Anion intercalation chalcogenide phase change material and preparation method and application thereof

By dissolving non-metallic elements in ethylenediamine to form anionic precursor solution and sonicating with chalcogen compounds, the 2H-1T phase transition of chalcogen compounds is achieved, which solves the energy density and structural stability of all-solid lithium batteries, and improves the Conductivity and electrochemical properties provide high-performance negative electrode materials for lithium-ion batteries.

CN118929758APending Publication Date: 2024-11-12TONGJI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410983539.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The energy density of all-solid lithium batteries is limited by the theoretical specific capacity of the positive electrode material and the solid-solid poor contact between the positive electrode material and the sulfide solid electrolyte. In addition, the traditional alkali metal intercalation method has complex intercalation process, easy ion reaction and structure. Poor stability problem.

Method used

By dissolving non-metallic elements in ethylenediamine to form an anion precursor solution, mixing it with chalcogen compounds and sonicating it, the anion intercalation enters the chalcogen compounds layer, and the phase transition from 2H phase to 1T phase is achieved, and the phase transition from 2H phase to 1T phase is expanded. Layer spacing and improve structural stability.

Benefits of technology

Effectively realizes the 2H-1T phase transition, significantly improving the conductivity and electrochemical performance of the material. As the negative electrode material of lithium-ion battery, it exhibits excellent lithium storage performance with high capacity, large magnification and long cycles, solving the limitations of traditional methods. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929758A_ABST
    Figure CN118929758A_ABST
Patent Text Reader

Abstract

The invention relates to a phase change material of an anion intercalation chalcogenide as well as a preparation method and application of the phase change material. The chalcogenide phase change is realized through anion intercalation, and specifically, an anion precursor solution is formed by dissolving a nonmetal simple substance in ethidene diamine. The method comprises the following steps: mixing a chalcogenide with an anion precursor solution, and carrying out ultrasonic treatment, so that anions carried by ethylenediamine are intercalated into the interlayer of the chalcogenide; the method not only can enlarge the interlayer spacing of the chalcogenide and initiate the phase change of the chalcogenide from the 2H phase to the 1T phase, but also can ensure the structural stability of the material. The phase change result is represented by means of X-ray diffraction, Raman spectrum and the like. Research results show that the anion intercalation method can effectively realize 2H-1T phase change, the conductivity and electrochemical performance of the material are remarkably improved, and the material serving as a lithium ion negative electrode material has excellent lithium storage performance of high capacity, high rate and long circulation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrochemical technology, and in particular to a phase change material of an anion intercalated chalcogenide compound and a preparation method and application thereof. Background Art

[0002] The rapid development of electric vehicles has put forward higher and higher requirements on the safety and energy density of batteries. All-solid-state lithium batteries using sulfide solid electrolytes have become a very promising development target due to their superior safety performance, high ionic conductivity at room temperature and long cycle life. However, for all-solid-state lithium batteries, their energy density is widely limited by the theoretical specific capacity of the positive electrode material and the solid-solid poor contact between the positive electrode material and the sulfide solid electrolyte. Therefore, it is particularly important to develop high-performance positive electrode materials.

[0003] Chalcogenides, especially molybdenum disulfide (MoS2), tungsten disulfide (WS2) and tin disulfide (SnS2), are widely used in lithium-ion batteries, photocatalysis, electrocatalysis and other fields due to their unique layered structure and excellent physical and chemical properties. Among these chalcogenides, there are two main crystalline phases: 2H phase and 1T phase. The 2H phase is a semiconductor phase with low conductivity and high chemical stability; while the 1T phase is a metallic phase with excellent conductivity but relatively low stability. Traditionally, the phase transition of chalcogenides from 2H phase to 1T phase can be achieved by intercalation of alkali metal ions (such as lithium, sodium, potassium, etc.). However, this method has certain limitations, including complex intercalation process, easy reaction of intercalated ions, and poor structural stability of the material after phase transition. Summary of the invention

[0004] The purpose of the present invention is to provide a phase change material of anion intercalated chalcogenide in order to overcome the energy storage bottleneck of lithium-ion battery electrode materials and the application defects of chalcogenide in the prior art, and a preparation method and application thereof. The present invention realizes the phase change of chalcogenide by anion intercalation. Specifically, a non-metallic element (such as sulfur, phosphorus, etc.) is dissolved in ethylenediamine to form an anion precursor solution. The chalcogenide is mixed with the anion precursor solution and ultrasonically treated so that the anions carried by ethylenediamine are intercalated into the interlayer of the chalcogenide. This method can not only expand the interlayer spacing of the chalcogenide and induce its phase change from 2H phase to 1T phase, but also ensure the structural stability of the material. The phase change results are characterized by means of X-ray diffraction (XRD), Raman spectroscopy (Raman), etc. The research results show that the anion intercalation method can effectively realize the 2H-1T phase change, and significantly improve the conductivity and electrochemical properties of the material, as a lithium-ion negative electrode material with high capacity, high rate and long cycle excellent lithium storage performance. After the local 2H phase transforms into the 1T phase, the material has excellent conductivity and stability at the same time, thus exhibiting excellent lithium storage performance with high capacity, large rate and long cycle in applications such as lithium-ion batteries, providing a new way to develop high-performance lithium-ion battery negative electrode materials.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A method for preparing a phase change material of an anion intercalated chalcogenide compound comprises dissolving a non-metallic element with ethylenediamine to form an anion precursor solution, mixing the anion precursor solution with a chalcogenide compound to induce a phase change of the chalcogenide compound, and obtaining the phase change material of the anion intercalated chalcogenide compound.

[0007] Furthermore, after the anion precursor solution is mixed with the sulfide compound, the anions carried by ethylenediamine are intercalated into the interlayers of the sulfide compound, expanding the two-dimensional interlayer spacing of the sulfide compound and simultaneously inducing a phase change of the sulfide compound, wherein part of the 2H phase is transformed into the 1T phase, thereby obtaining a phase change material of the anion intercalated sulfide compound.

[0008] Furthermore, the specific preparation steps of the phase change material of the anion intercalated chalcogenide compound are as follows:

[0009] S1. Preparation of anion precursor solution:

[0010] Dissolving a non-metallic element in ethylenediamine to obtain an anion precursor solution;

[0011] S2. Intercalation of chalcogenides:

[0012] The sulfide compound is mixed with the anion precursor solution obtained in step S1, subjected to ultrasonic treatment, and the solid is collected by centrifugation, washed, and freeze-dried to obtain a phase change material of the anion intercalated sulfide compound.

[0013] Furthermore, in step S1, the non-metallic element includes sulfur, phosphorus, selenium and the like.

[0014] Furthermore, in step S1, the concentration range of the non-metallic element dissolved in ethylenediamine is 1 mg / mL to 50 mg / mL.

[0015] Furthermore, in step S1, the dissolving temperature is 25-60°C.

[0016] Furthermore, in step S1, the dissolution process of the non-metallic element in ethylenediamine requires stirring, and the stirring time is controlled to be 30 minutes to 6 hours.

[0017] Furthermore, in step S2, the mass ratio of the chalcogenide compound to the anion precursor solution is 1:(5-10).

[0018] Furthermore, in step S2, the chalcogenide compound includes MoS2, WS2, MoSe2 and WSe2, etc.

[0019] Furthermore, in step S2, the ultrasonic treatment time is 30 minutes to 12 hours, and the ultrasonic treatment temperature is 0°C to 60°C.

[0020] Furthermore, in step S2, the mixture after ultrasonic treatment is centrifuged and washed for multiple times to obtain a phase change material of anion intercalated chalcogenide.

[0021] Furthermore, in step S2, the washing liquid is deionized water, and the washing times are 3-10 times to ensure the removal of excess ethylenediamine on the surface of the phase change material.

[0022] Furthermore, in step S2, liquid nitrogen is required for rapid freezing before freeze-drying.

[0023] Furthermore, in step S2, the freeze-drying time is 1 day to 10 days, until completely freeze-dried.

[0024] The present invention also provides a phase change material of anion intercalated chalcogenide. The phase change material obtained by the above preparation method is a two-dimensional sheet structure assembled by chalcogenide. Anions are inserted between two layers of the chalcogenide. The interlayer distance between the two layers of the chalcogenide is

[0025] In addition, the present invention also provides an application of a phase change material of an anion intercalated sulfide compound, wherein the phase change material of an anion intercalated sulfide compound is used to prepare an electrode material of a secondary battery.

[0026] Furthermore, the secondary battery includes a lithium ion battery, a sodium ion battery, a potassium ion battery, a zinc ion battery, and the like.

[0027] Furthermore, the phase change material of the anion intercalated chalcogenide compound as a negative electrode material of a lithium ion battery has better conductivity and stability.

[0028] Furthermore, the preparation method of the lithium-ion battery is as follows:

[0029] S1. Mixing the phase change material of the anion intercalated chalcogenide compound with a conductive agent and a binder, adding N-methylpyrrolidone (NMP) as a solvent, grinding to a uniform black slurry, coating it on a current collector, and drying it in a vacuum drying oven to prepare an electrode sheet;

[0030] S2. Assemble the electrode sheet obtained in step S1 with a separator, an electrolyte and a counter electrode into a lithium-ion battery, and perform an electrochemical performance test to evaluate its energy storage performance.

[0031] Furthermore, in step S1, the conductive agent is selected from any one or more of acetylene black, carbon nanotubes and graphene.

[0032] Furthermore, in step S1, the binder is selected from any one or more of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC) or polyacrylic acid (PAA).

[0033] Furthermore, in step S1, the electrolyte is a conventional lithium-ion battery electrolyte, and the electrolyte includes ethylene carbonate (EC), diethyl carbonate (DEC) and lithium hexafluorophosphate (LiPF6).

[0034] Furthermore, in step S1, the mass ratio of the phase change material of the anion intercalated chalcogenide compound, the conductive agent and the binder is 6:1:1 to 10:1:1, preferably 8:1:1 and 7:2:1.

[0035] Furthermore, in step S1, the current collector is aluminum foil or copper foil, and the coating thickness is 50 to 200 μm.

[0036] Furthermore, in step S1, the vacuum drying temperature is 60-90° C., and the drying time is 6-12 hours.

[0037] The technical principles of the present invention are as follows:

[0038] The present invention proposes a method for realizing phase change of chalcogenide compounds by anion intercalation, aiming to improve the conductivity and electrochemical properties of the material. The technical principle is based on the action of ethylenediamine (EDA), and EDA is dissolved in non-metallic elements (such as sulfur, phosphorus, etc.) to form a solution containing anions. The solution is ultrasonically treated with a chalcogenide (such as MoS2), so that the anions (such as sulfur ions and phosphorus ions) carried by EDA are inserted into the interlayer of the chalcogenide compound to expand its two-dimensional interlayer spacing. At the same time, the intercalation of anions triggers the phase change of the chalcogenide from the 2H phase to the 1T phase. The 2H phase is a semiconductor phase with poor conductivity, while the 1T phase is a metal phase with better conductivity. The local 2H-1T phase change is realized by anion intercalation, which not only ensures the structural stability of the material, but also improves the conductivity of the local area, thereby significantly improving the reaction kinetics of chalcogenide compounds in the secondary battery energy storage process, so that it has excellent capacity, rate and cycle performance.

[0039] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0040] 1. The present invention innovatively utilizes anion intercalation to realize the phase change of chalcogenide compounds, providing a simpler and more effective technical approach, which not only maintains the structural stability of the material, but also improves its electrical conductivity and reaction kinetics, providing new possibilities for the application of chalcogenide compounds in the field of energy storage and conversion.

[0041] 2. The present invention dissolves non-metallic elements such as sulfur or phosphorus by ethylenediamine, and after ultrasonic treatment of the mixed solution and chalcogenide for a period of time, ethylenediamine enters the van der Waals interlayer of the chalcogenide with dissolved anions, expands the two-dimensional interlayer spacing of the chalcogenide, and induces the chalcogenide to undergo a phase change, wherein part of the 2H phase of the chalcogenide is transformed into a 1T phase. Compared with the prior art, the most common method for achieving phase change of chalcogenide compounds is the alkali metal intercalation method, which generally intercalates alkali metal ions (such as lithium, sodium, potassium, etc.) into the interlayer of the chalcogenide by chemical intercalation or electrochemical intercalation to achieve its transformation from 2H phase to 1T phase. However, so far, there has been no report on a method for achieving phase change of chalcogenide compounds by anion intercalation. Finally, after the present invention realizes the transformation of the 2H phase of chalcogenide compounds into the 1T phase by anion intercalation, it has excellent lithium storage performance with high capacity, high rate and long cycle as a secondary battery electrode material.

[0042] 3. Innovation: The present invention adopts the anion intercalation method for the first time to realize the phase change of chalcogenide compounds, breaking through the limitations of the traditional alkali metal ion intercalation method and filling the gap in the prior art.

[0043] 4. Improve electrical conductivity. Through anion intercalation, local phase transition from 2H phase to 1T phase is achieved. 1T phase is a metallic phase with higher electrical conductivity, thereby improving the overall electrical conductivity of the material and helping to accelerate the reaction kinetics.

[0044] 5. Structural stability: Although the 1T phase has better conductivity, its structural stability is not as good as that of the 2H phase. The present invention realizes local phase transition through anion intercalation, which not only maintains the overall structural stability of the material, but also improves the conductivity in the local area.

[0045] 6. High-efficiency energy storage performance. The electrode material prepared by the present invention can be used in secondary batteries for excellent energy storage performance. For example, when used as a negative electrode material for lithium-ion batteries, it exhibits excellent energy storage performance of high capacity, large rate and long cycle, effectively improving the overall performance of the battery.

[0046] 7. The process is simple. Compared with the traditional complicated alkali metal intercalation method, the method of the present invention has a simple process flow, is easy to operate, is suitable for large-scale production, and improves production efficiency.

[0047] 8. Wide adaptability. The method of the present invention is applicable to the preparation of a variety of sulfide compounds, not only limited to MoS2, but also applicable to other sulfide compounds such as MoSe2, and has wide adaptability and flexibility.

[0048] 9. Environmental protection and safety. The materials and processes used in the preparation process are environmentally friendly, avoiding the use of toxic and harmful chemical reagents. The process is highly safe and is beneficial to environmental protection and production safety.

[0049] In summary, the present invention has significant advantages in improving the energy storage performance, conductivity and process simplicity of secondary battery electrode materials, and has broad application prospects and market value. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 This is the SEM photograph of the MoS2-P composite material with coexisting 2H-1T phases prepared in Example 1.

[0051] Figure 2 XRD spectra of MoS2 obtained in Comparative Example 1 and the MoS2-P composite material prepared in Example 1.

[0052] Figure 3 Raman spectra of MoS2 obtained in Comparative Example 1 and the MoS2-P composite material prepared in Example 1.

[0053] Figure 4 The lithium ion battery cycle performance of the MoS2 obtained in Comparative Example 1 and the MoS2-P composite material prepared in Example 1. DETAILED DESCRIPTION

[0054] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0055] In conjunction with the accompanying drawings, some embodiments of the present invention are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments may be combined with each other.

[0056] Example 1

[0057] This embodiment provides a method for preparing a phase change material of an anion intercalated chalcogenide compound, which realizes the MoS2 phase change by using a phosphorus ion intercalation method. The specific preparation steps are as follows:

[0058] S1. Preparation of anion precursor solution:

[0059] A certain amount of phosphorus (P) is dissolved in ethylenediamine (EDA) to form an anion precursor solution. The concentration of the anion precursor solution is controlled at 5 mg / mL, stirred evenly, and set aside.

[0060] S2, anion intercalation treatment:

[0061] MoS2 powder (2H phase) and anion precursor solution are mixed in a mass ratio of 1:10; the mixed solution is placed in an ultrasonic processor and subjected to ultrasonic treatment to obtain a reaction product.

[0062] The ultrasonic treatment time was 3 hours and the ultrasonic power was 300W to ensure that ethylenediamine was carried by sulfide ions (P 3 -) are uniformly intercalated into the interlayers of MoS2, enlarging its two-dimensional interlayer spacing. The heating process causes part of MoS2 to transform from 2H phase to 1T phase.

[0063] S3. Preparation of phase change materials of anion intercalated chalcogenide compounds

[0064] After the reaction is completed, it is cooled naturally to room temperature. The reaction product is taken out and washed repeatedly with deionized water several times until the washing liquid has no obvious color change and is washed to neutral. Then the sample aqueous solution is frozen with liquid nitrogen for 1 hour and then placed in a freeze dryer. After freeze drying for 3 days, the final MoS2-P composite material with 2H-1T phase coexistence is collected.

[0065] like Figure 1 As shown, the SEM photograph of the MoS2-P composite material with coexisting 2H-1T phases shows that after anion (P) intercalation, MoS2 still maintains a two-dimensional lamellar structure, and the intercalation method does not destroy the two-dimensional structure.

[0066] In addition, this embodiment also provides an application of a phase change material of an anion intercalated chalcogenide compound, wherein the phase change material of an anion intercalated chalcogenide compound is used to prepare a lithium ion battery, and the specific preparation steps are as follows:

[0067] S1. Preparation of negative electrode sheet for lithium-ion battery:

[0068] The 2H-1T phase coexisting MoS2-P composite material prepared above was mixed with acetylene black and polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1, N-methylpyrrolidone (NMP) was added as a solvent, and the mixture was ground into a uniform black slurry; the black slurry was evenly coated on a copper foil with a coating thickness of 100 μm; the coated electrode sheet was dried in a vacuum drying oven at 80°C for 12 hours to obtain a negative electrode sheet for a lithium-ion battery.

[0069] S2. Battery assembly and performance testing:

[0070] The lithium-ion battery negative electrode sheet and the metal lithium sheet obtained in step S1 are assembled into a button battery, and a standard electrolyte is used. The charge and discharge performance of the button battery is tested.

[0071] Comparative Example 1

[0072] This comparative example provides a MoS2 powder (2H phase), which was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. with a CAS number of 1317-33-5.

[0073] In addition, this comparative example also provides an application of MoS2 powder, wherein the MoS2 powder is used to prepare a lithium ion battery, and the specific preparation steps are the same as those in Example 1.

[0074] Electrochemical performance test

[0075] As attached Figure 2 As shown, the XRD patterns of the MoS2 obtained in Comparative Example 1 and the MoS2-P composite material prepared in Example 1 show that the van der Waals interlayer spacing of the unintercalated MoS2 is The van der Waals interlayers of the MoS2-P composite material after P anion intercalation are This indicates that the intercalation method of Example 1 successfully achieves the intercalation of anions and expands them to the van der Waals interlayers of the sulfide.

[0076] As attached Figure 3 As shown, the Raman spectra of the MoS2 obtained in Comparative Example 1 and the MoS2-P composite material prepared in Example 1 show that the unintercalated MoS2 has only two peaks, one of which is E 1 2g , one is A 1g, these two vibration peaks are characteristic peaks of the 2H phase, indicating that the unintercalated MoS2 only exists in the 2H phase. However, when the P anion is intercalated, the Raman spectrum of the sample shows the presence of E 1 2g and A 1g In addition to the peaks, there are also J1, J2, J3 and E 1g , and the vibration peak of this part is the characteristic peak of 1T phase. This shows that in addition to the 2H phase, the sample after P anion intercalation also has 1T phase, indicating that the intercalation method of Example 1 successfully achieved the partial phase transition of sulfide.

[0077] As attached Figure 4 As shown in the figure, when the MoS2 obtained in Comparative Example 1 and the MoS2-P composite material prepared in Example 1 were used as negative electrode materials for lithium-ion batteries to test the cycle performance, the test results showed that the reversible specific capacity of the MoS2-P intercalation layer was 1100 mAh g -1 The capacity of pure MoS2 is only about 850 mAh g -1 about.

[0078] The above results show that the 2H-1T phase coexisting MoS2-P composite material has excellent lithium storage performance as a lithium-ion negative electrode material, including high capacity, large rate and long cycle stability.

[0079] Example 2

[0080] This embodiment provides a method for preparing a phase change material of an anion intercalated chalcogenide compound, which realizes the phase change of MoS2 by using a sulfur ion intercalation method. The specific preparation steps are as follows:

[0081] S1. Preparation of anion precursor solution:

[0082] A certain amount of sulfur (S) is dissolved in ethylenediamine (EDA) to form an anion precursor solution. The concentration of the anion precursor solution is controlled at 2 mg / mL, stirred evenly, and set aside.

[0083] S2, anion intercalation treatment:

[0084] MoS2 powder (2H phase) and anion precursor solution are mixed at a mass ratio of 1:5. The mixed solution is placed in an ultrasonic processor and subjected to ultrasonic treatment to obtain a reaction product.

[0085] The ultrasonic treatment time was 4 hours and the ultrasonic power was 350W to ensure that ethylenediamine carried sulfide ions (S 2- ) are uniformly intercalated into the interlayers of MoS2, enlarging its two-dimensional interlayer spacing. The heating process causes part of MoS2 to transform from 2H phase to 1T phase.

[0086] S3. Preparation of phase change materials of anion intercalated chalcogenide compounds

[0087] After the reaction is completed, it is cooled naturally to room temperature. The reaction product is taken out and washed repeatedly with deionized water several times until the washing liquid has no obvious color change and is washed to neutral. Then the sample aqueous solution is frozen with liquid nitrogen for 2 hours and then placed in a freeze dryer. After freeze drying for 2 days, the final MoS2-S composite material with 2H-1T phase coexistence is collected.

[0088] In addition, this embodiment also provides an application of a phase change material of an anion intercalated chalcogenide compound, wherein the phase change material of an anion intercalated chalcogenide compound is used to prepare a lithium ion battery, and the specific preparation steps are as follows:

[0089] S1. Preparation of negative electrode sheet for lithium-ion battery:

[0090] The prepared 2H-1T phase coexisting MoS2-S composite material is mixed with acetylene black and polyvinylidene fluoride (PVDF) in a mass ratio of 7:2:1, N-methylpyrrolidone (NMP) is added as a solvent, and the mixture is ground into a uniform black slurry; the black slurry is evenly coated on a copper foil with a coating thickness of 120 μm; the coated electrode sheet is dried in a vacuum drying oven at 70°C for 10 hours to obtain a negative electrode sheet for a lithium-ion battery.

[0091] S2. Battery assembly and performance testing:

[0092] The lithium-ion battery negative electrode sheet obtained in step S1 and the metal lithium sheet are assembled into a button cell, and a standard electrolyte is used. The charge and discharge performance of the button cell is tested. The 2H-1T phase coexisting MoS2-S composite material has excellent lithium storage performance as a lithium-ion negative electrode material, including high capacity, high rate and long cycle stability.

[0093] Example 3

[0094] This embodiment provides a method for preparing a phase change material of an anion intercalated chalcogenide compound, which realizes the phase change of MoSe2 by using a sulfur ion intercalation method. The specific preparation steps are as follows:

[0095] S1. Preparation of anion precursor solution:

[0096] A certain amount of sulfur (S) is dissolved in ethylenediamine (EDA) to form an anion precursor solution. The concentration of the anion precursor solution is controlled at 6 mg / mL, stirred evenly, and set aside.

[0097] S2, anion intercalation treatment:

[0098] MoSe2 powder (2H phase) and anion precursor solution were mixed at a mass ratio of 1:8. The mixed solution was placed in an ultrasonic processor and subjected to ultrasonic treatment to obtain a reaction product.

[0099] The ultrasonic treatment time was 2.5 hours and the ultrasonic power was 320W to ensure that ethylenediamine with sulfur ions (S2-) was uniformly intercalated into the interlayer of MoSe2 to expand its two-dimensional interlayer spacing. The heating treatment process caused part of MoSe2 to transform from 2H phase to 1T phase.

[0100] S3. Preparation of phase change materials of anion intercalated chalcogenide compounds

[0101] After the reaction is completed, it is cooled naturally to room temperature. The reaction product is taken out and washed repeatedly with deionized water several times until the washing liquid has no obvious color change and is washed to neutral. Then the sample aqueous solution is frozen with liquid nitrogen for 1.5 hours and then placed in a freeze dryer. After freeze drying for 2.5 days, the final MoSe2-S composite material with 2H-1T phase coexistence is collected.

[0102] In addition, this embodiment also provides an application of a phase change material of an anion intercalated chalcogenide compound, wherein the phase change material of an anion intercalated chalcogenide compound is used to prepare a lithium ion battery, and the specific preparation steps are as follows:

[0103] S1. Preparation of negative electrode sheet for lithium-ion battery:

[0104] The prepared 2H-1T phase coexisting MoSe2-S composite material was mixed with acetylene black and polyvinylidene fluoride (PVDF) at a mass ratio of 7.5:1.5:1. N-methylpyrrolidone (NMP) was added as a solvent and ground into a uniform black slurry. The black slurry was evenly coated on a copper foil with a coating thickness of 110 μm. The coated electrode sheet was dried in a vacuum drying oven at 85°C for 11 hours to obtain a negative electrode sheet for a lithium-ion battery.

[0105] S2. Battery assembly and performance testing:

[0106] The lithium-ion battery negative electrode sheet obtained in step S1 and the metal lithium sheet are assembled into a button cell, and a standard electrolyte is used. The charge and discharge performance of the button cell is tested. The 2H-1T phase coexisting MoSe2-S composite material has excellent lithium storage performance as a lithium-ion negative electrode material, including high capacity, high rate and long cycle stability.

[0107] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a phase change material of an anion intercalated chalcogenide compound, characterized in that: A non-metallic element is dissolved by ethylenediamine to form an anion precursor solution, and the anion precursor solution is mixed with a chalcogenide compound to induce a phase change of the chalcogenide compound, thereby obtaining a phase change material of an anion intercalated chalcogenide compound.

2. The method for preparing a phase change material of an anion intercalated chalcogenide compound according to claim 1, characterized in that: After the anion precursor solution is mixed with the chalcogenide, the anions carried by ethylenediamine are intercalated into the interlayers of the chalcogenide, expanding the two-dimensional interlayer spacing of the chalcogenide and simultaneously inducing a phase change of the chalcogenide, wherein part of the 2H phase is transformed into the 1T phase, thereby obtaining a phase change material of the anion intercalated chalcogenide.

3. The method for preparing a phase change material of an anion intercalated chalcogenide compound according to claim 1, characterized in that: The specific preparation steps of the phase change material of the anion intercalated chalcogenide compound are as follows: S1. Preparation of anion precursor solution: Dissolving a non-metallic element in ethylenediamine to obtain an anion precursor solution; S2. Intercalation of chalcogenides: The sulfide compound is mixed with the anion precursor solution obtained in step S1, subjected to ultrasonic treatment, and the solid is collected by centrifugation, washed, and freeze-dried to obtain a phase change material of the anion intercalated sulfide compound.

4. The method for preparing a phase change material of an anion intercalated chalcogenide compound according to claim 3, characterized in that: In step S1, the non-metallic element includes sulfur, phosphorus and selenium; The concentration range of the non-metallic element dissolved in ethylenediamine is 1 mg / mL to 50 mg / mL; The dissolving temperature is 25-60°C.

5. The method for preparing a phase change material of an anion intercalated chalcogenide compound according to claim 3, characterized in that: In step S2, the mass ratio of the chalcogenide compound to the anion precursor solution is 1:(5-10); The chalcogenide compounds include MoS2, WS2, MoSe2 and WSe2; The washing liquid is deionized water, and the washing times are 3-10 times; The freeze-drying time is 1 day to 10 days.

6. A phase change material of an anion intercalated chalcogenide compound, characterized in that: The phase change material obtained by the preparation method according to any one of claims 1 to 5 is a two-dimensional sheet structure assembled by chalcogenide compounds, anions are inserted between two layers of the chalcogenide compounds, and the interlayer distance between the two layers of the chalcogenide compounds is 7. Application of a phase change material of an anion intercalated chalcogenide, characterized in that: The phase change material of anion intercalated sulfide compound obtained by the preparation method described in any one of claims 1 to 5 is used to prepare electrode materials for secondary batteries.

8. The use of a phase change material of an anion intercalated chalcogenide compound according to claim 7, characterized in that: The secondary batteries include lithium ion batteries, sodium ion batteries, potassium ion batteries and zinc ion batteries.

9. The use of a phase change material of an anion intercalated chalcogenide compound according to claim 8, characterized in that: The phase change material of the anion intercalated chalcogenide compound is used as the negative electrode material of the lithium ion battery. The preparation method of the lithium ion battery is as follows: S1. Mix the phase change material of the anion intercalated chalcogenide compound with a conductive agent and a binder, add N-methylpyrrolidone as a solvent, grind to a uniform black slurry, apply it on a current collector, and dry it in a vacuum drying oven to prepare an electrode sheet; S2. Assemble the electrode sheet obtained in step S1 with a separator, an electrolyte and a counter electrode into a lithium-ion battery.

10. The use of a phase change material of an anion intercalated chalcogenide compound according to claim 9, characterized in that: In step S1, the conductive agent is selected from any one or more of acetylene black, carbon nanotubes and graphene; The binder is selected from any one or more of polyvinylidene fluoride, carboxymethyl cellulose or polyacrylic acid; The electrolyte comprises ethylene carbonate, diethyl carbonate and lithium hexafluorophosphate; The mass ratio of the phase change material of the anion intercalated chalcogenide compound, the conductive agent and the binder is 6:1:1 to 10:1:1; The current collector is aluminum foil or copper foil, and the coating thickness is 50 to 200 μm; The vacuum drying temperature is 60-90° C., and the drying time is 6-12 hours.