl acetyl citrate, di(butoxyethoxyethyl) adipate, mixed ether esters, dioctyl trimellitate, dioctyl terephthalate or diisononyl phthalate.
[0033] The preparation method of the conductive wear-resistant nitrile rubber material of the present invention comprises the following steps:
[0034] Step (1) firstly, modifying graphene and carbon nanotubes respectively by using a coupling agent to obtain modified graphene and modified carbon nanotubes for standby use; then, taking deionized water in a beaker, adding a water-soluble dispersant into the beaker, and stirring with a high-speed disperser, stirring for 5 to 10 minutes, adding modified graphene and modified carbon nanotubes, and continuing to stir for 30 to 60 minutes to obtain a mixed solution of modified graphene and modified carbon nanotubes; taking nitrile latex and slowly adding it to the above mixed solution, continuing to stir with a high-speed disperser for 5 to 10 minutes, and then adding a flocculant for flocculation, collecting the flocculated solid mixture with a filter, washing it with deionized water for 3 to 5 times, and then putting it into an oven for drying to obtain a carbon nanotube graphene nitrile masterbatch for standby use;
[0035] Step (2) setting the initial temperature of the internal mixer to 60-80°C and the rotation speed to 60-80rpm, then putting the nitrile rubber and the carbon nanotube graphene nitrile masterbatch into the internal mixer, first plasticizing for 1-3min, then sequentially putting zinc oxide, stearic acid, antioxidant and dispersant into the internal mixer, continuing to internally mix for 1-3min, then putting high wear-resistant carbon black and plasticizer into the internal mixer, continuing to internally mix for 2-5min, lifting the top bolt of the internal mixer for cleaning, and then continuing to internally mix until the temperature is about 120-150°C to discharge the glue to obtain a film;
[0036] Step (3) adjusting the roller spacing of the open mill to 1.5 mm, adding the rubber sheet obtained in step (2) into the open mill for plasticizing 2 to 3 times, then adding sulfur and vulcanization accelerator, turning the rubber sheet left and right three times each, then adjusting the roller spacing of the open mill to 0.2 mm, performing thin passes 6 to 8 times, discharging the material, and leaving it at room temperature for 12 hours to obtain a rubber mix; finally, vulcanizing and performing performance tests on the rubber mix.
[0037] Further, the coupling agent includes silane coupling agents, such as γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, methacryloxy functional silane, bis-[γ-(triethoxysilyl)propyl]tetrasulfide or bis-[3-(triethoxysilyl)propyl]-disulfide, or a combination of several thereof.
[0038] Furthermore, the modification process of the coupling agent on graphene and carbon nanotubes is as follows: use a high-speed stirrer and an ultrasonic machine to add graphene or carbon nanotubes to water or ethanol for dispersion, then put the mixed solution into a constant temperature water bath at 50 to 80° C. for heating and stirring for 10 to 30 minutes, then slowly add the coupling agent and adjust the pH value to 3 to 5, continue heating and stirring for 30 to 60 minutes, then centrifuge, and put the precipitate into an oven for drying.
[0039] Furthermore, the water-soluble dispersant in step (1) includes any one or a combination of sodium dodecylbenzene sulfonate, polyethylene glycol, acrylic resin or hydroxymethyl cellulose.
[0040] Furthermore, the flocculant includes any one or a combination of calcium chloride, sodium chloride, dilute sulfuric acid, acetic acid or formic acid.
[0041] Furthermore, the drying temperature in step (1) is 50 to 80° C., and the drying time is 24 to 40 hours.
[0042] Embodiment 1: The embodiment of the present disclosure provides a conductive wear-resistant nitrile rubber material, which comprises the following components in parts by weight:
[0043] 160 grams of nitrile rubber, 50 grams of carbon nanotube graphene nitrile masterbatch, 70 grams of high wear-resistant carbon black N234, 10 grams of zinc oxide, 4 grams of stearic acid, 3 grams of antioxidant RD, 3 grams of antioxidant MB, 3 grams of microcrystalline wax, 15 grams of plasticizer DOP, 5 grams of liquid nitrile rubber, 3 grams of accelerator DM, 1 gram of accelerator CZ, and 3 grams of sulfur.
[0044] A method for preparing a conductive wear-resistant nitrile rubber material comprises the following steps:
[0045] (1) Take 2000 ml of ethanol in a beaker, and disperse 10 grams of carbon nanotubes in the ethanol under the action of a high-speed stirrer and an ultrasonic machine; then put the beaker into a constant temperature water bath at 60°C for heating and stirring for 30 minutes, then slowly add 1.5 grams of silane coupling agent Si-69 to the beaker, and adjust the pH value of the solution to 3.5 with acetic acid, continue the reaction for 60 minutes, then centrifuge, and put the precipitate into an oven at a temperature of 120°C for 48 hours to obtain modified carbon nanotube powder.
[0046] The modification of graphene is the same as the above step (1), which will not be repeated here. The amount of graphene used is 10 grams.
[0047] (2) Take 3000 ml of deionized water in a beaker, add 6 g of sodium dodecylbenzene sulfonate to the beaker and stir for 10 min under the stirring action of a high-speed stirrer, wherein the stirring speed of the high-speed stirrer is 2000 r / min; take the modified carbon nanotubes and modified graphene obtained in step (1), slowly add them to the above solution, adjust the speed of the high-speed stirrer to 1000 r / min, and continue stirring for 40 min for standby use.
[0048] Weigh 400 g of 20% nitrile latex in a beaker, stir it with a high-speed stirrer at a speed of 4000 r / min, then slowly add the mixed aqueous solution of carbon nanotubes and graphene prepared above into the beaker, and continue stirring for 30 minutes; then continue to add 500 g of 5% calcium chloride aqueous solution into the beaker, stir for 5 minutes, filter the condensed solid mixture with a 60-mesh filter, rinse it with deionized water 3 times, and put it in an oven at a temperature of 80°C to dry for 24 hours to obtain the carbon nanotube graphene nitrile masterbatch for use.
[0049] (3) The initial temperature of the internal mixer was set to 65°C and the speed was 65 rpm. Then, the nitrile rubber and carbon nanotube graphene nitrile masterbatch were put into the internal mixer and plasticized for 1.5 min. Then, zinc oxide, stearic acid, antioxidant RD and antioxidant MB, and microcrystalline wax were added in sequence and mixed for 1 min. Then, high wear-resistant carbon black N234, plasticizer DOP and liquid nitrile rubber were added and mixed for another 2 min. The top bolt on the internal mixer was lifted to clean it, and then mixed to about 140°C to discharge the glue to obtain a film.
[0050] Adjust the roller distance of the mixing mill to 1.5mm, add the rubber sheet from the internal mixer into the mixing mill for plasticizing 3 times, wrap the roller, then add sulfur and accelerator CZ, turn the rubber left and right three times each, then adjust the roller distance of the mixing mill to 0.2mm and perform thin pass 6 times, produce sheets according to the required thickness and size, stop for 12 hours, and obtain the mixed rubber; finally, vulcanize and perform performance tests on the mixed rubber.
[0051] Among them, the vulcanization temperature is 170°C, the vulcanization pressure is 10MPa, and the vulcanization time is Tc90+2min.
[0052] Embodiment 2: The embodiment of the present disclosure provides a conductive wear-resistant nitrile rubber material, which comprises the following components in parts by weight:
[0053] 160 grams of nitrile rubber, 50 grams of carbon nanotube graphene nitrile masterbatch, 70 grams of high wear-resistant carbon black N234, 10 grams of zinc oxide, 4 grams of stearic acid, 3 grams of antioxidant RD, 3 grams of antioxidant MB, 3 grams of microcrystalline wax, 15 grams of plasticizer DOP, 5 grams of liquid nitrile rubber, 3 grams of accelerator DM, 1 gram of accelerator CZ, and 3 grams of sulfur.
[0054] A method for preparing a conductive wear-resistant nitrile rubber material comprises the following steps:
[0055] (1) Take 2000 ml of ethanol in a beaker, and disperse 5 grams of carbon nanotubes in the ethanol under the action of a high-speed stirrer and an ultrasonic machine; then put the beaker into a constant temperature water bath at 60°C for heating and stirring for 30 minutes, then slowly add 1.5 grams of silane coupling agent Si-69 to the beaker, and adjust the pH value of the solution to 3.5 with acetic acid, continue the reaction for 60 minutes, then centrifuge, and put the precipitate into an oven at a temperature of 120°C for 48 hours to obtain modified carbon nanotube powder.
[0056] The modification process of graphene is the same as the above step (1), wherein the amount of graphene used is 15 grams.
[0057] (2) Take 3000 ml of deionized water in a beaker, add 6 g of sodium dodecylbenzene sulfonate to the beaker and stir for 10 min under the stirring action of a high-speed stirrer, wherein the stirring speed of the high-speed stirrer is 2000 r / min; take the modified carbon nanotubes and modified graphene obtained in step (1), slowly add them to the above solution, adjust the speed of the high-speed stirrer to 1000 r / min, and continue stirring for 40 min for standby use.
[0058] Weigh 400 g of 20% nitrile latex in a beaker, stir it with a high-speed stirrer at a speed of 4000 r / min, then slowly add the mixed aqueous solution of carbon nanotubes and graphene prepared above into the beaker, and continue stirring for 30 minutes; then continue to add 500 g of 5% calcium chloride aqueous solution into the beaker, stir for 5 minutes, filter the condensed solid mixture with a 60-mesh filter, rinse it with deionized water 3 times, and put it in an oven at a temperature of 80°C to dry for 24 hours to obtain the carbon nanotube graphene nitrile masterbatch for use.
[0059] (3) The initial temperature of the internal mixer was set to 65°C and the speed was 65 rpm. Then, the nitrile rubber and carbon nanotube graphene nitrile masterbatch were put into the internal mixer for plasticization for 1.5 min. Then, zinc oxide, stearic acid, antioxidant RD and antioxidant MB, and microcrystalline wax were added in sequence. After mixing for 1 min, high wear-resistant carbon black N234, plasticizer DOP and liquid nitrile rubber were added. After mixing for another 2 min, the top bolt on the internal mixer was lifted for cleaning. Then, the internal mixer was mixed to about 140°C to discharge the glue and obtain a film.
[0060] Adjust the roller distance of the mixing mill to 1.5mm, add the rubber sheet from the internal mixer into the mixing mill for plasticizing 3 times, wrap the roller, then add sulfur and accelerator CZ, turn the rubber left and right three times each, then adjust the roller distance of the mixing mill to 0.2mm and perform thin pass 6 times, produce sheets according to the required thickness and size, stop for 12 hours, and obtain the mixed rubber; finally, vulcanize and perform performance tests on the mixed rubber.
[0061] Among them, the vulcanization temperature is 170°C, the vulcanization pressure is 10MPa, and the vulcanization time is Tc90+2min.
[0062] Embodiment 3: The embodiment of the present disclosure provides a conductive wear-resistant nitrile rubber material, which comprises the following components in parts by weight:
[0063] 160 grams of nitrile rubber, 50 grams of carbon nanotube graphene nitrile masterbatch, 70 grams of high wear-resistant carbon black N330, 10 grams of zinc oxide, 4 grams of stearic acid, 3 grams of antioxidant RD, 3 grams of antioxidant MB, 3 grams of microcrystalline wax, 20 grams of plasticizer DOP, 3 grams of accelerator DM, 1 gram of accelerator CZ, and 3 grams of sulfur.
[0064] A method for preparing a conductive wear-resistant nitrile rubber material comprises the following steps:
[0065] (1) Take 2000 ml of ethanol in a beaker, and disperse 15 g of carbon nanotubes in the ethanol under the action of a high-speed stirrer and an ultrasonic machine, wherein the stirring speed of the high-speed stirrer is 1000 r / min and the time is 30 min; then put the beaker into a constant temperature water bath at 80°C for heating and stirring for 30 min, then slowly add 1 g of silane coupling agent KH550 to the beaker, and adjust the pH value of the solution to 5 with acetic acid, continue the reaction for 40 min, then centrifuge, and put the precipitate into an oven at a temperature of 120°C for drying for 72 h to obtain modified carbon nanotube powder.
[0066] The modification process of graphene is the same as the above step (1), wherein the amount of graphene used is 5 grams.
[0067] (2) Take 3000 ml of deionized water in a beaker, add 4 g of sodium dodecylbenzene sulfonate and 4 g of polyvinyl alcohol into the beaker and stir for 20 min under the stirring action of a high-speed stirrer, wherein the stirring speed of the high-speed stirrer is 2500 r / min; take the modified carbon nanotubes and modified graphene obtained in step (1), slowly add them to the above solution, adjust the speed of the high-speed stirrer to 1000 r / min, and continue stirring for 60 min for standby use.
[0068] Weigh 400 g of 20% nitrile latex in a beaker, stir it with a high-speed stirrer at a speed of 5000 r / min, then slowly add the mixed aqueous solution of carbon nanotubes and graphene prepared above into the beaker, and continue stirring for 30 minutes; then continue to add 500 g of 5% dilute sulfuric acid into the beaker, stir for 10 minutes, filter the condensed solid mixture with a 60-mesh filter, rinse it with deionized water 3 times, and put it in an oven at 80°C to dry for 24 hours to obtain the carbon nanotube graphene nitrile masterbatch for use.
[0069] (3) The initial temperature of the internal mixer was set to 65°C and the speed was 65 rpm. Then, the nitrile rubber and carbon nanotube graphene nitrile masterbatch were put into the internal mixer for plasticization for 1.5 min. Then, zinc oxide, stearic acid, antioxidant RD and antioxidant MB, and microcrystalline wax were added in sequence. After mixing for 1 min, high wear-resistant carbon black N330 and plasticizer DOP were added. The internal mixer was mixed for another 2 min. The top bolt on the internal mixer was lifted for cleaning. The internal mixer was mixed to about 140°C to discharge the glue and obtain a film.
[0070] Adjust the roller distance of the mixing mill to 1.5mm, add the rubber sheet from the internal mixer into the mixing mill for plasticizing 3 times, wrap the roller, then add sulfur and accelerator CZ, turn the rubber left and right three times each, then adjust the roller distance of the mixing mill to 0.2mm and perform thin pass 6 times, produce sheets according to the required thickness and size, stop for 12 hours, and obtain the mixed rubber; finally, vulcanize and perform performance tests on the mixed rubber.
[0071] Among them, the vulcanization temperature is 170°C, the vulcanization pressure is 10MPa, and the vulcanization time is Tc90+2min.
[0072] Comparative Example 1: The conductive wear-resistant nitrile rubber material includes the following components in parts by weight:
[0073] 200 grams of nitrile rubber, 10 grams of carbon nanotubes, 10 grams of graphene, 70 grams of high wear-resistant carbon black N234, 10 grams of zinc oxide, 4 grams of stearic acid, 3 grams of antioxidant RD, 3 grams of antioxidant MB, 3 grams of microcrystalline wax, 15 grams of plasticizer DOP, 5 grams of liquid nitrile rubber, 3 grams of accelerator DM, 1 gram of accelerator CZ, and 3 grams of sulfur.
[0074] The preparation method of the conductive wear-resistant nitrile rubber material comprises the following steps:
[0075] The initial temperature of the internal mixer was set to 65°C and the speed was 65rpm. The nitrile rubber was then put into the internal mixer and plasticized for 1.5min. Zinc oxide, stearic acid, antioxidant RD and antioxidant MB, and microcrystalline wax were added in sequence and mixed for 1min. Graphene and carbon nanotubes were then added and mixed for 2min. Highly wear-resistant carbon black N234, plasticizer DOP and liquid nitrile rubber were then added and mixed for another 2min. The top bolt on the internal mixer was lifted for cleaning, and then mixed to about 140°C for debonding to obtain a film.
[0076] Adjust the roller distance of the mixing mill to 1.5mm, add the rubber sheet from the internal mixer into the mixing mill for plasticizing 3 times, wrap the roller, then add sulfur and accelerator CZ, turn the rubber left and right three times each, then adjust the roller distance of the mixing mill to 0.2mm and perform thin pass 6 times, produce sheets according to the required thickness and size, stop for 12 hours, and obtain the mixed rubber; finally, vulcanize and perform performance tests on the mixed rubber.
[0077] Among them, the vulcanization temperature is 170°C, the vulcanization pressure is 10MPa, and the vulcanization time is Tc90+2min.
[0078] Comparative Example 2: Commercially available conductive and wear-resistant nitrile rubber material.
[0079] The nitrile rubber materials obtained in Example 1, Example 2, and Example 3, Comparative Example 1, and commercially available conductive wear-resistant nitrile rubber materials were subjected to performance testing experiments, including tensile strength, tear strength, hardness, DIN volume abrasion, and volume resistivity. The test results are shown in Table 1.
[0080] Among them, the tensile strength is tested according to GB / T529-2009 standard, the tear strength is tested according to GB / T529-2008 standard, the Shore hardness is tested according to GB / T 531.1-2008 / ISO 7619-1:2004 standard, the DIN volume abrasion is tested according to GB / 9867-88 standard, and the volume resistivity is tested according to GB / T 2439-2001 standard.
[0081] Table 1 Test results of mechanical properties and electrical conductivity of different nitrile rubber materials
[0082]
[0083] It can be seen from Table 1 that the tensile strength of the conductive wear-resistant nitrile rubber material prepared by the present invention is not less than 23.5MPa, and the tear strength is 65-69KN / m. It can be seen that the mechanical properties of the conductive wear-resistant nitrile rubber of the present invention are greatly improved, and the Shore A hardness is equivalent to that of Comparative Example 1 and Comparative Example 2; the DIN volume wear of the conductive wear-resistant nitrile rubber material prepared by the present invention is 0.021-0.03cm 3 , while the DIN volume wear of comparative example 1 is 0.2 cm 3 The DIN volume wear of commercially available conductive wear-resistant nitrile rubber materials is 0.17 cm 3 It can be seen that the wear resistance of the conductive wear-resistant nitrile rubber material prepared by the present invention is significantly enhanced; the volume resistivity of the conductive wear-resistant nitrile rubber material prepared by the present invention is between 0.48 and 0.55Ω·cm, while the volume resistivity of comparative example 1 is 10Ω·cm, and the volume resistivity of the commercially available conductive wear-resistant nitrile rubber material is 2.9Ω·cm. It can be seen that the conductive performance of the conductive wear-resistant nitrile rubber material prepared by the present invention has obvious advantages.
[0084] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention scientifically matches nitrile rubber and carbon nanotube graphene nitrile masterbatch, and greatly improves the conductive properties of nitrile rubber materials under the action of high wear-resistant carbon black, zinc oxide, stearic acid, antioxidant, dispersant, plasticizer, vulcanization accelerator and sulfur; the nitrile rubber material also greatly improves wear resistance and mechanical properties. The preparation method mainly adopts two steps, firstly, the carbon nanotube graphene nitrile masterbatch is prepared by adopting a liquid phase wet mixing process, the dispersion of carbon nanotubes and graphene in rubber is improved, the carbon nanotubes, graphene and rubber molecular chains are fully combined, and the conductive network is improved; then, the nitrile rubber, carbon nanotube graphene nitrile masterbatch and various processing aids are evenly mixed by internal mixing and open mixing; the process is simple, the operation is convenient, and it is easy to realize industrialization.
[0085] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A conductive wear-resistant nitrile rubber material, characterized in that: The composition comprises the following components in parts by weight: 70-80 parts of nitrile rubber, 20-30 parts of carbon nanotube graphene nitrile masterbatch, 30-45 parts of high wear-resistant carbon black, 5-8 parts of zinc oxide, 2-5 parts of stearic acid, 3-5 parts of antioxidant, 2-5 parts of dispersant, 5-20 parts of plasticizer, 1-3 parts of vulcanization accelerator, and 1-3 parts of sulfur.
2. The conductive wear-resistant nitrile rubber material according to claim 1, characterized in that: The carbon nanotube content in the carbon nanotube-graphene-butadiene-nitrile masterbatch is 5% to 15%, and the graphene content is 5% to 15%.
3. The conductive wear-resistant nitrile rubber material according to claim 1, characterized in that: The antioxidant includes any one or a combination of N-cyclohexyl-N'-phenyl-p-phenylenediamine (antioxidant 4010), N-phenyl-N'-isopropyl-p-phenylenediamine (antioxidant 4010NA), N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (antioxidant 4020), 2,2,4-trimethyl-1,2-dihydroquinoline polymer (antioxidant RD) or 2-thiol benzimidazole (antioxidant MB).
4. The conductive wear-resistant nitrile rubber material according to claim 1, characterized in that: The dispersant includes any one of microcrystalline wax and paraffin wax or a combination of the two.
5. The conductive wear-resistant nitrile rubber material according to claim 1, characterized in that: The vulcanization accelerator includes any one or a combination of N-cyclohexyl-2-benzothiazole sulfenamide (accelerator CZ), 2-thiolbenzothiazole (accelerator M), benzothiazole disulfide (accelerator DM) or tetramethylthiuram disulfide (accelerator TMTD).
6. The conductive wear-resistant nitrile rubber material according to claim 1, characterized in that: The plasticizer includes any one or a combination of liquid nitrile rubber, dioctyl phthalate, tributyl acetyl citrate, di(butoxyethoxyethyl) adipate, mixed ether ester, dioctyl trimellitate, dioctyl terephthalate or diisononyl phthalate.
7. A method for preparing the conductive wear-resistant nitrile rubber material according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step (1) firstly uses a coupling agent to modify graphene and carbon nanotubes respectively, and set them aside; then takes deionized water in a beaker, adds a water-soluble dispersant into the beaker, stirs, then adds the modified graphene and carbon nanotubes, continues to stir, and obtains a mixed solution of graphene and carbon nanotubes; takes nitrile latex and slowly adds it to the mixed solution of graphene and carbon nanotubes, stirs, then adds a flocculant to flocculate, collects the flocculated solid mixture with a filter, washes it with deionized water for 3 to 5 times, and then puts it into an oven for drying, and obtains a carbon nanotube graphene nitrile masterbatch for standby use; Step (2) setting the initial temperature of the internal mixer to 60-80°C and the rotation speed to 60-80rpm, then putting the nitrile rubber and the carbon nanotube graphene nitrile masterbatch into the internal mixer, first plasticizing for 1-3min, then sequentially putting zinc oxide, stearic acid, antioxidant and dispersant into the internal mixer, continuing to internally mix for 1-3min, then putting high wear-resistant carbon black and plasticizer into the internal mixer, continuing to internally mix for 2-5min, lifting the top bolt of the internal mixer for cleaning, and then continuing to internally mix until the temperature is about 120-150°C to discharge the glue to obtain a film; Step (3) adjusting the roller spacing of the open mill to 1.5 mm, adding the rubber sheet obtained in step (2) into the open mill for plasticizing 2 to 3 times, then adding sulfur and vulcanization accelerator, turning the rubber sheet left and right three times each, then adjusting the roller spacing of the open mill to 0.2 mm, performing thin passes 6 to 8 times, discharging the material, and leaving it at room temperature for 12 hours to obtain a rubber mix; finally, vulcanizing and performing performance tests on the rubber mix.
8. The method for preparing the conductive wear-resistant nitrile rubber material according to claim 7, characterized in that: The water-soluble dispersant in step (1) includes any one or a combination of sodium dodecylbenzene sulfonate, polyethylene glycol, acrylic resin or hydroxymethyl cellulose.
9. The method for preparing the conductive wear-resistant nitrile rubber material according to claim 7, characterized in that: The flocculant includes any one or a combination of calcium chloride, sodium chloride, dilute sulfuric acid, acetic acid or formic acid.
10. The method for preparing the conductive wear-resistant nitrile rubber material according to claim 7, characterized in that: The drying temperature in step (1) is 50-80° C. and the drying time is 24-40 hours.
Citation Information
Cited By
Preparation method and application of nitrile rubber belt
CN119264495A
Preparation method and application of nitrile rubber belt
CN119264495B
Conductive rubber oil seal for hub bearing
CN121761033A
Electrically conductive rubber oil seal for wheel bearing
CN121761033B
Rubber roller and preparation method thereof
CN121895650A