Preparation method and application of magnesium aluminum fluoride nanocrystal rich in defects
By using defect-rich magnesium aluminum fluoride nanocrystals as fillers in polymer electrolytes, the mechanical properties and stability of polymer electrolytes are solved, and battery performance with high energy density and long cycle life is achieved.
Patent Information
- Application Number
- CN202410984997.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Existing polymer electrolytes have high crystallinity, weak mechanical properties and antioxidant properties limitations in battery applications, and the phase separation between PEO and PVDF-HFP blending systems is not conducive to performance improvement, making it difficult to develop low-cost, industrially scalable Solid-state batteries with high energy density and stable cycle life.
Using defect-rich magnesium aluminum fluoride nanocrystals as inorganic fillers, magnesium aluminum fluoride nanocrystals are prepared by low-cost vermiculite and hydrofluoric acid treatment, and PEO-based all-solid state or PEO/PVDF-HFP concrete gel polymer is added. In the electrolyte, its mechanical properties and lithium salt dissociation are enhanced, and phase separation is suppressed through ultrasonic dispersion and sealing stirring.
The mechanical and electrochemical properties of polymer electrolytes are improved, the compatibility between PEO and PVDF-HFP is enhanced, phase separation is suppressed, and the stability and long cycle life of polymer electrolytes are achieved.
Smart Images

Figure CN118929719A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing magnesium aluminum fluoride nanocrystals, in particular to a method for preparing defect-rich magnesium aluminum fluoride nanocrystals and application thereof. Background Art
[0002] Polymer electrolytes (PEs) are considered to be one of the promising contenders for battery electrolytes due to their light weight, high flexibility, excellent manufacturability, and strong adhesion to electrodes. Generally, PEs can be divided into solid polymer electrolytes (SPEs) and gel polymer electrolytes (GPEs). SPEs have superior safety, among which PEO can react with Li + Complexation to achieve Li + Transport and has been widely studied as an all-solid-state polymer main matrix. However, the high crystallinity, weak mechanical properties and antioxidant properties of PEO-based all-solid-state polymer electrolytes limit their practical applications. The key to improving their performance lies in increasing the dissociation degree of lithium salts in the electrolyte and reducing the crystallinity of the polymer to improve the movement of polymer segments. GPEs are composed of a polymer matrix containing a liquid electrolyte, which can provide a better electrode / electrolyte contact interface and higher ionic conductivity. In gel polymer electrolytes, PVDF-HFP itself has CF chemical bonds and sufficient electrolyte absorption capacity to become a rigid skeleton of the gel polymer electrolyte, but PVDF-HFP conducts Li + Poor ability; while PEO can achieve Li + Therefore, the blending of PEO and PVDF-HFP has been widely studied because of its complementary performance. However, the incompatibility between PEO and PVDF-HFP leads to phase separation, which is not conducive to the improvement of the performance of the blending system. The development of low-cost, industrially scalable solid-state batteries with high energy density and stable cycle life remains a challenge.
[0003] In summary, in order to solve the above technical problems, the present invention provides a method for preparing defect-rich magnesium aluminum fluoride nanocrystals and applications thereof. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation method and application of defect-rich magnesium aluminum fluoride nanocrystals. The present invention has the advantages of simple preparation method, low cost, rich fluorine elements and defects in the prepared defect-rich magnesium aluminum fluoride nanocrystals, adding defect-rich magnesium aluminum fluoride nanocrystals as inorganic fillers to polymer electrolytes, and in PEO-based all-solid polymer electrolyte systems, the electrolyte membrane has excellent mechanical properties, high lithium salt dissociation degree, and good electrochemical properties of the polymer electrolyte; in PEO / PVDF-HFP blended gel polymer electrolyte systems, the compatibility between PEO and PVDF-HFP is improved, the phase separation between polymers is suppressed, and the gel polymer electrolyte has good stability.
[0005] The technical solution of the present invention is a method for preparing defect-rich magnesium aluminum fluoride nanocrystals, comprising the following steps:
[0006] (1) Add 10-20 g of vermiculite to 400-500 mL of deionized water, stir in an oil bath at 50-70° C. for 8-12 h, let stand for 0.5-1.5 h, remove the impurities floating on the upper layer and the vermiculite that has not been dispersed and peeled off at the bottom layer, filter by suction, and dry at 50-70° C. for 15-30 h to obtain product A;
[0007] (2) Add 6-10 g of product A to 300-500 mL of deionized water, stir and disperse, add 30-50 mL of 30-40% hydrofluoric acid, stir in an oil bath at 40-80° C. for 6-10 h, vacuum filter, wash with deionized water until the pH of the deionized water is 6.5-7, and obtain rod-shaped magnesium aluminum fluoride nanocrystals, which are product B;
[0008] (3) Add 1-3 g of product B into 400-800 mL of deionized water, stir and disperse at 200-1000 rad / min for 10-50 min, seal and store at 15-35° C. for 5-15 days, and freeze-dry at -60--40° C. for 20-28 h to obtain defect-rich magnesium aluminum fluoride nanocrystals, denoted as MgAlF 5· 1.5H2O.
[0009] In the aforementioned method for preparing defect-rich magnesium aluminum fluoride nanocrystals, the vermiculite is thermally expanded vermiculite clay containing magnesium / aluminum oxide octahedrons.
[0010] In the aforementioned method for preparing defect-rich magnesium aluminum fluoride nanocrystals, in the step (1), 15 g of vermiculite is added to 450 mL of deionized water, stirred in an oil bath at 60° C. for 10 h, allowed to stand for 1 h, impurities floating on the upper layer and vermiculite that has not been dispersed and peeled off at the bottom layer are removed, filtered, and dried at 60° C. for 24 h to obtain product A.
[0011] In the aforementioned method for preparing defect-rich magnesium aluminum fluoride nanocrystals, in step (2), 8 g of product A is stirred and dispersed in 400 mL of deionized water, 40 mL of 35% hydrofluoric acid is added, and the mixture is stirred in an oil bath at 60° C. for 8 h, vacuum filtered, and washed with deionized water until the pH of the deionized water is 6.8-7 to obtain rod-shaped magnesium aluminum fluoride nanocrystals, which are product B.
[0012] In the aforementioned method for preparing defect-rich magnesium aluminum fluoride nanocrystals, in the step (3), 2 g of product B is added to 600 mL of deionized water, stirred and dispersed at 500 rad / min for 30 min, sealed and stored at 25° C. for 10 days, and freeze-dried at -50° C. for 24 h to obtain defect-rich magnesium aluminum fluoride nanocrystals.
[0013] The application of the defect-rich magnesium aluminum fluoride nanocrystals is to add the defect-rich magnesium aluminum fluoride nanocrystals as fillers into polymer electrolytes.
[0014] In the application of the aforementioned defect-rich magnesium aluminum fluoride nanocrystals, the defect-rich magnesium aluminum fluoride nanocrystals are specifically dried under vacuum at 80-120° C. for 20-28 hours, added into a polymer electrolyte, ultrasonically dispersed, and sealed and stirred.
[0015] In the application of the aforementioned defect-rich magnesium aluminum fluoride nanocrystals, the polymer electrolyte is a PEO-based all-solid polymer electrolyte or a PEO / PVDF-HFP blended gel polymer electrolyte.
[0016] 1. The present invention uses low-priced and abundant vermiculite as a raw material. The vermiculite is a thermally expanded vermiculite clay containing magnesium / aluminum oxide octahedron. Therefore, 10-20 g of vermiculite is added to 400-500 mL of deionized water, and the mixture is stirred in an oil bath at 50-70° C. for 8-12 hours. The weak interaction between the vermiculite lamellae is weakened by stirring shear force to peel off the vermiculite, thereby obtaining lamellae of nano vermiculite. The mixture is allowed to stand for 0.5-1.5 hours, and impurities floating on the upper layer and vermiculite that is not dispersed and peeled off at the bottom layer are removed. The mixture is filtered by suction, and dried at 50-70° C. for 15-30 hours to obtain a layered vermiculite (VS) whose main components are two layers of silicon oxide tetrahedron and interlayer magnesium / aluminum oxide octahedron.
[0017] 2. Treating magnesium-aluminum-rich vermiculite (VS) with hydrofluoric acid to prepare magnesium-aluminum fluoride nanocrystalline materials. The raw materials used are cheap, the process operation is simple, and the process conditions are simple. Specifically, 6-10g VS is added to 300-500mL deionized water, stirred and dispersed, and 30-50mL of 30-40% hydrofluoric acid is added. Stir in an oil bath at 40-80℃ for 6-10h. The silicon oxide on the layered vermiculite is etched away by hydrofluoric acid, and the Mg in the solution is 2+ and Al 3+With F - Combined to form rod-shaped magnesium aluminum fluoride nanocrystals.
[0018] 3. The defect-rich magnesium aluminum fluoride nanocrystals prepared by the present invention have rich fluorine elements and controllable defect concentration. Metal fluorides exist in dissociation equilibrium in water. 1-3g of rod-shaped magnesium aluminum fluoride nanocrystals are added to 400-800mL of deionized water, stirred and dispersed at 200-1000rad / min for 10-50min, and sealed and stored at 15-35℃ for 5-15 days. The defect-rich magnesium aluminum fluoride nanocrystals in the aqueous solution will release F into the aqueous solution. - As time goes by, F - The release brings about a higher fluorine vacancy concentration. The present invention controls the sealed storage time to 5-15 days to achieve the F in metal fluoride - Release and regulate the fluorine vacancies in the material to the optimal concentration. Too low a fluorine vacancy concentration is not conducive to the dissociation of lithium salts and the transmission of lithium ions in the material, while a higher fluorine vacancy concentration will lead to a strong interaction between the filler and the polymer and reduce the antioxidant capacity of the polymer.
[0019] 4. The present invention vacuum dries the defect-rich magnesium aluminum fluoride nanocrystals at 80-120° C. for 20-28 hours, adds them to a polymer electrolyte, disperses them ultrasonically, and stirs them in a sealed manner in order to remove moisture adsorbed in the material. Ultrasound is used to evenly disperse the filler, and sealed stirring is used to prevent the influence of moisture in the air.
[0020] 5. The defect-rich magnesium aluminum fluoride nanocrystal (MAF) material prepared by the present invention is used as a filler in a PEO-based all-solid polymer electrolyte system. The filler reduces the polymer crystallinity through internal multi-scale effects, and the hydrogen bonds established between MAF and PEO help to improve the mechanical properties of SPE and broaden its voltage stability window (ESW). The abundant fluorine vacancies on MAF enhance the fixation of MAF on lithium salt anions and weaken the Li-F bond. The lithium salt dissociation degree in the polymer is high and rapid lithium ion transmission is achieved. Therefore, the corresponding PEO-based all-solid polymer electrolyte has good electrochemical properties.
[0021] 6. The defect-rich magnesium aluminum fluoride nanocrystal (MAF) material prepared by the present invention is used as a filler in the PEO / PVDF-HFP blended gel polymer electrolyte system. MAF, as an inorganic filler, acts as a compatibilizer, interacts with the surfaces of the two polymer components to form an interpenetrating polymer network, and improves the miscibility and stability between PEO and PVDF-HFP in the blended gel polymer. The interaction between the fluoride and the polymer enhances the interfacial bonding between the components, improves the segmental motion of the polymer, hinders the phase separation of the system, eliminates phase agglomeration, and prepares a blend with strong interphase bonds. The ion migration and stability of the gel polymer membrane are enhanced by eliminating phase separation and interfacial defects. Therefore, the battery assembled with the gel polymer membrane has long-term cycle stability.
[0022] In summary, the present invention has the advantages of simple preparation method and low cost. The prepared defect-rich magnesium aluminum fluoride nanocrystals have rich fluorine elements and defects. The defect-rich magnesium aluminum fluoride nanocrystals are added to the polymer electrolyte as inorganic fillers. In the PEO-based all-solid-state polymer electrolyte system, the electrolyte membrane has excellent mechanical properties, high lithium salt dissociation degree, and good electrochemical properties of the polymer electrolyte. In the PEO / PVDF-HFP blended gel polymer electrolyte system, the compatibility between PEO and PVDF-HFP is improved, the phase separation between polymers is suppressed, and the gel polymer electrolyte has the beneficial effect of good stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is an explanatory diagram of the heat-expanded vermiculite clay and the layered vermiculite (VS) of the present invention; wherein a is a digital picture of the heat-expanded vermiculite clay, b is a digital picture of the layered vermiculite (VS) obtained after treatment, c is a SEM picture of the layered vermiculite (VS), a mapping picture of Al, Mg, Fe, Si and O elements of the layered vermiculite (VS), and d is the content of various components in the layered vermiculite (VS) tested by XRF;
[0024] Figure 2 1 is a diagram showing the change in the material phase structure after the silicon oxide in the layered vermiculite (VS) is etched away with hydrofluoric acid, wherein a is the XRD diagram of the layered vermiculite (VS), b is the XRD diagram of the defect-rich magnesium aluminum fluoride nanocrystals, and c is a schematic diagram of the preparation of magnesium aluminum fluoride nanocrystals by etching the layered vermiculite (VS) with hydrofluoric acid;
[0025] Figure 3are scanning electron microscope (SEM) and transmission electron microscope (TEM) images of magnesium aluminum fluoride prepared in Example 2 of the present invention; wherein a is a scanning electron microscope (SEM) image of magnesium aluminum fluoride; b is a transmission electron microscope (TEM) image of magnesium aluminum fluoride, and c is a TEM image of magnesium aluminum fluoride and a corresponding mapping diagram of Al, Mg, F and O elements;
[0026] Figure 4 1 is a structure of defect-rich magnesium aluminum fluoride nanocrystals prepared in comparative example 1, embodiment 2 and comparative example 2 of the present invention and a characterization diagram of defect concentration change (the obtained materials are respectively recorded as MAF-1, MAF-2, and MAF-3); wherein, a is a digital photo of MAF-1, MAF-2, and MAF-3 dispersed in water; b is an EPR graph of MAF-1, MAF-2, and MAF-3; cd is an XPS fine spectrum of Mg 1s and Al 2s of the material; ef is an XRD spectrum of MAF-1, MAF-2, and MAF-3;
[0027] Figure 5 Figure 1 is a diagram of the mechanism of action of the rod-shaped magnesium aluminum fluoride nanocrystals in the present invention in a PEO-based polymer electrolyte calculated by first principle (DFT) simulation; wherein, Figure a is a configuration diagram of magnesium aluminum fluoride nanocrystals with a fluorine vacancy (denoted as MAF) and magnesium aluminum fluoride nanocrystals without fluorine vacancies (denoted as MAF(Ideal)), b is the adsorption of PEO on MAF and MAF(Ideal) configurations, c is the adsorption of lithium salt LiTFSI on PEO, MAF and MAF(Ideal), d is the adsorption of Li + and the calculated results of adsorption energy (Eb) of LiTFSI on PEO, MAF and MAF-FV configurations;
[0028] Figure 6 The present invention is comparative example 1, and the samples of embodiment 2 and comparative example 2 are applied to the performance comparison analysis of PEO-based all-solid polymer electrolyte according to application example 1 (the polymer membrane without filler is recorded as SPE-0, and the polymer membranes with MAF-1, MAF-2 and MAF-3 are recorded as SPE-MAF-1, SPE-MAF-2 and SPE-MAF-3 respectively); wherein a is the ionic conductivity bar graph of the polymer membrane at 50° C., b is the DSC graph of the polymer membrane, c is the lithium ion migration number of the polymer membrane at 50° C., d is the XRD graph of the polymer membrane, e is the voltage stability window graph of the polymer membrane at 50° C., and f is the thermogravimetric graph of the polymer membrane;
[0029] Figure 7The performance analysis of MAF-2 of Example 2 of the present invention applied to PEO-based all-solid polymer electrolyte according to Application Example 1 (the polymer membrane without filler is marked as SPE-0, and the polymer membrane with MAF-2 added is marked as SPE-MAF-2); wherein ab is the SEM image of the polymer membrane, c is the stress-strain image of the polymer membrane, d is the nanoindentation image of the polymer membrane, and e is the SEM image of the polymer membrane at 730-755cm -1 Raman spectra in the wavenumber range of , e is the constant current lithium plating / stripping electrochemical cycle, f is the rate cycle, and g is the long cycle diagram at 1C;
[0030] Figure 8 The performance comparison analysis of the samples of Comparative Example 1 and Example 2 of the present invention added to the composite membrane of PEO / PVDF-HFP blend according to Application Example 2 (the PEO / PVDF-HFP blended composite membrane without adding filler is recorded as CPE, and the PEO / PVDF-HFP blended composite membranes with adding MAF-1 and MAF-2 are recorded as CPE-MAF-1 and CPE-MAF-2 respectively). Wherein, ac are SEM images of CPE, CPE-MAF-1 and CPE-MAF-2 membranes, d is the XRD image of the membrane, and e is the infrared spectrum of the membrane;
[0031] Fig. 9 The invention discloses a comparative analysis of the electrochemical properties of a blended gel polymer electrolyte formed by soaking a composite membrane of CPE, CPE-MAF-1 and CPE-MAF-2 in an electrolyte (DOL / DME (1:1, v / v) 1M LiTFSI) (CPE, CPE-MAF-1 and CPE-MAF-2 are respectively recorded as GPE, GPE-MAF-1 and GPE-MAF-2 after being soaked in the electrolyte); wherein a is a histogram of electrolyte absorption rate, b is a Tafel curve graph, c is an ionic conductivity graph, and d is a long cycle graph at 1C. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.
[0033] Embodiment 1: A method for preparing defect-rich magnesium aluminum fluoride nanocrystals, comprising the following steps:
[0034] (1) Add 10 g of vermiculite to 400 mL of deionized water, stir in an oil bath at 50° C. for 8 h, let stand for 0.5 h, remove the impurities floating on the upper layer and the vermiculite that has not been dispersed and peeled off at the bottom layer, filter with suction, and dry at 50° C. for 15 h to obtain product A;
[0035] (2) Add 6 g of product A to 300 mL of deionized water, stir and disperse, add 30 mL of 30% hydrofluoric acid, stir in an oil bath at 40° C. for 6 h, vacuum filter, and wash with deionized water until the pH of the deionized water is 6.5 to obtain rod-shaped magnesium aluminum fluoride nanocrystals, which are product B.
[0036] (3) 1 g of product B was added to 400 mL of deionized water, stirred and dispersed at 200 rad / min for 10 min, sealed and stored at 15°C for 5 days, and freeze-dried at -60°C for 20 h to obtain defect-rich magnesium aluminum fluoride nanocrystals MgAlF 5· 1.5H2O(MAF).
[0037] Example 2: A method for preparing defect-rich magnesium aluminum fluoride nanocrystals, comprising the following steps:
[0038] (1) Add 15 g of vermiculite to 450 mL of deionized water, stir in an oil bath at 60° C. for 10 h, let stand for 1 h, remove the impurities floating on the upper layer and the vermiculite that has not been dispersed and peeled off at the bottom layer, filter with suction, and dry at 60° C. for 24 h to obtain product A;
[0039] (2) 8 g of product A was dispersed in 400 mL of deionized water, 40 mL of 35% hydrofluoric acid was added, and the mixture was stirred in an oil bath at 60° C. for 8 h. The mixture was vacuum filtered and washed with deionized water until the pH of the deionized water was 6.8-7 to obtain rod-shaped magnesium aluminum fluoride nanocrystals, which are product B.
[0040] (3) 2 g of product B was added to 600 mL of deionized water, stirred and dispersed at 500 rad / min for 30 min, sealed and stored at 25°C for 10 days, and freeze-dried at -50°C for 24 h to obtain defect-rich magnesium aluminum fluoride nanocrystals MgAlF 5· 1.5H2O(MAF), recorded as MAF-2.
[0041] Embodiment 3: A method for preparing defect-rich magnesium aluminum fluoride nanocrystals, comprising the following steps:
[0042] (1) Add 20 g of vermiculite to 500 mL of deionized water, stir in an oil bath at 70° C. for 12 h, let stand for 1.5 h, remove the impurities floating on the upper layer and the vermiculite that has not been dispersed and peeled off at the bottom layer, filter with suction, and dry at 70° C. for 30 h to obtain product A;
[0043] (2) Add 10 g of product A to 500 mL of deionized water, stir and disperse, add 50 mL of 40% hydrofluoric acid, stir in an oil bath at 80° C. for 10 h, vacuum filter, and wash with deionized water until the pH of the deionized water is 7 to obtain rod-shaped magnesium aluminum fluoride nanocrystals, which are product B.
[0044] (3) 3 g of product B was added to 800 mL of deionized water, stirred and dispersed at 1000 rad / min for 50 min, sealed and stored at 35°C for 15 days, and freeze-dried at -40°C for 28 h to obtain defect-rich magnesium aluminum fluoride nanocrystals MgAlF 5· 1.5H2O(MAF).
[0045] Application Example 1:
[0046] The defect-rich magnesium aluminum fluoride nanocrystals MgAlF prepared in Examples 1-3 are 5· 1.5H2O(MAF), added as filler to polymer electrolyte.
[0047] In the application of the aforementioned defect-rich magnesium aluminum fluoride nanocrystals, the defect-rich magnesium aluminum fluoride nanocrystals are specifically dried under vacuum at 80-120° C. for 20-28 hours, added into a polymer electrolyte, ultrasonically dispersed, and sealed and stirred.
[0048] In the aforementioned application of defect-rich magnesium aluminum fluoride nanocrystals, the polymer electrolyte is a PEO-based all-solid polymer electrolyte.
[0049] The specific process is as follows: 0.028 g MAF was first added to 15 mL anhydrous acetonitrile and ultrasonically stirred to make it completely dispersed, and then 0.4 g PEO (Aladdin, Mw = 6 × 10 5 g / mol), 0.14g lithium salt (LiTFSI, McLean, 99%), magnetic stirring at room temperature for 24 hours, and then evacuating the slurry in a vacuum box for 15 minutes to remove the gas in the solution. The solution was then cast on a polytetrafluoroethylene (PTFE) mold, dried at 40°C to remove most of the solvent, and then vacuum dried at 60°C for 24 hours to completely remove the solvent to obtain a polymer electrolyte membrane (SPE). The prepared polymer electrolyte membrane first constructed a steel sheet symmetrical battery and a lithium sheet symmetrical battery to test their corresponding lithium ion conductivity, lithium ion migration number and lithium plating / stripping. In addition, the polymer electrolyte was also used to construct a lithium iron phosphate battery to test charging and discharging.
[0050] Application Example 2:
[0051] The defect-rich magnesium aluminum fluoride nanocrystals MgAlF prepared in Examples 1-3 are 5· 1.5H2O(MAF), added as filler to polymer electrolyte.
[0052] In the application of the aforementioned defect-rich magnesium aluminum fluoride nanocrystals, the defect-rich magnesium aluminum fluoride nanocrystals are specifically dried under vacuum at 80-120° C. for 20-28 hours, added into a polymer electrolyte, and stirred by ultrasonic sealing.
[0053] In the application of the aforementioned defect-rich magnesium aluminum fluoride nanocrystals, the polymer electrolyte is a PEO / PVDF-HFP blended gel polymer electrolyte.
[0054] The specific process is that MAF (0.035g) is first added to 5mL of organic solvent DMF, ultrasonically stirred and dispersed, and then PVDF-HFP (0.25g) is added and stirred. After PVDF-HFP is completely dissolved, 10mL of anhydrous acetonitrile solvent and PEO (0.250g) are added, and magnetic stirring is performed at 40°C for 24 hours, and then the slurry is vacuumed in a vacuum box for 15 minutes to remove the gas in the solution, and then the solution is cast on a polytetrafluoroethylene (PTFE) mold, and dried at 50°C to remove most of the solvent, and then vacuum dried at 60°C for 12 hours to completely remove the solvent to obtain a PEO / PVDF-HFP blended composite membrane (referred to as CPE-MAF). In a glove box filled with argon, the prepared polymer membrane is placed in an organic electrolyte solution and soaked for 2 hours to obtain a PEO / PVDF-HFP blended gel polymer electrolyte membrane (referred to as GPE-MAF). The PEO / PVDF-HFP-MAF gel electrolyte was used to assemble the battery to test the ionic conductivity and charge-discharge cycle.
[0055] Comparative Example 1: A method for preparing defect-rich magnesium aluminum fluoride nanocrystals, comprising the following steps:
[0056] (1) Add 15 g of vermiculite to 450 mL of deionized water, stir in an oil bath at 60° C. for 10 h, let stand for 1 h, remove the impurities floating on the upper layer and the vermiculite that has not been dispersed and peeled off at the bottom layer, filter with suction, and dry at 60° C. for 24 h to obtain product A;
[0057] (2) 8 g of product A was dispersed in 400 mL of deionized water, 40 mL of 35% hydrofluoric acid was added, and the mixture was stirred in an oil bath at 60° C. for 8 h. The mixture was vacuum filtered and washed with deionized water until the pH of the deionized water was 6.8-7 to obtain rod-shaped magnesium aluminum fluoride nanocrystals, which are product B.
[0058] (3) 2 g of product B was added to 600 mL of deionized water, stirred and dispersed at 500 rad / min for 30 min, sealed and stored at 25° C. for 1 day, and freeze-dried at −50° C. for 24 h to obtain defect-rich magnesium aluminum fluoride nanocrystals, which were recorded as MAF-1.
[0059] Comparative Example 2: A method for preparing defect-rich magnesium aluminum fluoride nanocrystals, comprising the following steps:
[0060] (1) Add 15 g of vermiculite to 450 mL of deionized water, stir in an oil bath at 60° C. for 10 h, let stand for 1 h, remove the impurities floating on the upper layer and the vermiculite that has not been dispersed and peeled off at the bottom layer, filter with suction, and dry at 60° C. for 24 h to obtain product A;
[0061] (2) 8 g of product A was dispersed in 400 mL of deionized water, 40 mL of 35% hydrofluoric acid was added, and the mixture was stirred in an oil bath at 60° C. for 8 h. The mixture was vacuum filtered and washed with deionized water until the pH of the deionized water was 6.8-7 to obtain rod-shaped magnesium aluminum fluoride nanocrystals, which are product B.
[0062] (3) 2 g of product B was added to 600 mL of deionized water, stirred and dispersed at 500 rad / min for 30 min, sealed and stored at 25° C. for 20 days, and freeze-dried at −50° C. for 24 h to obtain defect-rich magnesium aluminum fluoride nanocrystals, which were recorded as MAF-3.
[0063] Experimental data:
[0064] 1. Figure 1 The heat-expanded vermiculite clay and the layered vermiculite (VS) of the present invention are illustrated in FIG. a, wherein a is a digital image of the heat-expanded vermiculite clay, b is a digital image of the layered vermiculite (VS) obtained after treatment, c is a SEM image of the layered vermiculite (VS), a mapping image of Al, Mg, Fe, Si and O elements of the layered vermiculite (VS), and d is the content of various components in the layered vermiculite (VS) tested by XRF; as shown in FIG. a, the heat-expanded vermiculite has a high impurity content, therefore, the heat-expanded vermiculite is dispersed in a deionized water solution. The layered vermiculite (VS) was obtained by stirring, peeling and drying in water as shown in FIG. b. As shown in FIG. c, the EDS element spectrum test results of the layered vermiculite (VS) showed that the vermiculite was a layered silicate rich in Al, Mg, Fe, Si and O, wherein the contents of various components were shown in FIG. d. The contents of SiO2, Fe2O3, Al2O3 and MgO in the layered vermiculite (VS) were 48.52wt.%, 21.14wt.%, 12.77wt.% and 10.21%, respectively. Therefore, by Figure 1 It can be seen that layered vermiculite (VS) is a layered silicate rich in magnesium and aluminum elements.
[0065] 2. Figure 2The figure shows the change in the material phase structure after the silicon oxide in the layered vermiculite (VS) is etched away with hydrofluoric acid, where a is the XRD diagram of the layered vermiculite (VS), b is the XRD diagram of the defect-rich magnesium aluminum fluoride nanocrystals, and c is a schematic diagram of the preparation of magnesium aluminum fluoride nanocrystals by etching the layered vermiculite (VS) with hydrofluoric acid. Figure a shows that the diffraction peaks of the layered vermiculite (VS) at 2θ of 6.03°, 8.95°, and 27.83° correspond to the (001) crystal plane in the vermiculite structure and the (001) and (003) crystal planes of phlogopite, respectively. The (001) crystal plane at 6.03° is the basic reflection feature of vermiculite, indicating the presence of double-layer water in the interlayer region of the silicate plate. As shown in Figure b, the material obtained after hydrofluoric acid etching of layered vermiculite (VS) has new diffraction peaks compared to layered vermiculite (VS). By comparing the standard XRD card (PDF#39-0665), it is confirmed that the material is magnesium aluminum fluoride crystal (MgAlF5·1.5H2O, denoted as MAF). The diffraction peaks at 15.7°, 18.1°, 25.25°, 29.5°, 29.7°, 30.8°, and 31.8° correspond to MgAlF 5· 1.5H2O (101), (011), (211), (301), (220), (202) crystal planes. In addition, the XRD spectrum of the material obtained after etching did not show the diffraction peak of layered vermiculite (VS), indicating that the vermiculite crystal structure has been destroyed by hydrofluoric acid and a new phase of magnesium aluminum fluoride has been generated. Figure c shows the process of preparing magnesium aluminum fluoride nanocrystals by hydrofluoric acid etching layered vermiculite (VS). Hydrofluoric acid can etch away the silicon oxide on the layered vermiculite (VS). The Mg in the solution 2+ and Al 3+ With F - Combined to form rod-shaped nanocrystals MgAlF5·1.5H2O. Figure 2 The results show that hydrofluoric acid etching of layered vermiculite (VS) will lead to the destruction of the crystal structure of layered vermiculite (VS) and the formation of a new phase MgAlF5·1.5H2O.
[0066] 3. Figure 3 The scanning electron microscope (SEM) and transmission electron microscope (TEM) images of magnesium aluminum fluoride prepared in Example 2 of the present invention are shown; wherein a is a scanning electron microscope (SEM) image of magnesium aluminum fluoride; b is a transmission electron microscope (TEM) image of magnesium aluminum fluoride; and c is a TEM image of magnesium aluminum fluoride and a corresponding mapping diagram of Al, Mg, F and O elements. As shown in Figures ab, it can be seen from the SEM and TEM images that the magnesium aluminum fluoride is a one-dimensional rod-shaped nanocrystal, and from the mapping diagram in Figure c, it can be seen that the Al, Mg, F and O elements in the magnesium aluminum fluoride are uniformly distributed, which is consistent with the elements shown by the XRD phase. Figure 3 It can be seen that magnesium aluminum fluoride is rod-shaped nanocrystals.
[0067] 4. Figure 4 The present invention is a comparative example 1, embodiment 2 and comparative example 2 of the present invention, and the structure of the defect-rich magnesium aluminum fluoride nanocrystals prepared and the defect concentration change characterization diagram (the obtained materials are respectively recorded as MAF-1, MAF-2, and MAF-3); wherein, a is a digital photo of MAF-1, MAF-2, and MAF-3 dispersed in water; b is an EPR diagram of MAF-1, MAF-2, and MAF-3; cd is the XPS fine spectrum of Mg 1s and Al 2s of the material; ef is the XRD spectrum of MAF-1, MAF-2, and MAF-3; it can be seen from Figure a that as the sealed storage time of the rod-shaped magnesium aluminum fluoride nanocrystal material in water increases, the color of the material gradually deepens, from white to light yellow and then to yellow, and the color change is due to the color center caused by the defect vacancies. From the electron paramagnetic resonance (EPR) test in Figure b, it can be seen that the signals of MAF-1, MAF-2 and MAF-3 in the EPR spectrum at g value of 2.004 (considered to be fluorine vacancies) gradually increase, which indicates that the longer the MAF is sealed and stored in water, the greater the concentration of defect vacancies in the material. From Figure cd, it can be seen that with the increase of fluorine vacancy concentration, the characteristic adsorption peaks in the X-ray photoelectron spectroscopy (XPS) of Mg1s and Al2s in the material shift to lower binding energy. This is because fluorine vacancies, as positively charged centers, change the chemical environment of the material elements. From Figure ef, it can be seen that although MAF-1, MAF-2 and MAF-3 have different defect concentrations, their crystal structures are the same, and a series of characteristic peaks of their XRD still coincide with the PDF standard card of MgAlF5·1.5H2O, but with the increase of defect concentration, the 101 peak of the material shifts. This is because the high concentration of defects causes lattice distortion, thereby increasing the (101) plane spacing.
[0068] 5. Figure 5 Figure 1 is a diagram of the mechanism of action of the rod-shaped magnesium aluminum fluoride nanocrystals in the present invention in a PEO-based polymer electrolyte calculated by first principle (DFT) simulation; Figure a is a configuration diagram of magnesium aluminum fluoride nanocrystals with a fluorine vacancy (denoted as MAF) and magnesium aluminum fluoride nanocrystals without fluorine vacancies (denoted as MAF(Ideal)), b is the adsorption of PEO on MAF and MAF(Ideal) configurations, c is the adsorption of lithium salt LiTFSI on PEO, MAF and MAF(Ideal), d is the adsorption of Li + and the calculated results of adsorption energy (Eb) of LiTFSI on PEO, MAF and MAF-FV configurations;
[0069] As shown in Figure a, in order to explore the role of fluorine vacancies in MAF, the configurations of magnesium aluminum fluoride nanocrystals with one fluorine vacancy (denoted as MAF) and magnesium aluminum fluoride nanocrystals without fluorine vacancies (denoted as MAF(Ideal)) were constructed for computational simulation; Figure b shows the interaction between MAF and MAF(Ideal) and PEO. The F in MAF(Ideal) is close to the H in the PEO chain to form an HF bond, and its binding energy (Eb) is -1.79eV; PEO not only forms an HF bond on the surface of MAF, but also forms an OH bond between the O of PEO and the H on the surface of MAF, so the binding energy between PEO and MAF is -2.42eV. This result shows that MAF containing fluorine vacancies has a stronger interaction with PEO, thus forming a more firmly bonded polymer-filler interface. Figure c simulates the adsorption of LiTFSI on the surfaces of PEO, MAF (Ideal) and MAF. The Li atom in LiTFSI is close to the oxygen atom in PEO, which leads to the formation of Li-O bond with a binding energy of -1.2 eV. LiTFSI forms a Li-F bond on MAF (Ideal) with a binding energy of -2.19 eV. LiTFSI not only forms a Li-F bond on MAF, but the Al atom in MAF also attracts the O atom on the anion in LiTFSI to form an Al-O bond. The binding energy between LiTFSI and MAF is -2.42 eV. + The calculated results of the binding energy adsorbed on the surfaces of PEO, MAF (Ideal) and MAF are shown in Figure d. MAF has the strongest binding energy (Li-F) with LiTFSI, which means that MAF with fluorine vacancies is more conducive to the dissociation of lithium salt LiTFSI. The binding energy (Li-O) between PEO and LiTFSI is the lowest, which is not conducive to the dissociation of lithium salt. At the same time, MAF shows a weaker binding energy with Li than MAF (Ideal). + The binding energy of the lithium ions is therefore more conducive to the rapid migration of lithium ions. Figure 5 It can be seen that the fluorine vacancies in MAF enhance the interaction between MAF and PEO as well as LiTFSI, while reducing the interaction between MAF and Li + The combined Li-F bond strength enables high lithium salt dissociation and fast lithium ion transport.
[0070] 6. Figure 6The present invention is comparative example 1, and the samples of embodiment 2 and comparative example 2 are applied to the performance comparison analysis of PEO-based all-solid polymer electrolyte according to application example 1 (the polymer membrane without filler is recorded as SPE-0, and the polymer membranes with MAF-1, MAF-2 and MAF-3 are recorded as SPE-MAF-1, SPE-MAF-2 and SPE-MAF-3 respectively); wherein a is the ionic conductivity bar graph of the polymer membrane at 50° C., b is the DSC graph of the polymer membrane, c is the lithium ion migration number of the polymer membrane at 50° C., d is the XRD graph of the polymer membrane, e is the voltage stability window graph of the polymer membrane at 50° C., and f is the thermogravimetric graph of the polymer membrane;
[0071] It can be seen from Figure a that SPE-MAF-2 has the highest ionic conductivity, which is 0.50 mS cm -1 , is SPE-MAF-1 (0.25 mS cm -1 ) is twice as high as SPE-0 (0.11 mS cm -1 ), which shows that the addition of MAF filler improves the ionic conduction of the polymer membrane. This is because the introduction of MAF destroys the ordered arrangement of the polymer chains, resulting in an increase in the amorphous region. With the increase of fluorine vacancies in MAF, the ionic conductivity of the polymer membrane first rises and then decreases. This is because the charged center caused by the vacancy defect can help improve the interaction between the filler and the lithium salt anion while reducing the Li-F bond strength between the filler and the lithium salt, which is beneficial to promote the dissociation of the lithium salt and produce more free electrolyte ions. However, with the increase of the vacancy concentration, the dissociation of the lithium salt will reach saturation, and too high a concentration of vacancy defects will lead to a strong interaction between the filler and the lithium salt anion, thereby limiting the transmission of the lithium salt anion and reducing the overall ionic conductivity. Figure b shows the lithium ion migration number (t Li+ ), SPE-MAF-2 (0.40) and SPE-MAF-3 (0.39) Li+It is significantly higher than SPE-MAF-1 (0.32) and SPE-0 (0.145). The addition of MAF increases the number of lithium ion migration. Vacancies are conducive to the dissociation of lithium salts, thereby increasing the number of lithium ion migration. However, since lithium ions mainly rely on their hopping transport on the PEO chain, when the lithium ions produced by the dissociation of lithium salts reach saturation, it will not bring a higher number of lithium ion transfers because the free movement of the chain is not enhanced. As shown in Figure c, the voltage stability window of SPE-MAF-2 is as high as 4.6V, and it has the minimum current response, while SPE-0, SPE-MAF-1 and SPE-MAF-3 have a larger current response, and their voltage stability windows are 4.1, 4.4, and 4.4V, respectively, indicating that SPE-MAF-2 has the best electrochemical stability. The change in the voltage stability window is due to the fact that the fluorine in MAF acts as an anchor point for hydrogen bonds in PEO, which changes the electron cloud density of the -OH group in PEO, thereby reducing its reactivity, improving the antioxidant capacity of PEO, and improving the voltage stability window. Fluorine vacancies change the electron cloud density of atoms in MAF, which can enhance the hydrogen bonds between PEO and MAF and further improve the antioxidant capacity of PEO. However, high concentrations of fluorine vacancies may lead to the formation of weak bonds in the polymer, thereby reducing the voltage stability window of the polymer film. As shown in Figure d, the glass transition temperatures (Tg) of SPE-0, SPE-MAF-1, SPE-MAF-2 and SPE-MAF-3 are -45.4℃, -53.3℃, -53.7℃ and -53.5℃, respectively, which indicates that the addition of MAF with surface defects destroys the orderly arrangement of polymer chains, leading to an increase in amorphous regions, thereby reducing the crystallinity of the polymer film and helping to improve the ionic conductivity of the polymer electrolyte membrane. Figure e also proves that after the introduction of MAF filler, the (120) and (112) adsorption peaks in the XRD pattern of the polymer film move to lower angles and the peak intensity weakens. This is due to the interaction between MAF and PEO chains, which leads to an increase in the plane spacing and a decrease in crystallinity. Figure f shows the thermogravimetric results of the polymer membranes. At about 200°C, all polymer membranes have a weight loss of about 3wt.%, which comes from the water adsorbed by the polymer membranes when exposed to air. The weight loss of 65wt.% in the polymer membrane at 250-350°C corresponds to the mass ratio of PEO in the polymer membrane. It can be clearly seen that the decomposition temperature of PEO decreases. The main reason for the decrease in the decomposition temperature of PEO is the strong interaction between MAF and PEO. The weight loss after 336°C corresponds to the decomposition of LiTFSI. The decomposition temperature of LiTFSI in SPE-MAF-1 is higher than that of SPE-MAF-2 and SPE-MAF-3. This is because the increase in fluorine vacancies enhances the interaction between MAF and LiTFSI, resulting in a decrease in the decomposition temperature of LiTFSI.Finally, 5 wt.% of the remaining weight in SPE-0 comes from the mass of lithium oxide produced after the thermal decomposition of LiTFSI, while 10 wt.% of the remaining weight in SPE-MAF-1, SPE-MAF-2, and SPE-MAF-3 is composed of fillers and lithium oxide. Figure 6 It can be seen that adding MAF to polymer electrolyte can improve the performance of polymer electrolyte, and MAF-2 with moderate fluorine vacancy concentration can obtain the highest ionic conductivity, lithium ion migration number and voltage stability window. This is because the increase of fluorine vacancies can enhance the interaction between filler and lithium salt, filler and polymer, and reduce the interaction between filler and Li + The interaction between them is conducive to the dissociation of lithium salts and the hopping transport of lithium ions, but too high a concentration of fluorine vacancies will lead to a strong interaction between the filler and the polymer, which will reduce the oxidation resistance of the polymer and reduce its voltage stability window.
[0072] 7. Figure 7 The performance analysis of MAF-2 of Example 2 of the present invention applied to PEO-based all-solid polymer electrolyte according to Application Example 1 (the polymer membrane without filler is marked as SPE-0, and the polymer membrane with MAF-2 added is marked as SPE-MAF-2); wherein ab is the SEM image of the polymer membrane, c is the stress-strain image of the polymer membrane, d is the nanoindentation image of the polymer membrane, and e is the SEM image of the polymer membrane at 730-755cm -1 Raman spectra in the wavenumber range of , e is the constant current lithium plating / stripping electrochemical cycle, f is the rate cycle, and g is the long cycle diagram at 1C;
[0073] As can be seen from Figures ab, the SPE-0 membrane has obvious PEO spherulites, and there are obvious gaps between the spherulites. When MAF-2 is added, the size of the spherulites in the SPE-MAF-2 membrane is reduced and the gaps are filled, confirming that the addition of MAF-2 affects the crystallinity of PEO. As can be seen from Figure c, the elastic modulus and maximum tensile strength of the SPE-MAF-2 membrane are 1.97 and 26.4 MPa, respectively, which are 3.6 and 5.8 times that of the polymer membrane without filler (SPE-0), respectively. Its elongation at break (~1614%) is also much higher than that of the polymer membrane without filler (~718%). The improvement in mechanical properties is due to the strong bonding between the filler and the polymer, which makes MAF-2 play a good buffering role for stress. As can be seen from Figure d, the compression modulus of the SPE-MAF-2 membrane increased from 40 MPa to 347 MPa, indicating that the SPE-MAF-2 membrane has a higher resistance to lithium dendrite growth. As shown in Figure e, for the polymer membrane at 730-755 cm -1The Raman peak fitting calculation at 100 nm shows that the lithium salt dissociation degree of SPE-0 is 77%, while that of SPE-MAF-2 is increased to 95%. As shown in Figure f, the polymer membrane is matched with LiFePO4 to assemble lithium metal batteries. At 0.2C, 0.5C, 1C and 2C, the average discharge capacity of the battery assembled by SPE-MAF-2 is 166.97 mAh g -1 、161.07mAh g -1 、147.2mAhg -1 and 117.3mAh g -1 , even at high current densities of 5C and 10C, the battery can still charge and discharge normally, while the battery assembled with SPE-0 fails at 10C and cannot be charged and discharged normally. As shown in Figure g, at 0.1 mA cm -2 At a current density of 1.5 200 s, the lithium symmetric battery assembled with SPE-0 showed a short circuit after only 280 hours, while the lithium symmetric battery assembled with SPE-MAF-2 showed a lower overpotential and the cycle life was extended to about 1400 hours without obvious short circuit. This shows that the SPE-MAF-2 membrane can achieve highly reversible lithium plating / stripping compared to the SPE-0 membrane. As shown in Figure h, under 1C conditions, the LiFePO4 battery assembled with SPE-MAF-2 provides 160.1 mAh g -1 High discharge capacity, maintaining 100.2 mAh g after 1000 cycles -1 , with good cycle stability. However, the LiFePO4 battery assembled with SPE-0 was overcharged after more than 70 cycles. As the cycle continued, the battery returned to normal, but it was overcharged again after the 650th cycle and the battery failed. Figure 7 It can be seen that adding MAF-2 with an appropriate fluorine vacancy concentration to the polymer electrolyte can significantly reduce the crystallinity of the polymer membrane and significantly improve the mechanical strength, lithium salt dissociation degree and charge and discharge cycle performance of the polymer membrane.
[0074] 8. Figure 8 The performance comparison analysis of the samples of Comparative Example 1 and Example 2 added to the PEO / PVDF-HFP blended composite membrane according to Application Example 2 (the PEO / PVDF-HFP blended composite membrane without adding filler is recorded as CPE, and the PEO / PVDF-HFP blended composite membranes with adding MAF-1 and MAF-2 are recorded as CPE-MAF-1 and CPE-MAF-2 respectively). Wherein, ac is the SEM images of CPE, CPE-MAF-1 and CPE-MAF-2 membranes, d is the XRD image of the membrane, and e is the infrared spectrum of the membrane;
[0075] As can be seen from Figure ac, the CPE blended composite film without filler in Figure a has obvious discrete protruding grains, which is due to the PEO spherulites with high crystallinity, and its microscopic surface is a rough surface with many tiny pores. This is because PEO and PVDF-HFP are thermodynamically incompatible systems, and phase separation occurs between PEO and PVDF-HFP. As can be seen from Figure bc, the CPE-MAF-1 film introduced with MAF-1 has a smooth surface morphology and no obvious filler agglomeration, while the surface of the CPE-MAF-2 film with MAF-2 with a higher defect concentration as filler is corrugated in the macroscopic morphology and has uniform linear protrusions, but is still smooth in the microscopic. This change in surface morphology is due to the fact that MAF, as an inorganic filler, interacts with the surfaces of the two polymer components, plays a compatibilizer role, forms an interpenetrating polymer network, enhances the interfacial bonding between the components, improves the segmental motion of the polymer, hinders the phase separation of the system, and eliminates phase agglomeration. As shown in Figure d, it can be seen from the XRD graph that there is an obvious PEO crystallization peak in the CPE film, while the PEO crystallization peak in the CPE-MAF-1 film is very weak, and there is almost no PEO crystallization peak in CPE-MAF-2, which indicates that the PEO crystallinity decreases after the introduction of MAF. As shown in Figure e, compared with CPE, CPE-MAF-1 and CPE-MAF-2 have a higher PEO crystallinity at 2880 cm -1 and 1463cm -1 The symmetrical stretching vibration and bending vibration peaks corresponding to CH2 at 1096cm - 1 and 842cm -1 The symmetrical stretching peak and deformation vibration peak of COC at 1723 cm-1 were also weakened. The weakening of these vibration peaks about PEO may be due to the weakening of the interchain force due to the formation of hydrogen bonds and the loss of PEO crystallinity after the addition of MAF. In addition, the membranes of CPE-MAF-1 and CPE-MAF-2 showed a decrease in the peaks at 1723 cm-1. -1 A C=O double bond is generated at the CPE film, which is not present in the CPE film. This is due to the interaction between MAF, PEO, and PVDF-HFP. Figure 8 It can be seen that the introduced MAF filler plays the role of a compatibilizer. MAF acts as an intermediate bridge to connect PEO and PVDF-HFP, promoting the blending and cross-linking between the polymer matrices, while the vacancies further enhance the compatibilization effect of MAF filler on PEO and PVDF-HFP.
[0076] 9. Fig. 9The invention discloses a comparative analysis of the electrochemical properties of a blended gel polymer electrolyte formed after CPE, CPE-MAF-1 and CPE-MAF-2 blended composite membranes are soaked in (DOL / DME (1:1, v / v) 1M LiTFSI) electrolyte (CPE, CPE-MAF-1 and CPE-MAF-2 are respectively recorded as GPE, GPE-MAF-1 and GPE-MAF-2 after being soaked in electrolyte); wherein a is a histogram of electrolyte absorption rate, b is a Tafel curve graph, c is an ionic conductivity graph, and d is a long cycle graph at 1C;
[0077] As can be seen from Figure a, the absorption capacity of the polymer membrane for liquid electrolyte (DOL / DME (1:1, v / v) 1M LiTFSI) is 227% for the CPE membrane without filler, and 78.5% and 75.4% for the membrane containing MAF-1 and MAF-2, respectively. This is mainly attributed to the large number of tiny pores in the CPE membrane due to phase separation, which provides conditions for electrolyte adsorption. The interaction between MAF and PEO and PVDF-HFP promotes the cross-linking of PEO and PVDF-HFP, forming a closer connection interface between the three materials, with low micro-porosity, so its electrolyte absorption rate is lower. As shown in Figure b, the volume resistance of GPE, GEP-MAF-1 and GEP-MAF-2 membranes are 2.85Ω, 2.41Ω, and 1.69Ω, respectively, and the corresponding ionic conductivity is 2.19×10 -3 S cm -1 , 2.34×10 -3 S cm -1 and 3.34×10 -3 S cm -1 , the highest ionic conductivity of GPE-MAF-2 is due to the lowest crystallinity of PEO in the membrane. Ions can be transported not only through the adsorbed electrolyte, but also through the amorphous region of PEO. As shown in Figure c, the interface resistances of GPE, GEP-MAF-1 and GEP-MAF-2 with metallic lithium are 106Ω, 76Ω, and 67Ω, respectively, indicating that GPE with MAF-1 and MAF-2 as fillers has better interfacial compatibility with metallic lithium sheets. Figure d is the Tafel curve of a lithium symmetric battery assembled with a gel polymer electrolyte membrane. The exchange currents of GPE, GEP-MAF-1 and GEP-MAF-2 are 99.4μA, 170.6μA and 195.1μA, respectively, showing that GPE-MAF-2 has faster Li at the lithium / gel polymer electrolyte membrane interface. + The introduction of MAF reduces the crystallinity of PEO and inhibits phase separation, so the gel polymer electrolyte has a large ionic conductivity and fast Li transport kinetics at the interface. +As shown in Figure e, the initial discharge capacities of LiFePO4 batteries assembled with GPE, GEP-MAF-1, and GEP-MAF-2 under 1C conditions are comparable, which are 158.1 mAh g -1 、157.3mAh g -1 、157.6mAh g -1 After 800 cycles of charge and discharge, the discharge capacity showed obvious differences. The discharge specific capacities of GPE, GEP-MAF-1 and GEP-MAF-2 were 32.86 mAh g -1 、70.23mAh g -1 、93.1mAh g -1 , GEP-MAF-2 has a stable charge-discharge long cycle. Fig. 9 It can be seen that MAF, as an inorganic filler, interacts with the surfaces of the two polymer components, improves the chain segment movement of the polymer, plays the role of a compatibilizer, enhances the compatibility between PEO and PVDF-HFP, hinders the phase separation of the system, and eliminates phase agglomeration, thereby achieving a stable and long cycle of the PEO / PVDF-HFP blended gel polymer electrolyte.
[0078] The present applicant also conducted a study on the defect-rich magnesium aluminum fluoride nanocrystals MgAlF 5· 1.5H2O(MAF) was subjected to the experimental tests and analyses described in 3-9 above, and the results obtained were comparable to those of the above tests and analyses.
Claims
1. A method for preparing defect-rich magnesium aluminum fluoride nanocrystals, characterized in that: The following steps are involved: (1) Add 10-20 g of vermiculite to 400-500 mL of deionized water, stir in an oil bath at 50-70° C. for 8-12 h, let stand for 0.5-1.5 h, remove the impurities floating on the upper layer and the vermiculite that has not been dispersed and peeled off at the bottom layer, filter by suction, and dry at 50-70° C. for 15-30 h to obtain product A; (2) Add 6-10 g of product A to 300-500 mL of deionized water, stir and disperse, add 30-50 mL of 30-40% hydrofluoric acid, stir in an oil bath at 40-80° C. for 6-10 h, vacuum filter, wash with deionized water until the pH of the deionized water is 6.5-7, and obtain rod-shaped magnesium aluminum fluoride nanocrystals, which are product B; (3) Add 1-3 g of product B into 400-800 mL of deionized water, stir and disperse at 200-1000 rad / min for 10-50 min, seal and store at 15-35° C. for 5-15 days, and freeze-dry at -60--40° C. for 20-28 h to obtain defect-rich magnesium aluminum fluoride nanocrystals, denoted as MgAlF 5· 1.5H2O.
2. The method for preparing defect-rich magnesium aluminum fluoride nanocrystals according to claim 1, characterized in that: The vermiculite is thermally expanded vermiculite clay containing magnesium / aluminum oxide octahedrons.
3. The method for preparing defect-rich magnesium aluminum fluoride nanocrystals according to claim 1, characterized in that: In the step (1), 15 g of vermiculite was added to 450 mL of deionized water, stirred in an oil bath at 60° C. for 10 h, allowed to stand for 1 h, impurities floating on the upper layer and undispersed vermiculite on the bottom layer were removed, filtered, and dried at 60° C. for 24 h to obtain product A.
4. The method for preparing defect-rich magnesium aluminum fluoride nanocrystals according to claim 1, characterized in that: In the step (2), 8 g of product A is stirred and dispersed in 400 mL of deionized water, 40 mL of 35% hydrofluoric acid is added, and the mixture is stirred in an oil bath at 60° C. for 8 h, vacuum filtered, and washed with deionized water until the pH of the deionized water is 6.8-7 to obtain rod-shaped magnesium aluminum fluoride nanocrystals, which are product B.
5. The method for preparing defect-rich magnesium aluminum fluoride nanocrystals according to claim 1, characterized in that: In the step (3), 2 g of product B is added to 600 mL of deionized water, stirred and dispersed at 500 rad / min for 30 min, sealed and stored at 25° C. for 10 days, and freeze-dried at -50° C. for 24 h to obtain defect-rich magnesium aluminum fluoride nanocrystals.
6. The use of defect-rich magnesium aluminum fluoride nanocrystals according to any one of claims 1 to 5, characterized in that: The defect-rich magnesium aluminum fluoride nanocrystals are added to a polymer electrolyte as a filler.
7. The use of defect-rich magnesium aluminum fluoride nanocrystals according to claim 6, characterized in that: Specifically, the defect-rich magnesium aluminum fluoride nanocrystals are vacuum dried at 80-120° C. for 20-28 hours, added into a polymer electrolyte, ultrasonically dispersed, and sealed and stirred.
8. The use of defect-rich magnesium aluminum fluoride nanocrystals according to claim 6, characterized in that: The polymer electrolyte is a PEO-based all-solid polymer electrolyte or a PEO / PVDF-HFP blended gel polymer electrolyte.