In-situ preparation method of high-sensitivity VLEED spin analyzer target material
By using molecular beam epitaxy and magnetron sputtering techniques to prepare semi-metallic magnetic thin film targets with high spin polarizability, the problems of low spin polarizability and uneven surface of VLEED spin analyzer targets were solved, and high-sensitivity and stable electron spin measurement was achieved.
Patent Information
- Application Number
- CN202410961154.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
Existing VLEED spin analyzers suffer from low target spin polarization, uneven surfaces, and poor stability, resulting in low measurement efficiency.
Molecular beam epitaxy and magnetron sputtering techniques are used to prepare high spin polarizability semi-metallic magnetic thin film targets with atomically flat surfaces, such as Co2FeAl and Fe3O4, in a vacuum, ensuring large differences in surface stability and reflectivity.
The sensitivity and stability of the VLEED electron spin analyzer were improved, the relative difference in reflectivity of electrons on magnetized targets in different directions was increased, and the measurement efficiency was improved.
Smart Images

Figure CN118910566A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an in-situ preparation method of a high-sensitivity VLEED spin analyzer target material, and belongs to the cross-technical field of combining vacuum magnetic film growth technology with electron spin analysis technology. Background Art
[0002] At present, the analyzers for measuring electron spin mainly include Mott type, Spin-LEED type and VLEED type analyzers. Among them, VLEED is the electron spin analyzer with the highest measurement efficiency. Its measurement method is: first accelerate (decelerate) the electron kinetic energy to 6eV, then measure the reflectivity of the electron on the ferromagnetic target magnetized in the +Z and -Z directions respectively, and analyze the spin of the incident electron in the Z direction by measuring the relative difference between the two reflectivities.
[0003] Ferromagnetic materials usually selected as targets can achieve spin measurement, but their spin polarization is low. The relative difference in reflectivity of electrons on ferromagnetic targets magnetized in the +Z and -Z directions is small, so the measurement efficiency is low. In order to improve the measurement efficiency, it is necessary to select ferromagnetic materials with higher spin polarization. Semi-metallic ferromagnetic materials, such as Co2FeAl, Fe3O4, etc., have a Fermi surface that passes through the conduction band of one spin-oriented electron energy band and at the same time passes through the band gap of the opposite spin-oriented electron energy band. In other words, the conduction electrons of this material have only one spin orientation and theoretically have a 100% spin polarization. The surface of semi-metallic ferromagnetic materials has long-term stability and is suitable for the measurement of electron spin.
[0004] In addition, the flatness of the ferromagnetic film surface is closely related to the spin measurement efficiency. At present, the main methods for preparing ferromagnetic films by physical deposition are pulsed laser deposition (PLD), molecular beam epitaxy (MBE) and sputtering. The pulsed laser deposition method is only suitable for the growth and preparation of small-area films. The deposition of large-area films is prone to unevenness, which seriously affects the measurement efficiency. The molecular beam epitaxy and magnetron sputtering methods can prepare high-quality epitaxial ferromagnetic single crystal films and maintain the atomic-level flatness of the surface. Summary of the invention
[0005] In order to overcome the above-mentioned deficiencies of the prior art, the present invention provides an in-situ preparation method of a high-sensitivity VLEED spin analyzer target, which is used to solve the problems of low measurement efficiency caused by low spin polarization rate, uneven surface and poor stability of the existing VLEED spin analyzer target.
[0006] The technical solution adopted by the present invention is to use molecular beam epitaxy or magnetron sputtering technology to in-situ vacuum prepare a semi-metallic magnetic thin film target material with a high spin polarization rate and an atomically flat surface, such as Co2FeAl, Fe3O4, while the surface has long-term stability, thereby increasing the relative difference in reflectivity of electrons on the ferromagnetic target magnetized in the +Z and -Z directions, and improving the sensitivity and stability of the VLEED electron spin analyzer.
[0007] In the technical solution adopted by the present invention, a Co2FeAl single crystal thin film is grown on MgO by molecular beam epitaxy technology, and the three elements are deposited simultaneously by a thermal evaporation beam source furnace (K-cell), and the stoichiometric ratio of Co:Fe:Al is 2:1:1. The stoichiometric ratio of the three elements is determined by the thermal evaporation beam source furnace depositing on a quartz crystal at a corresponding temperature, and the deposition temperatures of the three elements are 1400°C, 1150°C, and 950°C, respectively, and the temperature stability does not exceed 0.1°C.
[0008] The technical solution adopted by the present invention is to prepare Fe3O4(001) single crystal thin film by magnetron sputtering technology, comprising the following steps:
[0009] Step 1: Install the target and obtain chamber vacuum;
[0010] Step 2: Substrate pretreatment;
[0011] Step 3: Pre-sputtering;
[0012] Step 4: Deposition of thin film.
[0013] Specifically, in step 1, a high-purity Fe (99.95%) target is used, and the vacuum degree of the chamber must reach 1×10 - 8 Torr.
[0014] The step 2 is: placing the MgO (001) substrate in acetone, alcohol and deionized water for ultrasonic cleaning for 30 minutes in sequence to remove oil and impurities on the surface of the substrate. After cleaning, the substrate is blown dry with nitrogen, placed in a sample holder, and introduced into the growth chamber through a vacuum system. The substrate is heated to 500°C for annealing for 30 minutes, and then cooled to the growth temperature of 300°C.
[0015] The step 3 is: introducing a mixed gas of high-purity argon (99.999%) and oxygen (99.999%), and adjusting the pumping rate to stabilize the gas pressure during sputtering at 4×10 -3 Torr. The ratio of oxygen and argon is controlled by an electronically controlled flow valve, the flow rate of oxygen is controlled to 1.5sccm, and the flow rate of argon is controlled to about 50sccm. Use a radio frequency power supply, set the power supply power to 50W, start pre-sputtering, and the time is 15min.
[0016] In step 4, during the deposition of the thin film, the substrate temperature was maintained at 300° C. and rotated at a speed of 5 rpm. Thin films of different thicknesses were deposited by controlling the sputtering time.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The semi-metallic ferromagnetic materials Co2FeAl and Fe3O4 have high spin polarization, which can increase the relative difference in reflectivity of electrons on ferromagnetic targets magnetized in the +Z and -Z directions, and improve the sensitivity of the VLEED electron spin analyzer;
[0019] 2. Molecular beam epitaxy and magnetron sputtering technology can produce high-quality ferromagnetic films with atomically flat surfaces, improving the film's reflectivity to electrons;
[0020] 3. In-situ vacuum preparation can reduce the adsorption of surface impurities caused by the contact between the film and the air, and improve the reflectivity of the film to electrons. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the working principle diagram of the VLEED spin analyzer.
[0022] Figure 2 RHEED patterns of Co2FeAl films along the
[100] (a) and
[110] (b) directions,
[0023] Figure 3 This is the atomic force microscope image of the Co2FeAl film surface.
[0024] Figure 4 The spin polarization test results of Co2FeAl film are shown in Figure 2.
[0025] Figure 5 This is the RHEED pattern of Fe3O4 film.
[0026] Figure 6 is the XRD pattern of Fe3O4 film.
[0027] Figure 7 The spin polarization test results of Fe3O4 film. DETAILED DESCRIPTION
[0028] In order to deepen the understanding of the present invention, the present embodiment is described in detail below with reference to the accompanying drawings.
[0029] Example 1: See Figure 1-Figure 7 , an in-situ preparation method for high-sensitivity VLEED spin analyzer targets, based on Figure 1The working principle diagram of the VLEED spin analyzer shown uses molecular beam epitaxy and magnetron sputtering technology to in-situ vacuum prepare semi-metallic magnetic thin film targets with atomically flat surfaces and high spin polarization rates, such as Co2FeAl and Fe3O4. At the same time, the surface has long-term stability, which improves the sensitivity and stability of the VLEED electron spin analyzer.
[0030] The Co2FeAl film prepared in the present invention is an epitaxial film grown on a MgO (100) substrate using a custom-made MBE device from Bostech, UK. The length and width of the substrate are both 10 nm. Before growth, the substrate needs to be placed in acetone ultrasound for 5 minutes, then cleaned with anhydrous ethanol, and finally cleaned with deionized water to remove the solvent adsorbed on the surface, and then blown dry with high-purity nitrogen. Then quickly put it into the loadlock and wait until the vacuum reaches 10 -7 After reaching the mbar level, it is introduced into the MBE growth chamber. Before growth, the MgO substrate needs to be annealed at 600K to remove the gas and moisture adsorbed on the surface and to achieve another reorganization of the lattice. The RHEED image of MgO can be clearly observed.
[0031] The present invention uses a method of co-growth of three elements. The stoichiometric ratio of the three elements can be determined by the temperature of the corresponding beam source furnace calibrated by a quartz crystal oscillator. The corresponding relationship between the quartz crystal oscillator and the beam source furnace temperature has been detected by a step profiler. The quartz crystal oscillator monitors the thickness per unit area, that is, the deposition rate, which is converted into a stoichiometric ratio:
[0032]
[0033] In the present invention, when the stoichiometric ratio is 2:1:1, the corresponding growth temperatures are 1385°C: 1151°C: 941°C respectively. The growth temperature of the thin film substrate is 250°C, and the entire growth process is monitored by a reflection high energy electron diffractometer (RHEED) to ensure that the film is in a single crystal state throughout the process.
[0034] Figure 2 The RHEED pattern of the Co2FeAl film displayed has clear and slender stripes, proving that the film grown by this method has a smooth surface and good crystallinity.
[0035] Figure 3 The atomic force microscope image of the Co2FeAl film surface shown proves that the film surface is atomically flat.
[0036] Figure 4 The spin-resolved photoelectron spectrum of the Co2FeAl film grown by this method is shown, and the spin polarization rate obtained by the test is 55±3%, which is consistent with the value obtained by theoretical calculation.
[0037] The present invention adopts a magnetron sputtering method to prepare a high-quality epitaxial single crystal Fe3O4 (001) film on a MgO (001) substrate, and characterizes the excellent performance of the film through a variety of experimental means. The present invention has a simple process, repeatability, low cost, no pollution, and is suitable for industrial application.
[0038] The following is a further description of the method for preparing high-quality epitaxial single crystal Fe3O4(001) thin films on MgO(001) substrates by magnetron sputtering in combination with specific embodiments and drawings:
[0039] Install high-purity Fe (99.95%) target material, evacuate the chamber, and the vacuum degree must reach 1×10 -8 Torr.
[0040] Take a 10×10mm MgO (001) substrate, put it in an acetone solution for ultrasonic cleaning for 30 minutes, then put it in anhydrous ethanol for ultrasonic cleaning for 30 minutes, and finally use deionized water for ultrasonic cleaning for 30 minutes, and blow it dry with nitrogen. The cleaned substrate is loaded into the sample holder and introduced into the growth chamber of magnetron sputtering through the vacuum interconnection system. Then set the annealing temperature to 500℃, anneal for 30 minutes, and set the speed to 5rpm. After annealing, maintain the growth temperature of 300℃, and introduce a mixed gas of high-purity argon (99.999%) and oxygen (99.999%). By adjusting the pumping rate, the gas pressure during sputtering is stabilized at 4×10 -3 Torr. The ratio of oxygen and argon is controlled by an electronically controlled flow valve, the flow rate of oxygen is controlled to 1.5sccm, and the flow rate of argon is controlled to about 50sccm. Use a radio frequency power supply, set the power supply power to 50W, start pre-sputtering, and the time is 15min.
[0041] The sample stage baffle was opened to start film deposition. After 15 minutes and 13 seconds, the baffle was closed to obtain a 50nm thick Fe3O4(100) film. Films of different thicknesses can be deposited by changing the time.
[0042] Figure 5 The RHEED pattern shows that the epitaxial relationship of the film is Fe3O4(001)
[001] / / MgO(001)
[001] . The Fe3O4(001) surface shows a clear The reconstruction and RHEED stripes are clear and slender, which proves that the film grown by this method has a smooth surface and good crystallinity.
[0043] Figure 6 The XRD patterns shown indicate that the Fe3O4(001) films grown by this method have a consistent orientation.
[0044] Figure 7The spin-resolved photoelectron spectrum of the 40nm Fe3O4 film grown by this method is shown, and the spin polarization rate obtained by the test is -42±3%, which is consistent with the value obtained by theoretical calculation.
[0045] In summary, the present invention discloses an in-situ preparation method of a high-sensitivity VLEED spin analyzer target, including: using molecular beam epitaxy or magnetron sputtering technology to in-situ vacuum prepare a high spin polarization rate semi-metal magnetic film target with atomic-level flat surface, such as Co2FeAl and Fe3O4, and the surface has long-term stability, thereby increasing the relative difference in reflectivity of the ferromagnetic target magnetized in the +Z and -Z directions and the reflectivity of the electron on the film, and improving the sensitivity and stability of the VLEED electron spin analyzer. Therefore, the present invention effectively overcomes various shortcomings in the prior art and has a high industrial utilization value.
[0046] It should be noted that the above embodiments are not intended to limit the protection scope of the present invention, and equivalent changes or substitutions made on the basis of the above technical solutions all fall within the protection scope of the claims of the present invention.
Claims
1. An in-situ preparation method for a high-sensitivity VLEED spin analyzer target, characterized in that: Molecular beam epitaxy or magnetron sputtering technology is used to in-situ vacuum prepare semi-metallic magnetic thin film targets with atomically flat surfaces and high spin polarization rate, including Co2FeAl and Fe3O4(001) films, whose surfaces have long-term stability.
2. The in-situ preparation method of a high-sensitivity VLEED spin analyzer target according to claim 1, characterized in that: The molecular beam epitaxy technology is used to in-situ vacuum prepare the Co2FeAl film with a high spin polarization rate and an atomically flat surface. A 1.8nm Co2FeAl single crystal film is grown on a MgO substrate. During the whole process, the stoichiometric ratio of the single crystal film is controlled by the temperature of the beam source furnace, and the whole process is monitored in real time by RHEED.
3. The in-situ preparation method of a high-sensitivity VLEED spin analyzer target according to claim 1, characterized in that: The magnetron sputtering technology was used to prepare the Fe3O4(001) thin film with high spin polarization rate and atomic level flat surface in situ vacuum. The target material was a high purity Fe target with a purity higher than 99.95%. The back vacuum of the cavity was lower than 1×10 - 8 Torr, the gas pressure during sputtering is stable at 4×10 -3 Torr, the flow rate ratio of argon to oxygen is 50sccm:1.5sccm, and the RF power is 50W.
4. The in-situ preparation method of a high-sensitivity VLEED spin analyzer target according to claim 1, characterized in that: The method for in-situ vacuum preparation of a high spin polarization rate semi-metallic magnetic film target Fe3O4 (001) film with a flat surface at the atomic level using magnetron sputtering technology comprises the following steps: Step 1: Equipment preparation: install high-purity Fe target with purity higher than 99.95%, evacuate the chamber to a vacuum degree of 1×10 -8 Torr, Step 2: Substrate preparation, Step 3: Pre-sputtering, Step 4: Deposition of thin film.
5. The in-situ preparation method of a high-sensitivity VLEED spin analyzer target according to claim 4, characterized in that: Step 2: Substrate preparation, as follows: Place the MgO (001) substrate in acetone, alcohol and deionized water for ultrasonic cleaning for 30 minutes in sequence to remove oil and impurities on the surface of the substrate. After cleaning, use nitrogen to blow dry the substrate, put it in a sample holder, and transfer it into the growth chamber through a vacuum system. Heat the substrate to 500°C for annealing for 30 minutes, and then cool it to the growth temperature of 300°C.
6. The in-situ preparation method of a high-sensitivity VLEED spin analyzer target according to claim 4, characterized in that: Step 3: Pre-sputtering, as follows: introduce a mixture of high-purity argon (99.999%) and oxygen (99.999%), and adjust the pumping rate to stabilize the gas pressure during sputtering at 4×10 -3 Torr, the flow rate of oxygen is controlled at 1.5sccm, the flow rate of argon is controlled at 50sccm, an RF power supply is used, the power is set to 50W, and pre-sputtering is started for 15min.
7. The in-situ preparation method of a high-sensitivity VLEED spin analyzer target according to claim 4, characterized in that: Step 4: Depositing a thin film, specifically as follows: Step (4) is: during sputtering, the substrate temperature is maintained at 300°C, the sample stage rotation speed is 5rpm, the sample stage baffle is opened to start depositing the thin film, and the thickness of the deposited film is controlled according to the sputtering time.