Water-erosion-resistant compressor impeller
By using a combined structure of a high-entropy alloy layer and a superhydrophobic layer on the impeller, the service life of the MVR steam compressor impeller in a water erosion environment is solved, high hardness and wear resistance are achieved, the service life of the impeller is extended and the service life of the impeller is reduced. Water erosion risk.
Patent Information
- Application Number
- CN202411136422.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-19
AI Technical Summary
In MVR steam compressors, impeller materials are susceptible to damage caused by water droplets or water flow, resulting in reduced service life and potential unit accidents. Existing protection methods such as brazing Sitaili alloy sheets have stress corrosion problems, and coating bonding force Insufficient, easy to peel off.
Using a combined structure of a high-entropy alloy layer and a super-hydrophobic layer, the high-entropy alloy layer is prepared by laser cladding. The super-hydrophobic layer is composed of fluorosilicone resin, modified alumina crosslinker and modified hyperbranched polyester, with high hardness. , wear resistance and corrosion resistance, superhydrophobic layers reduce moisture erosion through low surface energy and high water contact angle.
It significantly improves the water corrosion resistance of the impeller, extends the service life, enhances the hardness and wear resistance of the impeller, reduces moisture corrosion, and avoids stress concentration and crack formation.
Smart Images

Figure BDA0004999556300000091 
Figure BDA0004999556300000101
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of impeller materials, and in particular to an anti-water erosion compressor impeller. Background Art
[0002] During the operation of the MVR steam compressor, the steam compressor blades work in wet steam containing water droplets. Under the combined effects of centrifugal force, steam force, excitation force and the scouring of water droplets carried by steam, the blades are easily damaged by water droplets or continuous water flow at high speeds, which seriously affects their service life. The existence of the above problems not only greatly reduces the variable efficiency of the steam compressor during operation, but also easily causes stress concentration in the scouring area. If it is operated for a long time without protection, the blades will form cracks and eventually break, further causing serious accidents of unit damage.
[0003] At present, the most common method to prevent impeller erosion is to braze the Stellite sheet on the back arc side of the blade. However, there is an unbonded area in the brazing area, and stress corrosion will occur at the joint, resulting in transverse cracks along the gaps of the Stellite sheet on the blade. In addition, the alloy sheet may fall off during high-speed operation, causing destructive effects on the unit. Preparing an anti-erosion coating on the impeller material through surface processing is an effective protection method. The surface of the coating is smooth and dense, which can protect the impeller, but the existing coating is prone to peeling and has weak bonding with the substrate, so it needs to be improved. Summary of the invention
[0004] In order to improve the anti-water erosion performance of a compressor impeller, the present application provides an anti-water erosion compressor impeller.
[0005] The present application provides an anti-water erosion compressor impeller adopts the following technical solution: An anti-water erosion compressor impeller comprises an impeller substrate, a high entropy alloy layer and a super hydrophobic layer, wherein the super hydrophobic layer is obtained by coating a super hydrophobic coating on the surface of the high entropy alloy layer, and the raw materials for preparing the super hydrophobic coating include the following components in parts by weight: 10-20 parts of fluorosilicone resin Modified alumina crosslinking agent 5-10 parts 40-60 parts of modified hyperbranched polyester 1-2 parts of triphenyl phosphite Titanium catalyst 0.4-0.6 parts 40-50 parts of solvent.
[0006] The impeller is protected by a high entropy alloy layer and a super hydrophobic layer. The high entropy alloy layer has high strength, high hardness, good wear resistance and corrosion resistance, can promote the formation of solid solution, and improve the ductility of the material; the super hydrophobic layer has low surface energy and a high water contact angle, and the fluorosilicone resin reduces the surface energy by introducing fluorine and silicon elements, thereby improving the hydrophobicity and stability; the modified alumina cross-linking agent introduces alumina into the coating to improve the wear resistance of the coating, the modified hyperbranched polyester has a high degree of branching and good reactivity, and the super hydrophobic coating prepared by reacting with the fluorosilicone resin and the modified alumina cross-linking agent has good hydrophobicity and stability, and improves the hardness, wear resistance and corrosion resistance of the super hydrophobic layer. Water droplets will quickly roll off the surface of the super hydrophobic layer, reducing the erosion of water on the impeller, compensating and repairing the impeller, and extending the service life of the impeller.
[0007] Preferably, the raw materials for preparing the fluorosilicone resin include hexadecyltrimethoxysilane, diphenyldimethoxysilane and heptadecafluorodecyltrimethoxysilane.
[0008] The fluorosilicone resin is obtained by the condensation of hexadecyltrimethoxysilane, diphenyldimethoxysilane and heptadecafluorodecyltrimethoxysilane. The fluorine-containing silane introduces fluorine element into the resin, thereby improving the stability of the resin, reducing the surface energy, and improving the weather resistance and anti-aging properties of the fluorosilicone resin. The fluorosilicone resin has good wettability and can adhere well to the substrate, so that the super-hydrophobic layer can better exert its anti-water erosion performance.
[0009] Preferably, the mass ratio of hexadecyltrimethoxysilane, diphenyldimethoxysilane and heptadecafluorodecyltrimethoxysilane is 1:0.5:(0.1-0.2).
[0010] The fluorosilicone resin prepared according to the above mass ratio has low surface energy, good stability and weather resistance.
[0011] Preferably, the raw materials for preparing the modified alumina crosslinking agent include nano-alumina, dimethoxymethylchlorosilane and decanediamine.
[0012] Nano-alumina is modified by dimethoxymethylchlorosilane and decanediamine to improve its reactivity and increase its surface active groups, so that the nano-alumina is evenly dispersed in the side chains of the modified hyperbranched polyester; nano-alumina itself has high hardness and can form a hard particle structure on the coating surface to improve wear resistance. At the same time, it can reinforce the polyester molecules and improve their stability, thereby significantly improving the anti-water erosion performance of the super-hydrophobic layer.
[0013] Preferably, the modified hyperbranched polyester comprises an aliphatic cyclohexyl modifier, trimethylolpropane, neopentyl glycol and 2-hydroxypropionic acid.
[0014] Preferably, the raw materials for preparing the aliphatic cyclohexyl modifier include suberic acid and cyclohexene oxide.
[0015] Aliphatic cyclohexyl modifiers have both aliphatic chain segments and cyclohexyl groups, which can effectively improve the stability of polyester; cyclohexyl groups have good structural stability and rigidity, which can improve the hardness and wear resistance of polyester and reduce the impact of water erosion on the super-hydrophobic layer; aliphatic chain segments can increase the flexibility and ductility of polyester and reduce the damage to the coating caused by external forces, thereby improving the water erosion resistance of the impeller.
[0016] Preferably, the high entropy alloy layer is obtained by laser cladding of high entropy alloy powder, and the high entropy alloy powder includes the following components in mass fractions: molybdenum 21.33-22.75%, nickel 14.1-15.04%, cobalt 14.04-14.98%, iron 13.22-14.1%, chromium 12.31-13.13%, and the remainder is a reinforcing phase.
[0017] The mixed powder prepared by five elements of molybdenum, nickel, cobalt, iron and chromium has high mixing entropy, which can reduce the free energy of the solid solution phase, promote the formation of solid solution, and improve the strength and ductility of the high entropy alloy layer; the reinforcing phase can make up for the shortcomings of the high entropy alloy, improve the comprehensive performance of the high entropy alloy, and make the high entropy alloy layer have both high hardness and good corrosion resistance.
[0018] Preferably, the reinforcement phase includes silicon carbide, titanium nitride and cerium dioxide.
[0019] Silicon carbide and titanium nitride are intermetallic compounds with high strength and hardness. The two work synergistically as reinforcing phases to effectively improve the hardness and wear resistance of high-entropy alloys. They can also enhance the crystal structure of high-entropy alloys at the microscopic level, improve their strength and toughness, and reduce the damage caused by water impact during high-speed operation; cerium dioxide has good corrosion resistance and high-temperature oxidation resistance, and can improve the stability of high-entropy alloys; cerium dioxide can also inhibit grain growth, form a fine dispersed phase, regulate the microstructure, and enhance its ability to resist external forces, while reducing the friction coefficient of the high-entropy alloy surface and improving the water erosion resistance of the high-entropy alloy layer.
[0020] Preferably, the mass ratio of silicon carbide, titanium nitride and cerium dioxide is 1:1.55:(0.86-1.29).
[0021] The high entropy alloy layer prepared according to the above mass ratio has high hardness and good water erosion resistance.
[0022] Preferably, the anti-water erosion compressor impeller is prepared by the following steps: The impeller matrix is polished with sandpaper and an angle grinder, and the polished impeller matrix is cleaned with anhydrous ethanol to obtain a pretreated impeller matrix; the metal powder and the reinforcing phase are mixed and dispersed according to the ratio and ball-milled in a planetary ball mill to obtain a high-entropy alloy powder, and the high-entropy alloy powder is laser clad using coaxial powder feeding to obtain a high-entropy alloy layer; a super-hydrophobic coating is coated on the surface of the high-entropy alloy layer, and an anti-water erosion compressor impeller is obtained after drying.
[0023] The compressor impeller prepared according to the above steps has high hardness and good water erosion resistance.
[0024] In summary, the present application includes at least one of the following beneficial technical effects: 1. The impeller is protected by a high entropy alloy layer and a super hydrophobic layer. The high entropy alloy layer has high strength, high hardness, good wear resistance and corrosion resistance, can promote the formation of solid solution, and improve the ductility of the material; the super hydrophobic layer has low surface energy and a high water contact angle. Fluorosilicone resin reduces surface energy by introducing fluorine and silicon elements, and improves hydrophobicity and stability; the modified alumina cross-linking agent introduces alumina into the coating to improve the wear resistance of the coating. The modified hyperbranched polyester has a high degree of branching and good reactivity. The super hydrophobic coating prepared by reacting with fluorosilicone resin and modified alumina cross-linking agent has good hydrophobicity and stability, and improves the hardness, wear resistance and corrosion resistance of the super hydrophobic layer. Water droplets will quickly roll off the surface of the super hydrophobic layer, reducing the erosion of water on the impeller, compensating and repairing the impeller, and extending the service life of the impeller.
[0025] 2. Fluorosilicone resin obtained by condensation of hexadecyltrimethoxysilane, diphenyldimethoxysilane and heptadecafluorodecyltrimethoxysilane. Fluorosilane introduces fluorine element into the resin, improves the stability of the resin, reduces the surface energy, and improves the weather resistance and anti-aging properties of the fluorosilicone resin. The fluorosilicone resin has good wettability and can adhere well to the substrate, so that the superhydrophobic layer can better exert its anti-water erosion performance.
[0026] 3. Silicon carbide and titanium nitride are intermetallic compounds with high strength and hardness. The two work synergistically as reinforcing phases to effectively improve the hardness and wear resistance of high-entropy alloys. They can also enhance the crystal structure of high-entropy alloys at the microscopic level, improve their strength and toughness, and reduce the damage caused by water impact during high-speed operation; Cerium dioxide has good corrosion resistance and high-temperature oxidation resistance, and can improve the stability of high-entropy alloys; Cerium dioxide can also inhibit grain growth, form a fine dispersed phase, regulate the microstructure, and enhance its ability to resist external forces. At the same time, it reduces the friction coefficient of the high-entropy alloy surface and improves the water erosion resistance of the high-entropy alloy layer. DETAILED DESCRIPTION
[0027] The present application discloses an anti-water erosion compressor impeller. The raw materials used in the present application can be obtained from commercially available raw materials unless otherwise specified. The present application is further described in detail below in conjunction with the embodiments: Raw materials description: hexadecyltrimethoxysilane (CAS No.: 16415-12-6), diphenyldimethoxysilane (CAS No.: 6843-66-9), heptadecafluorodecyltrimethoxysilane (CAS No.: 83048-65-1), suberic acid (CAS No.: 505-48-6), cyclohexene oxide (CAS No.: 286-20-4), catalyst is organic bismuth catalyst (CAS No.: 67874-71-9), neopentyl glycol (CAS No.: 126-30-7), 2-hydroxypropionic acid (CAS No.: 849585-22-4), trimethylol Propane (CAS No.: 77-99-6), triphenyl phosphite (CAS No.: 101-02-0), and nano-alumina were purchased from Hubei Huifu Nanomaterials Co., Ltd., dimethoxymethylchlorosilane (CAS No.: 994-07-0), decanediamine (CAS No.: 646-25-3), the titanium catalyst was tetrabutyl titanate (CAS No.: 5593-70-4), the solvent was propylene glycol methyl ether acetate (CAS No.: 108-65-6), methyltriethoxysilane (CAS No.: 2031-67-6), and silitai alloy was purchased from Suzhou Kentailier Welding Technology Co., Ltd.
[0028] Example 1 Preparation of fluorosilicone resin: 18.75 kg of hexadecyltrimethoxysilane, 9.375 kg of diphenyldimethoxysilane and 1.875 kg of heptadecafluorodecyltrimethoxysilane were mixed and dispersed in 40 L of anhydrous ethanol to obtain a silane dispersion. 15 L of deionized water was added to the silane dispersion under stirring at 200 rpm and a 50°C water bath. The addition was completed within 30 min. After reacting for 3 h, the temperature was raised to 130°C and the reaction was continued for 30 min to obtain a product solution. The product solution was rotary evaporated to remove the solvent to obtain a fluorosilicone resin.
[0029] Preparation of aliphatic cyclohexyl modifier 12.79 kg of suberic acid, 7.21 kg of cyclohexene oxide and 0.08 kg of catalyst were mixed and dispersed, heated to 70° C. under nitrogen protection, stirred and refluxed at a speed of 200 rpm for 2 hours, and cooled to below 30° C. to obtain an aliphatic cyclohexyl modifier.
[0030] Preparation of modified hyperbranched polyester 47.48 kg of neopentyl glycol, 38.93 kg of 2-hydroxypropionic acid and 13.59 kg of trimethylolpropane were heated to melt to obtain a molten mixture, and stirring was started at a rate of 200 rpm. After keeping warm for 1 hour, 2 kg of triphenyl phosphite was added, and the temperature was raised to 240 ° C at a rate of 12 ° C / h for reaction for 2 hours, and the water was evaporated. The temperature was kept for 1 hour, and then the temperature was lowered to 180 ° C, 20 L of xylene and 15 kg of aliphatic cyclohexyl modifier were added, and the temperature was raised to 220 ° C again for reaction for 2 hours, and then reduced pressure distillation was performed, and the temperature was lowered to below 30 ° C to obtain a hyperbranched polyester.
[0031] Preparation of modified alumina crosslinking agent 15.3 kg of nano-alumina and 2.11 kg of dimethoxymethylsilyl chloride were dispersed in 200 mL of toluene, stirred at 200 rpm for 2 h, then 0.5 L of deionized water was added, and the mixture was stirred at 200 rpm for 4 h in a water bath at 80 ° C., 2.59 kg of decanediamine was added, and the mixture was stirred at 200 rpm for 4 h in a water bath at 80 ° C., the product solution was filtered, the solid was washed with anhydrous ethanol, and the washed solid was dried in an oven at 80 ° C. for 6 h. The dried solid was ground to obtain a modified alumina cross-linking agent.
[0032] Preparation of superhydrophobic coatings 10 kg of fluorosilicone resin, 5 kg of modified alumina crosslinking agent, 40 kg of modified hyperbranched polyester, 1 kg of triphenyl phosphite and 0.4 kg of titanium catalyst were mixed and dispersed in 40 L of solvent, heated to 160 ° C for reaction until no water was evaporated, cooled to below 30 ° C and discharged to obtain a super hydrophobic coating.
[0033] Preparation of water erosion resistant compressor impeller The impeller substrate was polished with sandpaper and an angle grinder, and the polished impeller substrate was cleaned with anhydrous ethanol to obtain a pretreated impeller substrate. 21.33kg of molybdenum, 14.1kg of nickel, 14.04kg of cobalt, 13.22kg of iron, 12.31kg of chromium and 25kg of reinforcing phase were mixed and dispersed in a planetary ball mill and ball-milled at 300rpm for three hours. The mass ratio of silicon carbide, titanium nitride and cerium dioxide in the reinforcing phase was 1:1.55:0.86 to obtain a high entropy alloy powder. The high entropy alloy powder was laser clad using coaxial powder feeding, with a scanning speed of 10mm / s, a laser spot diameter of 3mm, a powder feeding speed of 1.2r / min, a laser power of 1200w, and an argon flow rate of 15L / min to obtain a high entropy alloy layer. The superhydrophobic coating was applied to the surface of the high entropy alloy layer and vacuum dried in an oven at 180℃ for 4h to obtain an anti-water erosion compressor impeller.
[0034] Example 2 Preparation of fluorosilicone resin: 17.65 kg of hexadecyltrimethoxysilane, 8.82 kg of diphenyldimethoxysilane and 3.53 kg of heptadecafluorodecyltrimethoxysilane were mixed and dispersed in 40 L of anhydrous ethanol to obtain a silane dispersion. 15 L of deionized water was added to the silane dispersion under stirring at 200 rpm and a 50°C water bath. The addition was completed within 30 min. After reacting for 3 h, the temperature was raised to 130°C and the reaction was continued for 30 min to obtain a product solution. The product solution was rotary evaporated to remove the solvent to obtain a fluorosilicone resin.
[0035] Preparation of aliphatic cyclohexyl modifier 12.79 kg of suberic acid, 7.21 kg of cyclohexene oxide and 0.08 kg of catalyst were mixed and dispersed, heated to 70° C. under nitrogen protection, stirred and refluxed at a speed of 200 rpm for 2 hours, and cooled to below 30° C. to obtain an aliphatic cyclohexyl modifier.
[0036] Preparation of modified hyperbranched polyester 47.48 kg of neopentyl glycol, 38.93 kg of 2-hydroxypropionic acid and 13.59 kg of trimethylolpropane were heated to melt to obtain a molten mixture, and stirring was started at a rate of 200 rpm. After keeping warm for 1 hour, 2 kg of triphenyl phosphite was added, and the temperature was raised to 240 ° C at a rate of 12 ° C / h for reaction for 2 hours, and the water was evaporated. The temperature was kept for 1 hour, and then the temperature was lowered to 180 ° C, 20 L of xylene and 15 kg of aliphatic cyclohexyl modifier were added, and the temperature was raised to 220 ° C again for reaction for 2 hours, and then reduced pressure distillation was performed, and the temperature was lowered to below 30 ° C to obtain a hyperbranched polyester.
[0037] Preparation of modified alumina crosslinking agent 15.3 kg of nano-alumina and 2.11 kg of dimethoxymethylsilyl chloride were dispersed in 200 mL of toluene, stirred at 200 rpm for 2 h, then 0.5 L of deionized water was added, and the mixture was stirred at 200 rpm for 4 h in a water bath at 80 ° C., 2.59 kg of decanediamine was added, and the mixture was stirred at 200 rpm for 4 h in a water bath at 80 ° C., the product solution was filtered, the solid was washed with anhydrous ethanol, and the washed solid was dried in an oven at 80 ° C. for 6 h. The dried solid was ground to obtain a modified alumina cross-linking agent.
[0038] Preparation of superhydrophobic coatings 20 kg of fluorosilicone resin, 10 kg of modified alumina crosslinking agent, 60 kg of modified hyperbranched polyester, 2 kg of triphenyl phosphite and 0.6 kg of titanium catalyst were mixed and dispersed in 50 L of solvent, heated to 160 ° C to react until no water was evaporated, cooled to below 30 ° C to obtain a super hydrophobic coating.
[0039] Preparation of water erosion resistant compressor impeller The impeller substrate was polished with sandpaper and an angle grinder, and the polished impeller substrate was cleaned with anhydrous ethanol to obtain a pretreated impeller substrate. 22.75kg molybdenum, 15.04kg nickel, 14.98kg cobalt, 14.1kg iron, 13.13kg chromium and 20kg reinforcing phase were mixed and dispersed in a planetary ball mill and ball milled at 300rpm for three hours. The mass ratio of silicon carbide, titanium nitride and cerium dioxide in the reinforcing phase was 1:1.55:1.29 to obtain a high entropy alloy powder. The high entropy alloy powder was laser clad using coaxial powder feeding, with a scanning speed of 10mm / s, a laser spot diameter of 3mm, a powder feeding speed of 1.2r / min, a laser power of 1200w, and an argon flow rate of 15L / min to obtain a high entropy alloy layer. The superhydrophobic coating was applied to the surface of the high entropy alloy layer and vacuum dried in an oven at 180℃ for 4h to obtain an anti-water erosion compressor impeller.
[0040] Example 3 Preparation of fluorosilicone resin: 18.18 kg of hexadecyltrimethoxysilane, 9.09 kg of diphenyldimethoxysilane and 2.73 kg of heptadecafluorodecyltrimethoxysilane were mixed and dispersed in 40 L of anhydrous ethanol to obtain a silane dispersion. 15 L of deionized water was added to the silane dispersion under stirring at 200 rpm and a 50°C water bath. The addition was completed within 30 min. After reacting for 3 h, the temperature was raised to 130°C and the reaction was continued for 30 min to obtain a product solution. The product solution was rotary evaporated to remove the solvent to obtain a fluorosilicone resin.
[0041] Preparation of aliphatic cyclohexyl modifier 12.79 kg of suberic acid, 7.21 kg of cyclohexene oxide and 0.08 kg of catalyst were mixed and dispersed, heated to 70° C. under nitrogen protection, stirred and refluxed at a speed of 200 rpm for 2 hours, and cooled to below 30° C. to obtain an aliphatic cyclohexyl modifier.
[0042] Preparation of modified hyperbranched polyester 47.48 kg of neopentyl glycol, 38.93 kg of 2-hydroxypropionic acid and 13.59 kg of trimethylolpropane were heated to melt to obtain a molten mixture, and stirring was started at a rate of 200 rpm. After keeping warm for 1 hour, 2 kg of triphenyl phosphite was added, and the temperature was raised to 240 ° C at a rate of 12 ° C / h for reaction for 2 hours, and the water was evaporated. The temperature was kept for 1 hour, and then the temperature was lowered to 180 ° C, 20 L of xylene and 15 kg of aliphatic cyclohexyl modifier were added, and the temperature was raised to 220 ° C again for reaction for 2 hours, and then reduced pressure distillation was performed, and the temperature was lowered to below 30 ° C to obtain a hyperbranched polyester.
[0043] Preparation of modified alumina crosslinking agent 15.3 kg of nano-alumina and 2.11 kg of dimethoxymethylsilyl chloride were dispersed in 200 mL of toluene, stirred at 200 rpm for 2 h, then 0.5 L of deionized water was added, and the mixture was stirred at 200 rpm for 4 h in a water bath at 80 ° C., 2.59 kg of decanediamine was added, and the mixture was stirred at 200 rpm for 4 h in a water bath at 80 ° C., the product solution was filtered, the solid was washed with anhydrous ethanol, and the washed solid was dried in an oven at 80 ° C. for 6 h. The dried solid was ground to obtain a modified alumina cross-linking agent.
[0044] Preparation of superhydrophobic coatings 15 kg of fluorosilicone resin, 7.5 kg of modified alumina crosslinking agent, 50 kg of modified hyperbranched polyester, 1.5 kg of triphenyl phosphite and 0.5 kg of titanium catalyst were mixed and dispersed in 45 L of solvent, heated to 160 ° C to react until no water was evaporated, cooled to below 30 ° C to obtain a super hydrophobic coating.
[0045] Preparation of water erosion resistant compressor impeller The impeller substrate was polished with sandpaper and an angle grinder, and the polished impeller substrate was cleaned with anhydrous ethanol to obtain a pretreated impeller substrate. 22.04kg molybdenum, 14.57kg nickel, 14.51kg cobalt, 13.66kg iron, 12.72kg chromium and 22.5kg reinforcing phase were mixed and dispersed in a planetary ball mill and ball milled at 300rpm for three hours. The mass ratio of silicon carbide, titanium nitride and cerium dioxide in the reinforcing phase was 1:1.55:1.075 to obtain a high entropy alloy powder. The high entropy alloy powder was laser clad using coaxial powder feeding, with a scanning speed of 10mm / s, a laser spot diameter of 3mm, a powder feeding speed of 1.2r / min, a laser power of 1200w, and an argon flow rate of 15L / min to obtain a high entropy alloy layer. The super hydrophobic coating was applied to the surface of the high entropy alloy layer and vacuum dried in an oven at 180℃ for 4h to obtain an anti-water erosion compressor impeller.
[0046] Example 4 Example 4 is based on Example 3. The only difference between Example 4 and Example 3 is that in Example 4, the amount of hexadecyltrimethoxysilane used is 19.35 kg, the amount of diphenyldimethoxysilane used is 9.68 kg, and the amount of heptadecafluorodecyltrimethoxysilane used is 0.97 kg.
[0047] Example 5 Example 5 is based on Example 3. The only difference between Example 5 and Example 3 is that in Example 5, the amount of hexadecyltrimethoxysilane used is 17.14 kg, the amount of diphenyldimethoxysilane used is 8.57 kg, and the amount of heptadecafluorodecyltrimethoxysilane used is 4.29 kg.
[0048] Example 6 Example 6 is based on Example 3. The only difference between Example 6 and Example 3 is that in Example 6, hexadecyltrimethoxysilane is replaced by methyltriethoxysilane when preparing the fluorosilicone resin.
[0049] Example 7 Example 7 is based on Example 3. The only difference between Example 7 and Example 3 is that in Example 7, diphenyldimethoxysilane is replaced by methyltriethoxysilane when preparing fluorosilicone resin.
[0050] Example 8 Example 8 is based on Example 3. The only difference between Example 8 and Example 3 is that in Example 8, no decanediamine is added when preparing the modified alumina crosslinking agent.
[0051] Example 9 Example 9 is based on Example 3. The only difference between Example 9 and Example 3 is that in Example 9, the aliphatic cyclohexyl modifier is replaced by cyclohexene oxide when preparing the modified hyperbranched polyester.
[0052] Example 10 Example 10 is based on Example 3, and the only difference between Example 10 and Example 3 is that in Example 10, the mass ratio of silicon carbide, titanium nitride and cerium dioxide is 1:1.55:0.75.
[0053] Embodiment 11 Example 11 is based on Example 3, and the only difference between Example 11 and Example 3 is that in Example 11, the mass ratio of silicon carbide, titanium nitride and cerium dioxide is 1:1.55:1.4.
[0054] Example 12 Example 12 is based on Example 3. The only difference between Example 12 and Example 3 is that silicon carbide is not added when preparing the high entropy alloy powder in Example 12.
[0055] Embodiment 13 Example 13 is based on Example 3. The only difference between Example 13 and Example 3 is that titanium nitride is not added when preparing the high entropy alloy powder in Example 13.
[0056] Embodiment 14 Example 14 is based on Example 3. The only difference between Example 14 and Example 3 is that no cerium dioxide is added when preparing the high entropy alloy powder in Example 14.
[0057] Comparative Example 1 Comparative Example 1 is based on Example 3, and the only difference between Comparative Example 1 and Example 3 is that in Comparative Example 1, the fluorosilicone resin is replaced by heptadecafluorodecyltrimethoxysilane.
[0058] Comparative Example 2 Comparative Example 2 is based on Example 3, and the only difference between Comparative Example 2 and Example 3 is that in Comparative Example 2, the modified alumina crosslinking agent is replaced by nano alumina.
[0059] Comparative Example 3 Comparative Example 3 is based on Example 3. The only difference between Comparative Example 3 and Example 3 is that in Comparative Example 3, no aliphatic cyclohexyl modifier is added when preparing the modified hyperbranched polyester.
[0060] Comparative Example 4 Comparative Example 4 is based on Example 3, and the only difference between Comparative Example 4 and Example 3 is that in Comparative Example 4, the high entropy alloy powder is replaced with sulphuric alloy.
[0061] Performance testing (1) Hardness test: Use a Vickers hardness tester to calculate the Vickers hardness of the sample. Each sample is tested three times and the average value is taken after measurement. The results are recorded in Table 1.
[0062] (2) Wear resistance test: Prepare the test specimens, clean them, dry them, weigh them and record the weight before wear, put them into the testing machine for wear test, clean and dry them again after the test, record the weight after wear, and calculate the weight loss after wear. Prepare three specimens for each sample, take the average value after measurement, and record the results in Table 1.
[0063] (3) Corrosion resistance test: Prepare the test specimens for the experiment, and place them in a simulated humid atmosphere for 3 weeks. Record the weight of the specimens before and after the experiment, and calculate the corrosion weight loss. Prepare three specimens for each sample, take the average value after measurement, and record the results in Table 1.
[0064] Table 1 Test results of impeller hardness and water erosion resistance It can be seen from Table 1 that the hardness of Examples 1-3 is greater than 936 HV, the weight loss due to wear is less than 0.26 g, and the weight loss due to corrosion is less than 8.2 mg, which shows that the compressor impeller prepared in the present application has high hardness and good water erosion resistance.
[0065] As can be seen from Table 1, the only difference between Examples 4 and 5 and Example 3 is that the mass ratio of hexadecyltrimethoxysilane, diphenyldimethoxysilane and heptadecafluorodecyltrimethoxysilane in Example 4 is 1:0.5:0.05, and the mass ratio of hexadecyltrimethoxysilane, diphenyldimethoxysilane and heptadecafluorodecyltrimethoxysilane in Example 5 is 1:0.5:0.25. Compared with Example 3, the hardness and water erosion resistance of Examples 4 and 5 are reduced; this is because the mass ratio of hexadecyltrimethoxysilane, diphenyldimethoxysilane and heptadecafluorodecyltrimethoxysilane is not within the specified range, too much or too little fluorine-containing silane will affect the hydrophobicity, stability and wetting properties, the stability of the super hydrophobic layer is reduced, and thus the hardness and water erosion resistance are reduced.
[0066] As can be seen from Table 1, the only difference between Examples 6 and 7 and Example 3 is that: in Example 6, hexadecyltrimethoxysilane is replaced with methyltriethoxysilane when preparing the fluorosilicone resin, and in Example 7, diphenyldimethoxysilane is replaced with methyltriethoxysilane when preparing the fluorosilicone resin. Compared with Example 3, the hardness and water erosion resistance of Examples 6 and 7 are reduced; this is because the synthetic components of the fluorosilicone resin are replaced, and the lack of phenyl and long-chain alkyl structures will affect the structural rigidity and ability to resist external impact of the fluorosilicone resin, thereby reducing the hardness and water erosion resistance.
[0067] As can be seen from Table 1, the only difference between Examples 8 and 9 and Example 3 is that: in Example 8, no decanediamine is added when preparing the modified alumina cross-linking agent, and in Example 9, the aliphatic cyclohexyl modifier is replaced by cyclohexene oxide when preparing the modified hyperbranched polyester. Compared with Example 3, Examples 8 and 9 have reduced hardness and water erosion resistance; this is because without adding decanediamine, the dispersibility and reactivity of the modified alumina cross-linking agent are reduced, thereby affecting the gain effect; when the aliphatic cyclohexyl modifier is replaced by cyclohexene oxide, the introduction of aliphatic long chains is lacking, the flexibility and ductility of the polyester are reduced, and the ability to resist external damage is weakened, thereby reducing the water erosion resistance.
[0068] As can be seen from Table 1, the only difference between Examples 10 and 11 and Example 3 is that the mass ratio of silicon carbide, titanium nitride and cerium dioxide in Example 10 is 1:1.55:0.75, and the mass ratio of silicon carbide, titanium nitride and cerium dioxide in Example 11 is 1:1.55:1.4. Compared with Example 3, the hardness and water erosion resistance of Examples 10 and 11 are reduced; this is because the mass ratio of silicon carbide, titanium nitride and cerium dioxide is not within the specified range, and too much or too little cerium dioxide will affect the microstructure and grain size distribution of the high entropy alloy, reduce the stability of the high entropy alloy, and thus the hardness and water erosion resistance are reduced.
[0069] It can be seen from Table 1 that the only difference between Examples 12, 13, and 14 and Example 3 is that: in Example 12, silicon carbide is not added when preparing the high entropy alloy powder, in Example 13, titanium nitride is not added when preparing the high entropy alloy powder, and in Example 14, cerium dioxide is not added when preparing the high entropy alloy powder. Compared with Example 3, the hardness and water erosion resistance of Examples 12, 13, and 14 are reduced; this is because the components of the reinforcing phase are reduced, and not adding silicon carbide or titanium nitride will destroy the synergistic effect of the two, thereby reducing the hardness and wear resistance of the high entropy alloy; not adding cerium dioxide will affect the microstructure of the high entropy alloy and increase the friction coefficient of its surface, thereby reducing the hardness and water erosion resistance.
[0070] It can be seen from Table 1 that the only difference between Comparative Example 1 and Example 3 is that: Comparative Example 1 replaces the fluorosilicone resin with heptadecafluorodecyltrimethoxysilane, and the hardness and water erosion resistance of Comparative Example 1 are significantly reduced compared with Example 3; this is because the fluorosilicone resin is replaced with heptadecafluorodecyltrimethoxysilane, lacking the co-condensation of alkyl silane and phenyl silane, and the rigidity, reactivity and compatibility of the fluorosilicone resin are reduced, thereby affecting the stability and bonding force of the super hydrophobic layer, so that the hardness and water erosion resistance are significantly reduced.
[0071] It can be seen from Table 1 that the only difference between Comparative Example 2 and Example 3 is that the modified alumina cross-linking agent is replaced by nano alumina in Comparative Example 2. Compared with Example 3, the hardness and water erosion resistance of Comparative Example 2 are significantly reduced; this is because the modified alumina cross-linking agent is replaced by nano alumina, and there is a lack of modification treatment, the nano alumina is prone to agglomeration, the dispersibility and reactivity are reduced, and the gain effect is greatly reduced, thereby greatly reducing the hardness and water erosion resistance of the impeller.
[0072] As can be seen from Table 1, the only difference between Comparative Example 3 and Example 3 is that no aliphatic cyclohexyl modifier is added when preparing the modified hyperbranched polyester in Comparative Example 3, and the hardness and water erosion resistance of Comparative Example 3 are reduced compared with Example 3; this is because without adding the aliphatic cyclohexyl modifier, the stability of the polyester is reduced, and the ability to resist external damage is weakened, thereby reducing the hardness and water erosion resistance of the impeller.
[0073] It can be seen from Table 1 that the only difference between Comparative Example 4 and Example 3 is that the high entropy alloy powder is replaced by Slit alloy in Comparative Example 4. Compared with Example 3, the hardness and water erosion resistance of Comparative Example 4 are significantly reduced; this is because the high entropy alloy powder is replaced by Slit alloy, and the high temperature performance and corrosion resistance of Slit alloy are slightly lacking, and the introduction of reinforcing phase is lacking, the hardness and corrosion resistance are reduced, and thus the hardness and water erosion resistance of the impeller are significantly reduced.
[0074] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A water erosion resistant compressor impeller, Features: The invention comprises an impeller substrate, a high entropy alloy layer and a super hydrophobic layer, wherein the super hydrophobic layer is obtained by coating a super hydrophobic coating on the surface of the high entropy alloy layer, and the raw materials for preparing the super hydrophobic coating include the following components in parts by weight: Fluorosilicone resin 10-20 parts Modified alumina crosslinking agent 5-10 parts 40-60 parts of modified hyperbranched polyester 1-2 parts of triphenyl phosphite Titanium catalyst 0.4-0.6 parts 40-50 parts of solvent.
2. The erosion-resistant compressor impeller according to claim 1, Features: The raw materials for preparing the fluorosilicone resin include hexadecyltrimethoxysilane, diphenyldimethoxysilane and heptadecafluorodecyltrimethoxysilane.
3. The erosion-resistant compressor impeller according to claim 2, Features: The mass ratio of hexadecyltrimethoxysilane, diphenyldimethoxysilane and heptadecafluorodecyltrimethoxysilane is 1:0.5:(0.1-0.2).
4. The erosion-resistant compressor impeller according to claim 1, Features: The raw materials for preparing the modified alumina cross-linking agent include nano alumina, dimethoxymethylchlorosilane and decanediamine.
5. The erosion-resistant compressor impeller according to claim 1, Features: The modified hyperbranched polyester comprises an aliphatic cyclohexyl modifier, trimethylolpropane, neopentyl glycol and 2-hydroxypropionic acid.
6. The water erosion resistant compressor impeller according to claim 5, Features: The raw materials for preparing the aliphatic cyclohexyl modifier include suberic acid and cyclohexene oxide.
7. The erosion-resistant compressor impeller according to claim 1, Features: The high entropy alloy layer is obtained by laser cladding high entropy alloy powder, wherein the high entropy alloy powder includes the following components in mass fractions: 21.33-22.75% molybdenum, 14.1-15.04% nickel, 14.04-14.98% cobalt, 13.22-14.1% iron, 12.31-13.13% chromium, and the remainder is a reinforcing phase.
8. The erosion-resistant compressor impeller according to claim 7, Features: The reinforcement phase includes silicon carbide, titanium nitride and cerium dioxide.
9. The erosion-resistant compressor impeller according to claim 8, Features: The mass ratio of silicon carbide, titanium nitride and cerium dioxide is 1:1.55:(0.86-1.29).
10. The erosion-resistant compressor impeller according to claim 1, Features: The anti-water erosion compressor impeller is prepared by the following steps: The impeller matrix is polished with sandpaper and an angle grinder, and the polished impeller matrix is cleaned with anhydrous ethanol to obtain a pretreated impeller matrix; the metal powder and the reinforcing phase are mixed and dispersed according to the ratio and ball-milled in a planetary ball mill to obtain a high-entropy alloy powder, and the high-entropy alloy powder is laser clad using coaxial powder feeding to obtain a high-entropy alloy layer; a super-hydrophobic coating is coated on the surface of the high-entropy alloy layer, and an anti-water erosion compressor impeller is obtained after drying.
Citation Information
Patent Citations
High-entropy alloy coating and preparation method thereof
CN105862035A
High-entropy alloy material with super-hydrophobic surface structure and preparation method of high-entropy alloy material
CN113684526A
Impeller and method for manufacturing same
JP2010229894A
Cited By
Modified fluorosilicone resin coating material with low thermal conductivity and high toughness as well as preparation method and application of modified fluorosilicone resin coating material
CN120888236A