Preparation method of thorium hydroxide concentrate

By adjusting the pH value in concentrated sulfuric acid rare earth roasted ore water soaking liquid, using ammonia water and magnesium oxide to achieve solid-liquid separation, the problem of solid-liquid separation is not easy to filtration, and the recovery efficiency of thorium element and the purity of the product are improved.

CN118929729APending Publication Date: 2024-11-12CHINA NORTHERN RARE EARTH (GROUP) HIGH TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411064821.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, when recovering thorium from concentrated sulfuric acid rare earth roasted ore, solid-liquid separation is not easy to filter, resulting in low production efficiency and low thorium content.

Method used

By adjusting the pH value of the water infusion liquid of concentrated sulfuric acid rare earth concentrate roasted ore with ammonia water to 2.0-2.5, and then adjusting the pH value to 4.5-5.3 with magnesium oxide, solid-liquid separation is achieved, and thorium hydroxide-rich that is easy to settle and filter Collection.

Benefits of technology

The production efficiency is improved, the thorium content of the thorium hydroxide-enriched substance is increased, and the entrainment of rare earth elements is reduced. The solid product obtained is granular and easy to filter.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004979044700000091
    Figure BDA0004979044700000091
Patent Text Reader

Abstract

The invention discloses a preparation method of thorium hydroxide concentrate, which comprises the following steps: 1) adjusting the pH value of water leaching liquid of concentrated sulfuric acid rare earth concentrate roasted ore to 2.0-2.5 by using ammonia water, and carrying out solid-liquid separation to obtain first mother liquor; and 2) adjusting the pH value of the first mother liquor to 4.5-5.3 by using magnesium oxide, and carrying out solid-liquid separation to obtain a solid, namely the thorium hydroxide enriched product. According to the preparation method disclosed by the invention, during solid-liquid separation, solids are easy to settle or filter, and the production efficiency can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a thorium hydroxide enriched product. Background Art

[0002] Thorium (Th) is a radioactive metal element. Thorium can be used to make alloys to increase the strength of metals. Thorium is also a common raw material for making advanced lenses. The energy stored in thorium decay is more than the sum of uranium, coal, oil and other fuels, and the thorium content is also higher than uranium, so thorium is a very promising material. Thorium can be bombarded with neutrons to obtain a nuclear fuel uranium-233. In addition, thorium is also a safer nuclear fuel than uranium.

[0003] Thorium generally exists in the form of compounds in minerals (such as monazite and thorite), usually mixed with rare earth metals. In the earth's crust, the average thorium content is twice that of uranium and is comparable to that of lead, cobalt, and bismuth. Its distribution is quite extensive, with more than 100 minerals, the most important of which are: (1) Phosphates: monazite (phosphates of cerium, other rare earths, and thorium, with a thorium content of about 4-6%); yttrium phosphate (phosphates of yttrium and other rare earths; containing a small amount of thorium); mixed rare earth ores (fluorocarbon cerium, monazite). (2) Oxides: thorite (thorium oxide, uranium oxide and a small amount of rare earths, with a ThO2 content of up to 40-90%). (3) Silicates: thorite (thorium oxide, silicon oxide, with a thorium content of up to 62%). The latter two minerals contain high thorium content, but these ores are very rare.

[0004] Rare earth ores are mainly processed by concentrated sulfuric acid roasting. Therefore, how to better recover thorium from concentrated sulfuric acid rare earth roasted ores is a problem that needs to be considered.

[0005] CN1721559A discloses a process for comprehensive recovery of rare earth and thorium from rare earth ores, comprising: mixing a mixed rare earth concentrate (a mixture of bastnaesite and monazite) or monazite rare earth ore with concentrated sulfuric acid and an iron-containing additive, and then roasting under appropriate conditions to make rare earth, thorium and some valuable elements such as iron and phosphorus form substances soluble in water or dilute acid solution; leaching the roasted ore with water or dilute acid and then directly filtering to obtain low-radioactive slag and water extract; neutralizing and filtering the water extract to enrich thorium, iron, phosphorus, etc. in the slag. The obtained iron-phosphorus-thorium slag is dissolved with an inorganic acid to obtain an iron-phosphorus-thorium solution, and then the thorium is extracted and recovered.

[0006] CN106978532A discloses a method for extracting rare earth, fluorine and thorium from fluorine-containing rare earth minerals with concentrated sulfuric acid, comprising: mixing fluorine-containing rare earth minerals with concentrated sulfuric acid; the mass percentage of rare earth oxides contained in a single fluorine-containing rare earth mineral or a mixed rare earth concentrate is 50-70%, the mass percentage of H2SO4 in the concentrated sulfuric acid is greater than 90%, and the weight ratio of the fluorine-containing rare earth mineral to the concentrated sulfuric acid is 1:0.6-1.0; the mixture is calcined at 120-180°C for 120-300 minutes; the reaction product after calcination is soaked in water, and the water soaking liquid is neutralized to a pH value of 3.5-4.5 to form a rare earth sulfate solution and an iron-thorium enriched product.

[0007] CN106978531A discloses a method for acid-base combined decomposition of mixed rare earth concentrate, comprising: mixing the mixed rare earth concentrate with concentrated sulfuric acid with a mass percentage of more than 92% in proportion, roasting and decomposing the mixture at 120-180°C for 150-300 minutes; neutralizing the water extract to form phosphorus-iron-thorium slag and rare earth sulfate solution; decomposing phosphorus-containing minerals and phosphorus-iron-thorium slag with sodium hydroxide solution with a mass percentage of 45%-70% at 130-180°C according to a weight ratio of mixed concentrate to sodium hydroxide of 1:0.1-0.2; washing the alkaline hydrolyzed ore, dissolving it with hydrochloric acid, neutralizing and removing impurities to form acid slag, iron-thorium slag and rare earth chloride solution.

[0008] In the above documents, the water extract of the roasted ore is directly neutralized to form an iron-thorium slag product, which is not easy to filter and has a low thorium content.

[0009] CN1667139A discloses a method for separating rare earth and thorium by decomposing a mixed rare earth concentrate, comprising: (1) mixing the rare earth concentrate with concentrated sulfuric acid; (2) aging the concentrate after mixing with sulfuric acid; (3) roasting the aging concentrate; (4) leaching the roasted ore produced by roasting with water, so that more than 95% of the rare earth and thorium are leached into the solution; then extracting and separating thorium and rare earth, washing and stripping to obtain a thorium nitrate product. The document mentions the use of direct extraction to separate thorium and rare earth, but the direct extraction method uses more extractants and has low efficiency. Summary of the invention

[0010] In view of this, the object of the present invention is to provide a method for preparing a thorium hydroxide enriched product, in which the solid is easy to settle and filter during solid-liquid separation, thereby improving production efficiency.

[0011] The present invention adopts the following technical solutions to achieve the above-mentioned purpose.

[0012] The present invention provides a method for preparing a thorium hydroxide enriched product, comprising the following steps:

[0013] 1) adjusting the pH value of the water infusion of concentrated sulfuric acid rare earth concentrate roasted ore to 2.0-2.5 with aqueous ammonia, and performing solid-liquid separation to obtain a first mother liquor;

[0014] 2) The pH value of the first mother liquor is adjusted to 4.5-5.3 with magnesium oxide, and the solid-liquid separation is performed to obtain a solid, which is a thorium hydroxide enriched product.

[0015] According to the preparation method of the present invention, preferably, in step 1), the concentrated sulfuric acid rare earth concentrate roasted ore is prepared by the following steps: 1 part by weight of rare earth concentrate and 1.2 to 1.5 parts by weight of concentrated sulfuric acid are roasted at 180 to 300° C. for 1.5 to 4 hours to obtain concentrated sulfuric acid rare earth concentrate roasted ore.

[0016] According to the preparation method of the present invention, preferably, the rare earth concentrate is selected from at least one of a mixed rare earth concentrate, monazite ore, and yttrium phosphate ore; the REO content in the rare earth concentrate is 30-68wt%, and the ThO2 content is greater than or equal to 0.05wt%.

[0017] According to the preparation method of the present invention, preferably, the concentration of H2SO4 in concentrated sulfuric acid is 80-98wt%; and the weight ratio of rare earth concentrate to concentrated sulfuric acid is 1:1.3-1.5.

[0018] According to the preparation method of the present invention, preferably, the calcination temperature is 200-300° C. and the calcination time is 2-3 h.

[0019] According to the preparation method of the present invention, preferably, step 1) also includes the following steps: leaching the concentrated sulfuric acid rare earth concentrate roasted ore with water to obtain a water extract of the concentrated sulfuric acid rare earth concentrate roasted ore; wherein the solid-liquid ratio is 1:5-10; and the leaching temperature is 10-50°C.

[0020] According to the preparation method of the present invention, preferably, in step 1), the pH value is adjusted to 2.2-2.5 with aqueous ammonia.

[0021] According to the preparation method of the present invention, preferably, in step 1), the concentration of aqueous ammonia is 5-20 wt %.

[0022] According to the preparation method of the present invention, preferably, in step 2), the pH value of the first mother liquor is adjusted to 4.7-5.3 with magnesium oxide.

[0023] According to the preparation method of the present invention, preferably, in step 2), the pH value of the first mother liquor is adjusted to 4.5-5.3 with magnesium oxide powder, and solid-liquid separation is performed to obtain thorium hydroxide enriched solid and rare earth sulfate solution.

[0024] The thorium hydroxide concentrate of the present invention is basically in granular form, easy to settle and filter, and can improve production efficiency. In addition, the preparation method of the present invention is not easy to carry rare earth elements, and the thorium content of the obtained thorium hydroxide concentrate is higher and the rare earth content is lower. DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0026] The method for preparing the thorium hydroxide concentrate of the present invention comprises the following steps: (1) an ammonia water adjustment step; (2) a magnesium oxide adjustment step. In certain embodiments, the method further comprises a rare earth concentrate roasting step and a water leaching step. The method is described in detail below.

[0027] <Steps of roasting rare earth concentrate>

[0028] In the present invention, the concentrated sulfuric acid rare earth concentrate roasted ore is obtained by mixing rare earth concentrate and concentrated sulfuric acid and then roasting. Specifically, the method comprises the following steps: roasting 1 part by weight of rare earth concentrate with 1.2 to 1.5 parts by weight of concentrated sulfuric acid at 180 to 300° C. for 1.5 to 4 hours to obtain concentrated sulfuric acid rare earth concentrate roasted ore. This is conducive to improving the decomposition rate of the rare earth concentrate, thereby facilitating the subsequent improvement of the leaching rate of thorium and rare earth elements.

[0029] In the present invention, the rare earth concentrate is selected from at least one of mixed rare earth concentrate, monazite ore and yttrium phosphate ore, preferably selected from at least one of mixed rare earth concentrate and monazite ore, and more preferably is a mixed rare earth concentrate.

[0030] The REO content in the rare earth concentrate is 30-68wt%, preferably 35-65wt%, more preferably 40-65wt%. The ThO2 content in the rare earth concentrate is greater than or equal to 0.05wt%, preferably greater than or equal to 0.1wt%, more preferably greater than or equal to 0.15wt% and less than 15wt%.

[0031] The weight ratio of rare earth concentrate to concentrated sulfuric acid can be 1:1.2-1.5, preferably 1:1.25-1.5, and more preferably 1:1.3-1.4. The concentration of H2SO4 in concentrated sulfuric acid can be 80-98wt%, preferably 85-98wt%, more preferably 90-98wt%, and even more preferably 92-98wt%. Such concentrated sulfuric acid and weight ratio are conducive to the subsequent process of separating thorium and rare earth elements, and increasing the thorium content in the enriched product.

[0032] In the present invention, the roasting temperature can be 180-300°C, preferably 200-300°C, and more preferably 220-280°C. The roasting time can be 1.5-4h, preferably 2-4h, and more preferably 2-3h. Such roasting conditions are conducive to the subsequent process of separating thorium and rare earth elements, and increasing the thorium content in the enriched product.

[0033] <Water leaching step>

[0034] The concentrated sulfuric acid rare earth concentrate roasted ore is leached with water to obtain a water leaching solution of the concentrated sulfuric acid rare earth concentrate roasted ore, so that valuable elements such as thorium can be leached.

[0035] In the present invention, when leaching with water, the solid-liquid ratio can be 1:5-10, preferably 1:6-10, and more preferably 1:7-10. The temperature during leaching can be 10-50°C, preferably 15-40°C, and more preferably 20-30°C. For example, leaching can be performed at room temperature. The leaching time can be 1.5-5h, preferably 2-4h, and more preferably 2-3h. This is conducive to improving the leaching rate of valuable elements.

[0036] According to one embodiment of the present invention, the rare earth concentrate is a mixed rare earth concentrate, and concentrated sulfuric acid rare earth concentrate roasted ore is leached with water and filtered to obtain a water leaching solution and leaching residue. The leaching residue is mainly calcium sulfate. The water leaching solution is an aqueous solution containing thorium and rare earth elements.

[0037] <Ammonia Adjustment Step>

[0038] The pH value of the water infusion of the concentrated sulfuric acid rare earth concentrate roasted ore is adjusted to 2.0-2.5 with ammonia water, and the solid-liquid separation is performed to obtain a first mother liquor. The present invention unexpectedly found that by first adjusting the water infusion to a specific pH value with ammonia water, and then adjusting the first mother liquor to a specific pH value with magnesium oxide after separation, the solid produced when the pH is adjusted is not viscous, but is basically granular, easy to settle or filter, and the production efficiency can be improved, and the obtained thorium hydroxide enriched solid is not easy to carry rare earth elements.

[0039] In the present invention, the concentration of aqueous ammonia is 5-20wt%, preferably 8-18wt%, more preferably 10-18wt%. For example, it can be 5wt%, 10wt%, 15wt%, 17.8wt%. In some preferred embodiments, the pH value of the water immersion liquid is adjusted to 2.2-2.5 with aqueous ammonia, and the solid-liquid separation is performed to obtain the first mother liquor.

[0040] <Magnesium oxide adjustment step>

[0041] The pH value of the first mother liquor is adjusted to 4.5-5.3 with magnesium oxide, and the solid-liquid separation is performed to obtain a solid, which is a thorium hydroxide enriched product. In this way, the solid product is easy to settle and filter, and the obtained thorium hydroxide enriched product solid is not easy to carry rare earth elements. The present invention finds that compared with continuing to adjust the pH value with ammonia water, continuing to adjust the pH value of the first mother liquor with magnesium oxide can better separate thorium and rare earth elements, and obtain a solid product that is easy to filter.

[0042] In the present invention, magnesium oxide powder is preferably used to adjust the pH value of the first mother solution.

[0043] In certain preferred embodiments, the pH value of the first mother liquor is adjusted to 4.7-5.3 with magnesium oxide.

[0044] According to one embodiment of the present invention, the pH value of the first mother liquor is adjusted to 4.5-5.3 with magnesium oxide, and solid-liquid separation is performed to obtain thorium hydroxide enriched solid and rare earth sulfate solution.

[0045] In the present invention, the obtained thorium hydroxide enriched solid can be further purified by conventional methods to extract thorium element. The obtained rare earth sulfate solution can be converted into rare earth carbonate or rare earth chloride solution as needed. No further details are given here.

[0046] The test methods used in the following examples are described below:

[0047] REO content: measured by oxalic acid weight method.

[0048] ThO2 content: determined by spectrophotometry.

[0049] Example 1

[0050] 1000g of mixed rare earth concentrate (REO content of 58.42wt%, ThO2 content of 0.216wt%) was stirred and mixed with 1300g of 98wt% concentrated sulfuric acid, and roasted at 280°C for 2h to obtain concentrated sulfuric acid rare earth concentrate roasted ore. The concentrated sulfuric acid rare earth concentrate roasted ore was leached with water at a solid-liquid ratio of 1:10, and filtered to obtain a water leaching solution and leaching residue.

[0051] The water extract was adjusted to pH 2.3 with 15 wt% ammonia water under stirring, filtered to obtain the first mother liquor. The first mother liquor was adjusted to pH 4.5 with magnesium oxide powder under stirring, filtered to obtain thorium hydroxide enriched solid.

[0052] Example 2

[0053] 1000g of mixed rare earth concentrate (REO content of 56.55wt%, ThO2 content of 0.192wt%) was stirred and mixed with 1200g of 98wt% concentrated sulfuric acid, and roasted at 270°C for 2.5h to obtain concentrated sulfuric acid rare earth concentrate roasted ore. The concentrated sulfuric acid rare earth concentrate roasted ore was leached with water at a solid-liquid ratio of 1:10, and filtered to obtain a water leaching solution and leaching residue.

[0054] The water extract was adjusted to pH 2.2 with 10 wt% ammonia water under stirring, filtered to obtain the first mother liquor. The first mother liquor was adjusted to pH 5.0 with magnesium oxide powder under stirring, filtered to obtain thorium hydroxide enriched solid.

[0055] Example 3

[0056] 1000g of mixed rare earth concentrate (REO content of 62.35wt%, ThO2 content of 0.232wt%) was stirred and mixed with 1400g of 98wt% concentrated sulfuric acid, and roasted at 260°C for 3h to obtain concentrated sulfuric acid rare earth concentrate roasted ore. The concentrated sulfuric acid rare earth concentrate roasted ore was leached with water at a solid-liquid ratio of 1:10, and filtered to obtain a water leaching solution and leaching residue.

[0057] The water extract was adjusted to pH 2.5 with 5 wt% ammonia water under stirring, filtered to obtain the first mother liquor. The first mother liquor was adjusted to pH 5.3 with magnesium oxide powder under stirring, filtered to obtain thorium hydroxide enriched solid.

[0058] Example 4

[0059] 1000g of mixed rare earth concentrate (REO content of 56.55wt%, ThO2 content of 0.205wt%) was stirred and mixed with 1300g of 98wt% concentrated sulfuric acid, and roasted at 300°C for 2h to obtain concentrated sulfuric acid rare earth concentrate roasted ore. The concentrated sulfuric acid rare earth concentrate roasted ore was leached with water at a solid-liquid ratio of 1:10, and filtered to obtain a water leaching solution and leaching residue.

[0060] The water extract was adjusted to pH 2.2 with 17.8 wt% ammonia water under stirring, filtered to obtain the first mother liquor. The first mother liquor was adjusted to pH 5.3 with magnesium oxide powder under stirring, filtered to obtain thorium hydroxide enriched solid.

[0061] Comparative Example 1

[0062] The following configurations are the same as those in Example 1: The pH value of the aqueous solution is adjusted to 2.3 with magnesium oxide powder under stirring, and filtered to obtain a first mother solution. The pH value of the first mother solution is adjusted to 4.5 with magnesium oxide powder under stirring, and filtered to obtain a thorium hydroxide enriched product.

[0063] Comparative Example 2

[0064] The following configurations are the same as those in Example 1: the water extract is adjusted to a pH of 2.3 with 15 wt% ammonia water under stirring, filtered to obtain a first mother liquor. The first mother liquor is adjusted to a pH of 4.5 with 15 wt% ammonia water under stirring, filtered to obtain a thorium hydroxide enriched product.

[0065] Comparative Example 3

[0066] The following configurations are the same as those in Example 1: The water solution is adjusted to a pH value of 2.3 with magnesium oxide powder under stirring, filtered to obtain a first mother solution. The first mother solution is adjusted to a pH value of 4.5 with 15 wt% ammonia water under stirring, filtered to obtain a thorium hydroxide enriched product.

[0067] Comparative Example 4

[0068] The following configurations are the same as those in Example 1: the water extract is stirred and adjusted to a pH value of 3.5 with 15 wt% ammonia water, filtered to obtain a first mother liquor. The first mother liquor is stirred and adjusted to a pH value of 4.5 with magnesium oxide powder, filtered to obtain a thorium hydroxide enriched product.

[0069] Table 1

[0070]

[0071] Note: In Table 1, all magnesium oxides used are magnesium oxide powders. In Comparative Example 4, during the step of adjusting the pH value with ammonia water, the filter cake contained thorium, and it was not easy to filter. The contents of thorium and rare earth elements in the solid product of thorium hydroxide enrichment were calculated in the form of oxides.

[0072] As can be seen from Table 1, the present invention first uses ammonia water to adjust the water extract to a specific pH value, and then uses magnesium oxide powder to adjust the first mother liquor to a specific pH value. The obtained thorium hydroxide enriched solid product is easy to filter and has a high thorium content.

[0073] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A method for preparing a thorium hydroxide enrichment, characterized in that: The steps include: 1) adjusting the pH value of the water infusion of concentrated sulfuric acid rare earth concentrate roasted ore to 2.0-2.5 with aqueous ammonia, and performing solid-liquid separation to obtain a first mother liquor; 2) The pH value of the first mother liquor is adjusted to 4.5-5.3 with magnesium oxide, and the solid-liquid separation is performed to obtain a solid, which is a thorium hydroxide enriched product.

2. The preparation method according to claim 1, characterized in that: In step 1), the concentrated sulfuric acid rare earth concentrate roasted ore is prepared by the following steps: 1 part by weight of rare earth concentrate and 1.2 to 1.5 parts by weight of concentrated sulfuric acid are roasted at 180 to 300° C. for 1.5 to 4 hours to obtain concentrated sulfuric acid rare earth concentrate roasted ore.

3. The preparation method according to claim 2, characterized in that: The rare earth concentrate is selected from at least one of mixed rare earth concentrate, monazite ore, and yttrium phosphate ore; the REO content in the rare earth concentrate is 30-68wt%, and the ThO2 content is greater than or equal to 0.05wt%.

4. The preparation method according to claim 2, characterized in that: The concentration of H2SO4 in concentrated sulfuric acid is 80-98wt%; the weight ratio of rare earth concentrate to concentrated sulfuric acid is 1:1.3-1.

5.

5. The preparation method according to claim 2, characterized in that: The calcination temperature is 200-300°C and the calcination time is 2-3h.

6. The preparation method according to claim 2, characterized in that: Step 1) also includes the following steps: leaching the concentrated sulfuric acid rare earth concentrate roasted ore with water to obtain a water infusion of the concentrated sulfuric acid rare earth concentrate roasted ore; wherein the solid-liquid ratio is 1:5-10; and the leaching temperature is 10-50°C.

7. The preparation method according to claim 1, characterized in that: In step 1), the pH value is adjusted to 2.2-2.5 with aqueous ammonia.

8. The preparation method according to claim 1, characterized in that: In step 1), the concentration of aqueous ammonia is 5 to 20 wt%.

9. The preparation method according to claim 1, characterized in that: In step 2), the pH value of the first mother liquor is adjusted to 4.7-5.3 with magnesium oxide.

10. The preparation method according to any one of claims 1 to 8, characterized in that: In step 2), the pH value of the first mother liquor is adjusted to 4.5-5.3 with magnesium oxide powder, and the solid-liquid separation is performed to obtain a thorium hydroxide enriched solid and a rare earth sulfate solution.