Method for efficiently reducing and rebalancing cutting residual stress of casing

By combining annealing heat treatment and vibration aging treatment, the problem of low efficiency in reducing residual stress during casing cutting is solved, achieving rebalancing and performance improvement of the casing, which is suitable for efficient stress reduction in large or complex casings.

CN118927001APending Publication Date: 2024-11-12HARBIN DONGAN ENGINE GRP +1

Patent Information

Application Number
CN202411094825.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing technologies are inefficient in eliminating residual stress from casing cutting, cannot effectively achieve rebalancing, and traditional methods do not process large or complex casings evenly, presenting technical bottlenecks.

Method used

The process employs a combination of annealing heat treatment and vibration aging treatment, including steps such as heating, heat preservation, natural cooling, and vibration aging. The casing is uniformly heated by a heater, and stress is induced using a vibration aging device. The effect is monitored using strain gauges and accelerometers.

Benefits of technology

It effectively eliminates residual stress in the casing, improves material stability and fatigue resistance, shortens the processing cycle, and enhances processing quality and long-term performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118927001A_ABST
    Figure CN118927001A_ABST
Patent Text Reader

Abstract

The invention discloses a method for efficiently reducing and rebalancing cutting residual stress of a casing, which comprises the following steps of: setting the heating temperature of a heater within a proper range, and uniformly heating the casing; a natural cooling mode is adopted; a measuring point is polished and cleaned through abrasive paper, the strain gauge and the casing are bonded through glue, and residual stress is measured through stress testing equipment; selecting vibration aging equipment; the vibration characteristics of the casing are monitored through an acceleration sensor, and the vibration aging effect is evaluated; the vibration aging can effectively restrain and eliminate the residual stress of the cartridge receiver part in a short time, the treatment period is shortened, and tiny displacement occurs in the material through vibration, so that deformation possibly occurring in subsequent machining is reduced, the fatigue life of the material is prolonged, and crack failure caused by stress concentration is reduced. Compared with traditional heat treatment, the crystal structure of the material cannot be remarkably changed through vibration aging, and the original performance is kept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal parts processing, in particular to a method for reducing and rebalancing residual stress in casing cutting with high efficiency. Background Art

[0002] During the machining process, the cutting operation of the casing often causes residual stress inside the material, thus affecting the performance and life of the product.

[0003] In the related art, the surface of the casing is struck to make the parts with residual stress yield, thereby relaxing the residual stress. However, for large or complex casings, it may be difficult to achieve comprehensive and uniform treatment by striking aging.

[0004] There are also methods that use vibration equipment to apply alternating stress to the casing to make it resonate, thereby reducing or eliminating residual stress by superimposing dynamic stress and residual stress, but its effect may be limited by factors such as the shape, size and material of the casing. In addition, for certain specific types of residual stress (such as deep residual stress), the effect of vibration aging may not be obvious;

[0005] The casing is kept at a high temperature for a period of time, and then slowly cooled to eliminate residual stress. Heat treatment has very strict requirements on the process, such as the temperature difference in the furnace, the control of the heating rate and the cooling rate. If it is not handled properly, it may cause cracking of the component or generate new residual stress. In addition, heat treatment usually takes a long time and consumes a lot of energy;

[0006] The above traditional methods of eliminating residual stress are often inefficient and cannot effectively achieve rebalancing, and there are certain technical bottlenecks. Summary of the invention

[0007] The object of the present invention is to provide a method for reducing and rebalancing the residual stress of the casing cutting with high efficiency, so as to solve the problems raised in the above-mentioned background technology.

[0008] To achieve the above object, the present invention provides the following technical solution: a method for reducing and rebalancing residual stress of a casing during cutting with high efficiency, comprising the following steps:

[0009] Step 1, material preparation: Take the receiver and clean the oil, rust and other contaminants on the surface of the receiver;

[0010] Step 2, heating: setting the heating temperature of the heater within a suitable range to heat the casing evenly;

[0011] Step 3, heat preservation treatment: after the heater reaches the target temperature, maintain the temperature for a suitable time;

[0012] Step 4, cooling stage: using natural cooling method to gradually reduce the temperature of the casing to room temperature;

[0013] Step 5: Residual stress detection: Sand and clean the measuring point with sandpaper, glue the strain gauge to the housing, and measure the residual stress with stress testing equipment;

[0014] Step 6, vibration aging equipment preparation: select vibration aging equipment, place the vibration source on the casing, and install the acceleration sensor on the casing;

[0015] Step 7, vibration setting: adjust the parameters of the vibration aging equipment, the vibration aging equipment excites the stress in the casing, the acceleration sensor monitors the vibration characteristics of the casing and evaluates the vibration aging effect;

[0016] Step 8: Vibration aging treatment: The vibration of the vibration aging equipment is divided into five aging frequencies, each period is eight minutes;

[0017] Step nine, effect check: After the vibration aging treatment is completed, the casing is tested for residual stress.

[0018] Furthermore, in step one, the receiver is fixed using a clamp that matches the receiver structure.

[0019] Furthermore, in step two, the heater sets a uniform heating curve, gradually increases the temperature and maintains it for a fixed time, and reasonably controls the heating rate to prevent local overheating of the casing from generating new stresses.

[0020] Furthermore, in step three, the holding time is determined according to the casing thickness and material properties, and the temperature change of the heater is monitored.

[0021] Furthermore, in step five, the elastic modulus of the 7050 aviation aluminum alloy is set to 69 and the Poisson's ratio is set to 0.3.

[0022] Furthermore, in step six, the vibration source is fixed to the receiver using a threaded clamp. The acceleration sensor should be located opposite the vibration source and at the point farthest from the receiver where the vibration is strongest, and ensure that the vibration source can provide sufficient fluctuation frequency and amplitude.

[0023] Furthermore, in step seven, the maximum current of the vibration aging equipment is adjusted to 15A, and the equipment alarms at 10A. The acceleration range of the vibration aging equipment during the test phase is 20m / s 2 -160m / s 2 , it can only start when it reaches this range; the speed range of the vibration aging equipment is 0-8000rpm.

[0024] Furthermore, in step nine, the residual stress before and after the casing treatment is compared to ensure that the casing rebalancing reaches the expected goal.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) The annealing heat treatment used in this method can effectively eliminate the residual stress generated during the casing processing, improve the overall stability of the material, and reduce the risk of deformation. By heating and slow cooling, the crystal structure of the material is improved, and the toughness, plasticity and fatigue resistance are improved.

[0027] (2) Vibration aging can effectively suppress and eliminate residual stress in the casing in a short time, shortening the overall processing cycle. Vibration causes a small displacement inside the material, thereby reducing deformation that may occur in subsequent processing. After effectively reducing residual stress, it helps to improve the fatigue life of the material and reduce crack failure caused by stress concentration. Compared with traditional heat treatment, vibration aging will not significantly change the crystal structure of the material and maintain the original performance.

[0028] (3) The method of combining annealing heat treatment with vibration aging treatment can not only effectively reduce the residual stress of the casing cutting, but also achieve the rebalancing of the casing, improve the processing quality and long-term performance, and has significant industrial application potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the strain gauge of the present invention being placed at the detection position of the casing;

[0030] Figure 2 It is a schematic diagram of the vibration aging device of the present invention being placed on a casing;

[0031] Figure 3 It is a schematic diagram of the acceleration sensor of the present invention being placed at the detection position of the casing;

[0032] Figure 4 It is a schematic diagram of the placement of the casing and the rubber support vibration isolation block of the present invention.

[0033] In the figure: 1. Casing; 2. Strain gauge; 3. Acceleration sensor; 4. Threaded clamp; 5. Vibration aging equipment; 6. Rubber support isolation block. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example:

[0036] See also Figure 1-4,The present invention provides a technical solution: a method for reducing and rebalancing the residual stress of the casing cutting with high efficiency;

[0037] Step 1, material preparation: Ensure that the surface of the receiver 1 is clean and free of oil, rust and other contaminants. Fix the receiver 1 in a suitable fixture to prevent deformation during heating.

[0038] Step 2 Heating process: Select appropriate heating equipment, such as a vacuum furnace, and set an appropriate heating temperature (generally between 600°C and 900°C, depending on the material of the casing 1). Apply a uniform heating curve, gradually increase the temperature and maintain it for a fixed time, and reasonably control the heating rate (including but not limited to controlling the heating rate to 20°C to 50°C per hour) to ensure that the temperature inside the material is evenly distributed, thereby preventing new stress caused by local overheating.

[0039] Step 3: Insulation treatment: After reaching the target temperature, maintain the temperature for a certain period of time (maintain the temperature for 2 to 4 hours, depending on the material setting of the casing 1). The insulation time is determined according to the thickness and material properties of the casing 1. Monitor the temperature change to ensure that it is within the specified range.

[0040] Step 4 Cooling stage: Use furnace cooling (natural cooling) to gradually reduce the material temperature to room temperature. During this process, rapid cooling should be avoided to reduce the re-generation of internal stress.

[0041] Step 5: Workpiece residual stress detection: Sand and clean the measuring point with sandpaper, glue the strain gauge 2 and the casing 1 workpiece with glue, and measure the residual stress with HK21A stress test equipment. The strain gauge 2 is electrically connected to the stress test equipment, and the elastic modulus of 7050 aviation aluminum alloy is set to 69 and the Poisson's ratio is set to 0.3. The residual stress measurement values ​​before vibration aging treatment are shown in Table 1.

[0042] Table 1 Residual stress test results before vibration aging treatment

[0043] Example Angle (°) Residual stress measurement value (MPa) 1 -11.39 -25.99 2 -38.42 -13.62 3 -42.83 -16.53

[0044] Step 6 Preparation of vibration aging equipment 5: Select HK3010 as vibration aging equipment 5, such as Figure 4 As shown, the casing 1 is placed on three rubber support vibration isolation blocks 6, the angle formed by the line between every two rubber support vibration isolation blocks 6 and the center of the casing 1 is 120°, and the vibration aging device 5 is fixed to the casing using a threaded clamp 4;

[0045] When placing the vibration aging device 5, the vibration aging device 5 should be located between the two rubber support vibration isolation blocks 6 and as far away from the rubber support vibration isolation blocks 6 as possible, and the acceleration sensor 3 should be installed. The acceleration sensor 3 should be located at the farthest vibration point from the opposite side of the vibration aging device 5 to the casing 1 with the strongest vibration feeling, ensuring that it can provide sufficient fluctuation frequency and amplitude to effectively excite the residual stress in the casing 1.

[0046] Step 7: Vibration setting: The vibration aging equipment 5 has three modes: spectrum aging, sub-resonance aging, and manual aging. Since the sub-resonance aging mode has a poor effect on the residual stress reduction of the casing 1, the spectrum aging mode is selected. The maximum current of this mode is 15A. The device alarms at 10A, and the current is generally below 7A; the acceleration range during the test phase is 20m / s 2 -160m / s 2 , it can only start when it reaches this range; the speed range is 0-8000rpm.

[0047] Step 8: Vibration aging treatment: divided into five aging frequencies, each period is eight minutes, a total of 40 minutes.

[0048] Step 9 Effect inspection: After the vibration aging treatment is completed, the residual stress is tested and step 1 is repeated. The residual stress measurement value and residual stress reduction rate after vibration aging treatment are shown in Table 2. Compare the residual stress before and after the treatment to ensure that the rebalancing of the casing 1 reaches the expected goal.

[0049] Table 2 Residual stress test results after vibration aging treatment

[0050]

[0051] Vibration aging can effectively suppress and eliminate some residual stress in the casing 1 in a short time, shorten the overall processing cycle, and cause a small displacement inside the material through vibration, thereby reducing the deformation that may occur in subsequent processing. After effectively reducing the residual stress, it helps to increase the fatigue life of the material and reduce crack failure caused by stress concentration. Compared with traditional heat treatment, vibration aging will not significantly change the crystal structure of the material and maintain the original performance.

[0052] The method combining annealing heat treatment and vibration aging treatment can not only effectively reduce the cutting residual stress of the casing 1, but also realize the rebalancing of the casing 1, improve the processing quality and long-term performance, and has significant industrial application potential.

[0053] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for reducing and rebalancing residual stress in high-efficiency casing cutting, characterized in that: The following steps are involved: Step 1, material preparation: Take the receiver and clean the oil, rust and other contaminants on the surface of the receiver; Step 2, heating: setting the heating temperature of the heater within a range that matches the material of the casing to heat the casing evenly; Step 3: Insulation treatment: After the heater reaches the target temperature, insulation is performed based on the casing material; Step 4, cooling stage: using natural cooling method to gradually reduce the temperature of the casing to room temperature; Step 5: Residual stress detection: Sand and clean the measuring point with sandpaper, glue the strain gauge to the housing, and measure the residual stress with stress testing equipment; Step 6, vibration aging equipment preparation: select vibration aging equipment, place the vibration source on the casing, and install the acceleration sensor on the casing; Step 7, vibration setting: adjust the parameters of the vibration aging equipment, the vibration aging equipment excites the stress in the casing, the acceleration sensor monitors the vibration characteristics of the casing and evaluates the vibration aging effect; Step 8: Vibration aging treatment: The vibration of the vibration aging equipment is divided into five aging frequencies, each period is eight minutes; Step nine, effect inspection: After the vibration aging treatment is completed, the casing is tested for residual stress.

2. The method for reducing and rebalancing high-efficiency casing cutting residual stress according to claim 1, characterized in that: In step one, the receiver is fixed using a clamp that matches the receiver structure.

3. The method for reducing and rebalancing high-efficiency casing cutting residual stress according to claim 1, characterized in that: In step two, the heater sets a uniform heating curve, gradually increases the temperature and maintains it for a fixed time, and controls the heating rate to prevent local overheating of the casing and the generation of new stresses.

4. The method for reducing and rebalancing high-efficiency casing cutting residual stress according to claim 1, characterized in that: In step three, the holding time is determined according to the casing thickness and material properties, and the temperature change of the heater is monitored.

5. The method for reducing and rebalancing high-efficiency casing cutting residual stress according to claim 1, characterized in that: In step five, the elastic modulus of 7050 aviation aluminum alloy is set to 69 and the Poisson's ratio is set to 0.

3.

6. The method for reducing and rebalancing high-efficiency casing cutting residual stress according to claim 1, characterized in that: In step six, use a threaded clamp to fix the vibration source to the receiver. The acceleration sensor should be located opposite the vibration source and at the point farthest from the receiver where the vibration is strongest, to ensure that the vibration source can provide sufficient fluctuation frequency and amplitude.

7. The method for reducing and rebalancing high-efficiency casing cutting residual stress according to claim 1, characterized in that: In step 7, adjust the maximum current of the vibration aging equipment to 15A. The equipment alarms at 10A. The acceleration range of the vibration aging equipment during the test phase is 20m / s 2 -160m / s 2 ; The speed range of vibration aging equipment is 0-8000rpm.

8. The method for reducing and rebalancing high-efficiency casing cutting residual stress according to claim 1, characterized in that: In step nine, the residual stresses before and after the receiver treatment are compared to ensure that the receiver rebalancing achieves the desired goal.

Citation Information

Patent Citations

  • Composite destressing process method

    CN101906599A

  • Method for eliminating internal stress and improving ultrahigh-strength steel thin-wall workpiece dimension accuracy

    CN106939371A

  • Cartridge receiver modal broadband vibration destressing method

    CN117625942A

  • Metal internal stress treatment device

    CN117737402A

  • Cooling device for turbine case

    JP2004190621A

Cited By

  • Process for machining a gh4169 type nickel-based superalloy annular casing

    CN122703264A