Waterborne polyurethane dispersion as well as preparation method and application thereof
By using diol with short branched side groups and silicon-based polyester monomers in the synthesis of aqueous polyurethane dispersions, combined with step-by-step polymerization and post-chain expansion processes, the poor environmental protection and high viscosity of solvents in the prior art are solved. Problem: The water-based polyurethane dispersion with low viscosity and good dispersion is achieved, which improves the leveling and water resistance of the coating, and is suitable for automotive coatings.
Patent Information
- Application Number
- CN202410991283.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The solvent used in the synthesis process of existing aqueous polyurethane dispersions has poor environmental protection and high viscosity, which affects the leveling and water resistance of the coating.
20 to 30 parts of polymer diol, 5 to 15 parts of isocyanate, 1.2 to 4 parts of epoxy resin, 1 to 3 parts of neutralizing agent, 0.01 to 0.05 parts of catalyst, 0.1 to 2 parts of post-chain extender and 35- The formula of 75 parts of deionized water is added, and the diol and silicon-based polyester monomer with short branched side groups is reduced through step-by-step polymerization and post-chain expansion processes, and the polymer viscosity is improved, dispersibility and water resistance are improved.
It realizes water-based polyurethane dispersion with low viscosity and good dispersion, which is suitable for automotive coatings, improves the leveling, adhesion and water resistance of the paint film, and meets environmental protection requirements.
Smart Images

Figure BDA0004958938630000071 
Figure BDA0004958938630000081 
Figure BDA0004958938630000082
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of modified waterborne polyurethane dispersions, and relates to a waterborne polyurethane dispersion and a preparation method and application thereof. Background Art
[0002] Waterborne polyurethane is a polymer material developed by using water as the dispersion medium instead of the organic solvent in traditional polyurethane. It can be formulated into a coating that contains no or only a small amount of organic solvent. It has the advantages of being non-toxic, non-flammable, non-polluting, energy-saving, safe and reliable, not easy to damage the coated surface, easy to operate and modify, etc. Waterborne polyurethane is showing a trend of gradually replacing solvent-based polyurethane.
[0003] There have been some reports on the synthesis of waterborne polyurethane. For example, CN101831236A discloses a waterborne metallic glitter base paint and a preparation method thereof, wherein the waterborne polyurethane dispersion used is prepared by an acetone method, which is environmentally friendly.
[0004] CN 110545925 B discloses a method for forming a multilayer coating film, wherein the polyurethane dispersion used is also a method using methyl ethyl ketone as a solvent and distilling it off under reduced pressure, which also does not meet the requirements of environmental protection.
[0005] Similarly, the cosolvent used in CN10459882B is N-methylpyrrolidone, etc., which is carcinogenic and is currently not recommended for use.
[0006] CN103980461B, CN106496485B, CN113621129B, CN117362575A, etc. all disclose the work of epoxy-modified waterborne polyurethane, but the epoxy resins they use have high viscosity, high polymer cross-linking degree, and require a large amount of solvent in the reaction, which is poor in environmental protection. At the same time, the obtained product has high viscosity, which is not conducive to the leveling of the coating preparation.
[0007] CN111909354B discloses a waterborne polyurethane resin and its preparation method and application. The resin is synthesized from polyol prepolymer, hydrophilic monomer, functional monomer, etc. The waterborne mid-coat for automobiles prepared using the resin has excellent stone chip resistance and paint film hardness, and the waterborne color paint for automobiles prepared using the resin has excellent adhesion and flexibility. However, the resin obtained by the method has a high viscosity, the compounding and leveling properties of the paint film are limited, and the resin acid value is very high, which is not conducive to water resistance. Summary of the invention
[0008] The object of the present invention is to provide an aqueous polyurethane dispersion with low viscosity, good dispersibility and excellent water resistance.
[0009] In order to achieve the above object, the technical solution of the present invention is as follows:
[0010] A waterborne polyurethane dispersion, the raw materials of which include 20-30 parts of polymer diol, 5-15 parts of isocyanate, 1.2-4 parts of hydrophilic chain extender, 0.6-2.1 parts of epoxy resin, 1-3 parts of neutralizer, 0.01-0.05 parts of catalyst, 8-18 parts of cosolvent, 0.1-2 parts of post-chain extender and 35-75 parts of deionized water;
[0011] The raw materials of the polymer diol include a diol with short-chain side groups, a silicon-based polyester monomer and a dibasic acid (anhydride) in a molar ratio of 1: (0.1-0.4): (0.4-1.3); the short-chain side groups in the diol with short-chain side groups are C1-C3 alkyl groups.
[0012] In a preferred embodiment, the number of carbon atoms in the main chain of the diol with short chain side groups is 3-6.
[0013] In a preferred embodiment, the diol with short-chain side groups is at least one of 3-methyl-1,5-pentanediol, neopentyl glycol, 2-methyl-1,3-propanediol, 1,3-butanediol, and 2,2,4-trimethyl-1,3-pentanediol.
[0014] The short chain side groups help reduce polymer viscosity while improving water resistance.
[0015] In one preferred embodiment, the silicon-based polyester monomer contains a structural unit of Si(OSiMe3)n, where n=2 or 3.
[0016] Compared with short-chain side groups, it has greater steric hindrance and greater rigidity than long-chain substituents, which is conducive to reducing molecular chain entanglement, and can more effectively increase the free volume between molecular chains and reduce the viscosity of the system. At the same time, siloxane has low surface energy, which can improve leveling and water resistance. The trimethylsiloxy structure is also more stable than conventional alkoxy groups such as methoxy groups, and is not easy to decompose during polyester synthesis.
[0017] In one preferred embodiment, the molar content of the silicon-based polyester monomer is 5% to 10%.
[0018] If the content of silicon-based polyester monomer is too low, it cannot effectively reduce polymer viscosity and improve water resistance. If the content of silicon-based polyester monomer is too high, the system compatibility is poor, the prepolymer is easy to phase separate, and it is difficult to hydrate and disperse to obtain a stable polymer dispersion.
[0019] In one preferred embodiment, the silicon-based polyester monomer can be synthesized from dialkoxysilanes, trialkoxysilanes, and trimethylsilyl end-capping agents of different structures.
[0020] In one preferred embodiment, the silicon-based polyester monomer is capped with hydrogen-containing alkoxysilane and trimethylsilyl capping agent, and then subjected to hydrosilylation reaction with 2-vinyl-1,3-propanediol to obtain a diol monomer with branched silicon groups in the side groups.
[0021] In one preferred embodiment, the silicon-based polyester monomer can be capped with hydrogen-containing alkoxysilane and trimethylsilyl capping agent, and then subjected to hydrosilylation with unsaturated dibasic acid (anhydride) to obtain a diacid (anhydride) monomer with branched silicon groups on the side groups.
[0022] In a preferred embodiment, the hydrogen-containing alkoxysilane is one or more of trimethoxysilane, triethoxysilane, methyldimethoxysilane and methyldiethoxysilane.
[0023] In one preferred embodiment, the silicon-based polyester monomer can be terminated by epoxyalkoxysilane and trimethylsilyl end-capping agent to obtain a polyester monomer with branched silicon groups in the side groups.
[0024] In one preferred embodiment, the epoxyalkoxysilane is one or more of 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, 3-(2,3-epoxypropyloxy)propyltriethoxysilane, 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexane)ethyltriethoxysilane, 3-(2,3-epoxypropyloxy)propylmethyldimethoxysilane, 3-(2,3-epoxypropyloxy)propylmethyldiethoxysilane, 2-(3,4-epoxycyclohexane)ethylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexane)ethylmethyldiethoxysilane.
[0025] In a preferred embodiment, the trimethylsilyl capping agent is one or more of trimethylmethoxysilane, hexamethyldimethoxysilane, trimethylsilanol, and trimethylchlorosilane.
[0026] In one preferred embodiment, the polymer diol has a number average molecular weight Mn of 500 to 10,000, preferably 1,000 to 5,000, and more preferably 1,500 to 3,500.
[0027] If the molecular weight is too high, the soft segment is too long, the product viscosity is high, and it is not conducive to hydration dispersion. If the molecular weight is too low, the soft segment is too short, and the flexibility, water resistance and chemical resistance will be relatively poor.
[0028] In a preferred embodiment, the isocyanate is at least one of isophorone diisocyanate IPDI, hexamethylene diisocyanate HDI, dicyclohexylmethane diisocyanate HMDI, toluene diisocyanate TDI, and diphenylmethane diisocyanate MDI.
[0029] Polymer diols and isocyanates are the main raw materials for high molecular weight polymers and provide the main macromolecular chain structure of the resin.
[0030] In one preferred embodiment, the hydrophilic chain extender is at least one of a dihydroxy compound containing a carboxyl group or a sulfonic acid group, polyethylene glycol, and a quaternary ammonium salt.
[0031] The hydrophilic chain extender provides hydrophilic groups and provides emulsification and dispersion stability for the waterborne polyurethane dispersion.
[0032] In a preferred embodiment, the dihydroxy compound containing a carboxyl group or a sulfonic acid group is at least one of dimethylol propionic acid, dimethylol butyric acid, and sodium 1,4-dihydroxy-2-butane sulfonate.
[0033] In one preferred embodiment, the epoxy resin is a hydroxyl-containing liquid epoxy resin, preferably at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, and hydrogenated bisphenol A epoxy resin.
[0034] In one preferred embodiment, the epoxy equivalent of the epoxy resin is less than 210 g / eq and the viscosity is less than 2000 cps. Too high epoxy equivalent and viscosity will easily lead to excessive increase in coating viscosity and poor leveling properties.
[0035] In one preferred embodiment, the epoxy resin is used in an amount of 3-7% of the amount of the polymer diol. If the epoxy resin is used in an amount that is too low, it will not improve the adhesion, and if it is used in an amount that is too high, it will easily cause the coating viscosity to increase too much, affecting the leveling property.
[0036] The hydroxyl groups in the epoxy resin react with isocyanate in the chain extension stage and participate in the growth of the polymer main chain, while the epoxy groups continue to react with amino groups in the post-chain extension and coating applications, which helps to increase the crosslinking degree of the polymer and improve the adhesion of the paint film.
[0037] In one preferred embodiment, the epoxy resin is preferably YD-113 or YDF-165.
[0038] In one preferred embodiment, the isocyanate index R of the polyurethane is 1.05 to 1.6, preferably 1.1 to 1.3. The isocyanate index R of the polyurethane is the ratio of isocyanate to polyol equivalent. If the R value is too low, the molecular weight of the prepolymer is too high, the viscosity is very high, the flexible segment is too long, and hydration dispersion is difficult. If the R value is too high, the rigid segment content is high, the polarity is too high, the NCO content is high, and it is easy to gel during hydration. Even if a dispersion can be obtained, its particle size is large, the viscosity is high, the stability is poor, and the flexibility and water resistance are also poor.
[0039] In a preferred embodiment, the neutralizing agent is at least one of triethylamine, triethanolamine, and N,N-dimethylethanolamine (DMEA).
[0040] The neutralizing agent is a compound that can ionize the hydrophilic group.
[0041] In a preferred embodiment, the post-chain extender is a diamine, such as at least one of ethylenediamine, butanediamine, and isophoronediamine (IPDA).
[0042] The post-chain extender can significantly increase the molecular weight of polyurethane, which helps to obtain a high molecular weight waterborne polyurethane dispersion.
[0043] In one preferred embodiment, the raw materials of the aqueous polyurethane dispersion also include a catalyst.
[0044] In a preferred embodiment, the catalyst is an organic tin catalyst, preferably at least one of dibutyltin dilaurate DBTDL and stannous octoate.
[0045] In a preferred embodiment, the raw materials of the aqueous polyurethane dispersion also include a cosolvent.
[0046] In a preferred embodiment, the co-solvent is at least one of N,N-dimethylacetamide DMAc and N,N-diethylformamide DEF.
[0047] In one preferred embodiment, the number average molecular weight Mn of the aqueous polyurethane dispersion is 10000 to 150000, preferably 20000 to 100000, more preferably 30000 to 60000. If the molecular weight is too low, the flexibility, water resistance and chemical resistance are poor, and if the molecular weight is too high, the viscosity is too high, the compatibility with other components is poor, and the leveling property is poor.
[0048] In one preferred embodiment, the acid value of the aqueous polyurethane dispersion is 5 to 12 mgKOH / g, preferably 7 to 9 mgKOH / g. If the acid value is too low, the dispersion stability is poor, and if the acid value is too high, the coating film has poor water resistance.
[0049] The viscosity of the aqueous polyurethane dispersion is 10 to 2000 mPa.s, preferably 30 to 1000 mPa.s, and more preferably 50 to 300 mPa.s. If the viscosity is too low, the mechanical properties are poor, and if the viscosity is too high, the leveling property of the coating is poor.
[0050] The solid content of the aqueous polyurethane dispersion is 20-60%, preferably 20-50%, more preferably 30-40%. If the solid content is too low, the drying is slow, the effective content is low, and the practicality is poor. If the solid content is too high, the dispersion stability is poor.
[0051] The present invention also claims a method for preparing the aqueous polyurethane dispersion, comprising:
[0052] S1. After removing water from the polymer diol in vacuum, add isocyanate at 45-55°C, raise the temperature to 80-90°C, react; then add a hydrophilic chain extender and a catalyst, continue the reaction; then add an epoxy resin and continue the reaction;
[0053] S2, cooling to 30-50°C, adding a neutralizing agent to react for 10 minutes to 1 hour, and then adding deionized water to disperse evenly under strong shearing conditions; then adding a post-chain extender, and continuing to stir and disperse for 10 minutes to 2 hours; to obtain the aqueous polyurethane dispersion.
[0054] The present invention also claims to protect the use of the aqueous polyurethane dispersion in preparing aqueous mid-coat or aqueous metallic basecoat for automobiles.
[0055] A water-based mid-coat for automobiles comprises 10-30 parts by weight of a water-based polyurethane dispersion.
[0056] In one preferred embodiment, the automotive water-based mid-coat further comprises, by weight, 10-30 parts of acrylic emulsion, 1-10 parts of amino resin, 10-20 parts of water-based polyester, 15-35 parts of color paste, 0.1-0.5 parts of wetting agent and 0.1-0.5 parts of defoaming agent.
[0057] A water-based metallic basecoat for automobiles comprises 10 to 30 parts by weight of a water-based polyurethane dispersion.
[0058] In one preferred embodiment, the automotive water-based metallic basecoat further comprises, by weight, 10-30 parts of acrylic emulsion, 1-10 parts of amino resin, 10-20 parts of aluminum paste, 1-5 parts of color paste, 0.1-0.5 parts of wetting agent, 0.1-0.5 parts of defoaming agent and 1-10 parts of cosolvent.
[0059] The present invention is dedicated to providing a synthesis and application of a water-based polyurethane dispersion for automobile paint. The synthesis process adopts a prepolymer method, has good environmental protection, low R value, and step-by-step polymerization and post-chain extension processes to ensure the acquisition of high molecular weight polyurethane. Short-chain side groups, branched silicon-based side groups and low-viscosity epoxy are added at a low content to keep the dispersion at a low viscosity, which is convenient for adjusting the leveling property during the preparation of the paint film. At the same time, the presence of silicon-based and epoxy-based groups is beneficial to the improvement of the water resistance and adhesion of the paint film, thereby meeting the requirements of automobile paint for moisture resistance, especially high-pressure water resistance.
[0060] The beneficial effects of the present invention are:
[0061] (1) Use a small amount of environmentally friendly high-boiling point solvents, no need for recycling, low VOC, easy to prepare automotive midcoat and color paint, and comply with regulations.
[0062] (2) Selecting polymer diols with short-chain side groups makes the polyurethane prepolymer have a lower viscosity and is easy to hydrate and disperse. The resulting waterborne polyurethane dispersion has a low viscosity and good compatibility with other materials. The resulting coating has good leveling properties and a smooth and flat paint film appearance.
[0063] (3) Use diols with branched silicon groups in the side groups. The branched structure can also keep the system at a low viscosity. At the same time, the low surface energy of siloxane can improve leveling and increase water resistance.
[0064] (4) Design a lower R value, use a small amount of low-viscosity epoxy resin for modification, and adopt a step-by-step polymerization and post-chain extension process to obtain a high molecular weight linear structure polyurethane dispersion. The automotive coating obtained based on this resin has excellent mechanical properties, good adhesion, good water and chemical resistance, good moisture resistance, and especially good high-pressure water washing adhesion. DETAILED DESCRIPTION
[0065] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.
[0066] The reagents used in the following examples are all available from commercial sources.
[0067] Example 1
[0068] Trimethoxysilane and trimethylmethoxysilane in a molar ratio of 1:3 were stirred at room temperature for 12 hours under the catalysis of 0.1M HCl for end-capping, and then hydrosilylation was carried out with 2-vinyl-1,3-propanediol in a molar ratio of 1:1 under the catalysis of 10ppm dibutyltin dilaurate at room temperature to obtain a diol monomer SiA with a tri(trimethylsiloxy)silyl group on the side group.
[0069] 2,2,4-trimethyl-1,3-pentanediol, silicon-based diol SiA and adipic acid were added to the reactor in a molar ratio of 1:0.2:1.1, heated to 165°C, reacted for 1.5 hours, heated to 185°C, reacted for 2 hours, heated to 200°C, and dehydrated by vacuum distillation until the acid value was 0.45 mgKOH / g and the hydroxyl value was 56 mgKOH / g. The obtained polyester diol was defined as PEPL1.
[0070] Example 2
[0071] Trimethoxysilane and hexamethyldisiloxane in a molar ratio of 2:3 were capped by stirring at room temperature for 12 hours under the catalysis of 0.1M HCl, and then hydrosilylated with fumaric acid in a molar ratio of 1:1 under the catalysis of 10ppm dibutyltin dilaurate at room temperature to obtain a diacid monomer SiB with a tri(trimethylsiloxy)silyl group on the side group.
[0072] 3-Methyl-1,5-pentanediol, silicon-based dibasic acid SiB and adipic acid were added to the reactor in a molar ratio of 1:0.25:0.65, heated to 165°C, reacted for 1.5 hours, heated to 185°C, reacted for 2 hours, heated to 200°C, and dehydrated by vacuum distillation until the acid value was 0.37 mgKOH / g and the hydroxyl value was 55 mgKOH / g. The obtained polyester diol was defined as PEPL2.
[0073] Example 3
[0074] Trimethoxysilane and trimethylsilanol were capped at a molar ratio of 1:3 under stirring at room temperature for 12 h under the catalysis of 0.1 M HCl, and then hydrosilylated with maleic anhydride at a molar ratio of 1:1 to obtain an anhydride monomer SiC with a tri(trimethylsiloxy)silyl group on the side group.
[0075] 2-Methyl-1,3-propanediol, silicon-based anhydride SiC and adipic acid were added to the reactor in a molar ratio of 1:0.15:0.4, heated to 165°C, reacted for 1.5 hours, heated to 185°C, reacted for 2 hours, heated to 200°C, and dehydrated by vacuum distillation until the acid value was 0.28 mgKOH / g and the hydroxyl value was 55.1 mgKOH / g. The obtained polyester diol was defined as PEPL3.
[0076] Example 4
[0077] 3-(2,3-epoxypropoxy)propyltrimethoxysilane and hexamethyldisiloxane were capped in a molar ratio of 2:3 under the catalysis of 0.1M HCl to obtain a polyester monomer SiD with a tri(trimethylsiloxy)silyl group on the side group.
[0078] Neopentyl glycol, silicon-based polyester monomer SiD and phthalic anhydride were added to the reactor in a molar ratio of 1:0.4:1.3, and 100 ppm of catalyst potassium acetate / dodecyltrimethylammonium bromide (1:1) was added, heated to 95°C, and reacted for about 6 hours to obtain a polyester diol with an acid value of 0.43 mgKOH / g and a hydroxyl value of 54.7 mgKOH / g. The obtained polyester diol was defined as PEPL4.
[0079] Comparative Example 1
[0080] 2,2,4-trimethyl-1,3-pentanediol, silicon-based diol SiA and adipic acid were added to the reactor in a molar ratio of 1:1:1.9, heated to 165°C, reacted for 1.5 hours, heated to 185°C, reacted for 2 hours, heated to 200°C, and dehydrated by vacuum distillation until the acid value was 0.35 mgKOH / g and the hydroxyl value was 54 mgKOH / g. The obtained polyester diol was defined as PEPL5.
[0081] Comparative Example 2
[0082] Dimethylmethoxysilane and trimethylmethoxysilane in a molar ratio of 1:1 were stirred at room temperature for 12 hours under the catalysis of 0.1M HCl for end-capping, and then hydrosilylation was carried out with 2-vinyl-1,3-propanediol in a molar ratio of 1:1 under the catalysis of 10ppm dibutyltin dilaurate at room temperature to obtain a diol monomer SiE with a trimethylsiloxysilyl group on the side group.
[0083] 2,2,4-trimethyl-1,3-pentanediol, silicon-based diol SiE and adipic acid were added to the reactor in a molar ratio of 1:0.2:1.1, heated to 165°C, reacted for 1.5 hours, heated to 185°C, reacted for 2 hours, heated to 200°C, and dehydrated by vacuum distillation until the acid value was 0.42 mgKOH / g and the hydroxyl value was 54 mgKOH / g. The obtained polyester diol was defined as PEPL6.
[0084] Example 5
[0085] The polyester diols of Examples 1-4 and Comparative Examples 1-2 were prepared into aqueous polyurethane dispersions according to the following method:
[0086] Put the polyester diol into the reactor, remove water in vacuum at 100-120℃ until the water content is <0.05%, and fill with nitrogen for protection. Cool down to 50℃, add isocyanate and cosolvent, heat up to 80-90℃, and react until the NCO content is <3.6%. Add hydrophilic monomer and catalyst, and continue to react until the NCO content is <2.8%. Add liquid epoxy resin and continue to react until the NCO content is <1.4%. Cool down to 30-50℃, add neutralizer and react for 10min-1h. Under strong shear conditions, slowly add deionized water to disperse evenly, which takes 10min-1h. Under strong shear conditions, add the solution of post-chain extender and deionized water, and continue to stir and disperse for 10min-2h. Filter to obtain waterborne polyurethane dispersion.
[0087] The formulations of the aqueous polyurethane dispersions prepared in the examples and comparative examples are shown in the following table.
[0088] Table 1 Formulation of waterborne polyurethane dispersion prepared in Example
[0089]
[0090]
[0091] Table 2 Comparative Example Preparation of Waterborne Polyurethane Dispersion Formula
[0092]
[0093]
[0094] The code and name of the components are:
[0095] YA-7620: Gaoding Fine Chemicals (Kunshan) Hexanediol Adipic Acid Polyester Polyol
[0096] P-2010: Japan Kuraray 3-methyl-1,5-pentanediol polyester polyol
[0097] IPDI: Isophorone diisocyanate
[0098] HDI: Hexamethylene diisocyanate
[0099] YD-113: Kunshan Guodu low viscosity bisphenol A epoxy resin
[0100] YDF-165: Kunshan Guodu low viscosity bisphenol A epoxy resin
[0101] DMPA: dimethylolpropionic acid
[0102] DMBA: dimethylolbutyric acid
[0103] IPDA: isophorone diamine
[0104] EDA: Ethylenediamine
[0105] When the reaction of formula 1-6 is carried out according to the formula composition in Table 1 and the synthesis method of Example 5, the raw materials are in accordance with the formula ratio, the reaction can be successfully completed, and an aqueous polyurethane dispersion that meets the specifications of solid content, viscosity, particle size, molecular weight, and acid value is obtained.
[0106] When the reaction of Formula 7 is carried out according to the formulation composition in Table 2 and the synthesis method of Example 5, the molecular weight of the obtained aqueous polyurethane dispersion is significantly lower due to the absence of a post-chain extension reaction stage.
[0107] When the reaction of Formula 8 was carried out according to the formulation composition of Table 2 and the synthesis method of Example 5, due to the high R value (1.76), the molecular weight of the obtained aqueous polyurethane dispersion was also low, and the particle size was large (110nm) and the viscosity was high (535cps).
[0108] When the reaction of Formula 10 was carried out according to the formulation composition of Table 2 and the synthesis method of Example 5, since the polyester polyol used did not contain short-chain side groups, the resulting aqueous polyurethane dispersion had a very high viscosity (120,500 cps) and a relatively coarse particle size (107.1 nm).
[0109] When the reaction of Formula 11 was carried out according to the formulation composition of Table 2 and the synthesis method of Example 5, the polyester polyol used contained short-chain side groups but no branched silicon-based side groups, and the resulting aqueous polyurethane dispersion had a relatively high viscosity (424 cps).
[0110] When the reaction of Formula 12 is carried out according to the formulation composition of Table 2 and the synthesis method of Example 5, the polyester polyol used contains short-chain side groups and branched silicon-based side groups, but the branched silicon-based side groups are monotrimethylsiloxysilyl side groups, and the steric hindrance effect is limited. The resulting aqueous polyurethane dispersion has a relatively high viscosity (346 cps) and a slightly coarse particle size (105 nm).
[0111] When the reaction of Formula 13 was carried out according to the formulation composition in Table 2 and the synthesis method of Example 5, it was difficult to obtain a stable and uniform aqueous polyurethane dispersion, which may be due to the excessively high silicon-based content causing phase separation in the prepolymer.
[0112] Example 6
[0113] Using the waterborne polyurethane dispersions synthesized in Table 1 and Table 2 (except Formulation 13), automotive waterborne midcoat and automotive waterborne 1K metallic basecoat were prepared according to the formulations in Table 3 and Table 4, respectively.
[0114] Table 3 Automotive water-based mid-coat formulation
[0115] raw material Manufacturer and Model m / g Waterborne polyurethane dispersion self made 15 Acrylic Emulsion Allnex 6801 12 Amino resin Allnex CYME1 325 6 Water-based polyester self made 12 Color paste self made 22 Wetting Agents Tego 4100 0.3 Defoaming agent BYK 024 0.1 Deionized water / 27
[0116] Table 4 Automotive water-based 1K metallic basecoat formulation
[0117]
[0118]
[0119] The electrophoresis plate was taken as the substrate, and the automotive water-based midcoat and automotive water-based 1K metallic basecoat prepared according to Table 3 and Table 4 were used. The basecoat and midcoat prepared with the water-based polyurethane dispersion of the same formula were sprayed in sequence according to the 3C1B process. The panels were sprayed and the comprehensive coating performance test results are shown in Tables 5 and 6.
[0120] Table 5 Performance test results of automotive coatings
[0121]
[0122]
[0123] Table 6 Test results of automotive coating performance
[0124]
[0125]
[0126] Adhesion (cross-cut) test is tested in accordance with GB / T 9286-2021. Impact strength is tested in accordance with GB / T 1732-2020. Stone impact resistance is tested in accordance with ISO 20567. Adhesion (high pressure water flushing) is tested in accordance with Q / JL J174007. Moisture resistance is tested in accordance with GB / T 1766 and Q / JL J174007. Water resistance, gasoline resistance, acid resistance and alkali resistance are all tested in accordance with GB / T 1766.
[0127] In Table 5, the waterborne polyurethane dispersions synthesized by Formula 1-Formula 6 are used to prepare the automotive waterborne intermediate coating and automotive waterborne 1K metallic base paint according to the formulas of Table 3 and Table 4, respectively. After spraying and making the plate according to the 3C1B process, the resulting automotive coating has a smooth appearance, adhesion (cross-cut) can reach level 0, high-pressure water impact does not fall off, stone impact resistance can reach level 1, and impact strength is higher than 35cm. In the water-resistant gasoline acid and alkali resistance test, blistering, discoloration, and adhesion can all meet the standards. In the moisture resistance test, high-pressure water flushing still does not fall off, which can meet the high standard requirements of automotive coatings for water resistance and impact resistance.
[0128] In Table 6, compared with Formula 1, Formula 7 has no post-chain extension in the aqueous polyurethane dispersion, no chain extension reaction between NCO in the polyurethane prepolymer and amino groups, and no further cross-linking reaction between the epoxy groups in the epoxy resin and amino groups, resulting in the prepared aqueous polyurethane dispersion having a lower molecular weight and a lower degree of cross-linking, and thus poor adhesion, especially when subjected to high-pressure water impact, the shedding area is >5%, which does not meet the standard. Its impact strength is also low, and its stone impact resistance only reaches Level 2. When tested for water resistance, gasoline resistance, and acid and alkali resistance, a small amount of blistering, discoloration, and shedding will occur.
[0129] Compared with Formula 1, Formula 8 has a higher R value of the waterborne polyurethane dispersion, a higher NCO content of the prepolymer, and a lower molecular weight. The resulting dispersion has a higher viscosity and a larger particle size when hydrated. The leveling property is poor when preparing the coating, and the paint film has a slight orange peel. The adhesion and flexibility are significantly deteriorated, and the corresponding impact strength is less than 30cm, which cannot meet the use requirements. Other performance indicators are worse than Formula 1.
[0130] Compared with Formulation 1, Formulation 9 does not add liquid epoxy resin during the synthesis of the aqueous polyurethane dispersion used. Therefore, there is no further reaction between epoxy and amino groups during the post-chain extension and coating application stages. The cross-linking density of the paint film is slightly lower, so the adhesion is slightly poor. The shedding area during high-pressure water impact is >5%, which does not meet the standard.
[0131] Compared with Formulation 1, Formulation 10 uses a polyester diol without short-chain side groups and branched silicon-based side groups during the synthesis of the aqueous polyurethane dispersion used. Therefore, the resulting aqueous polyurethane dispersion has extremely high viscosity, poor leveling when formulated into coatings, and obvious orange-striping on the paint film. At the same time, the lack of side groups also makes the water resistance and flexibility of the coating film worse, and the impact strength is significantly reduced. It is easy to fall off due to high-pressure water impact and cannot meet the use requirements.
[0132] Compared with Formula 1, Formula 11 uses P-2010, a product of Japan Kuraray Co., Ltd., in the synthesis of the aqueous polyurethane dispersion used, which contains short-chain side groups but no branched silicon-based side groups. Therefore, the resulting aqueous polyurethane dispersion has a slightly higher viscosity, poor leveling when preparing the coating, and a slightly orange paint film. The lack of silicon-based side groups also makes the coating slightly less water-resistant and easily falls off due to high-pressure water washing.
[0133] Compared with Formulation 1, Formulation 12 uses homemade polyester PEPL6 in the synthesis of the aqueous polyurethane dispersion used, which contains monotrimethylsiloxysilyl side groups, and has limited steric hindrance and insufficient effect on reducing viscosity. Therefore, the leveling property of the coating is slightly poor, and the paint film is slightly orange. At the same time, the improvement of the water resistance by the monosubstituted silicon-based side groups is also limited, and the high-pressure water flushing shedding area is >5%, which cannot meet the use requirements.
[0134] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. An aqueous polyurethane dispersion, characterized in that The raw materials include 20-30 parts of polymer diol, 5-15 parts of isocyanate, 1.2-4 parts of hydrophilic chain extender, 0.6-2.1 parts of epoxy resin, 1-3 parts of neutralizer, 0.01-0.05 parts of catalyst, 8-18 parts of cosolvent, 0.1-2 parts of post-chain extender and 35-75 parts of water; The raw materials of the polymer diol include a diol with short-chain side groups, a silicon-based polyester monomer and a dibasic acid (anhydride) in a molar ratio of 1:(0.1-0.4):(0.4-1.3); the short-chain side groups in the diol with short-chain side groups are C1-C3 alkyl groups.
2. The aqueous polyurethane dispersion according to claim 1, characterized in that The diol with short-chain side groups is at least one of 3-methyl-1,5-pentanediol, neopentyl glycol, 2-methyl-1,3-propanediol, 2,3-dimethyl-1,3-butanediol and 2,2,4-trimethyl-1,3-pentanediol.
3. The aqueous polyurethane dispersion according to claim 1, characterized in that The silicon-based polyester monomer contains a structural unit of Si(OSiMe3)n, where n is 2 or 3; the molar content of the silicon-based polyester monomer is 5% to 10%.
4. The aqueous polyurethane dispersion according to claim 1, characterized in that The silicon-based polyester monomer is synthesized from dialkoxysilane, trialkoxysilane and trimethylsilane end-capping agent; preferably, the silicon-based polyester monomer is end-capped with hydrogen-containing alkoxysilane and trimethylsilane end-capping agent, and then subjected to silylation with 2-vinyl-1,3-propanediol to obtain a diol monomer with branched silicon groups on the side groups; another preferred embodiment is that the silicon-based polyester monomer is end-capped with hydrogen-containing alkoxysilane and trimethylsilane end-capping agent, and then subjected to silylation with unsaturated dibasic acid (anhydride) to obtain a diacid (anhydride) monomer with branched silicon groups on the side groups; the silicon-based polyester monomer can be end-capped with epoxyalkoxysilane and trimethylsilane end-capping agent to obtain a polyester monomer with branched silicon groups on the side groups.
5. The aqueous polyurethane dispersion according to claim 4, characterized in that The hydrogen-containing alkoxysilane is one or more of trimethoxysilane, triethoxysilane, methyldimethoxysilane and methyldiethoxysilane; the epoxyalkoxysilane is 3-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(2,3-Epoxypropyloxy)propyltriethoxysilane, 2-(3,4-Epoxycyclohexane)ethyltrimethoxysilane, One or more of 2-(3,4-epoxycyclohexane)ethyltriethoxysilane, 3-(2,3-epoxypropyloxy)propylmethyldimethoxysilane, 3-(2,3-epoxypropyloxy)propylmethyldiethoxysilane, 2-(3,4-epoxycyclohexane)ethylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexane)ethylmethyldiethoxysilane; the trimethylsilyl end-capping agent is one or more of trimethylmethoxysilane, hexamethyldimethoxysilane, trimethylsilanol, and trimethylchlorosilane.
6. The aqueous polyurethane dispersion according to claim 1, characterized in that The number average molecular weight Mn of the polymer diol is 500 to 10,000; the isocyanate is at least one of isophorone diisocyanate IPDI, hexamethylene diisocyanate HDI, dicyclohexylmethane diisocyanate HMDI, toluene diisocyanate TDI, and diphenylmethane diisocyanate MDI; the hydrophilic chain extender is at least one of a dihydroxy compound containing a carboxyl group or a sulfonic acid group, polyethylene glycol, and a quaternary ammonium salt; preferably, the dihydroxy compound containing a carboxyl group or a sulfonic acid group is at least one of dimethylol propionic acid, dimethylol butyric acid, and sodium 1,4-dihydroxy-2-butane sulfonate.
7. The aqueous polyurethane dispersion according to claim 1, characterized in that The epoxy resin is a hydroxyl-containing liquid epoxy resin, preferably at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, and hydrogenated bisphenol A epoxy resin; the neutralizer is at least one of triethylamine, triethanolamine, and N,N-dimethylethanolamine DMEA; the post-chain extender is at least one of diamines, such as ethylenediamine, butanediamine, and isophoronediamine IPDA.
8. The aqueous polyurethane dispersion according to any one of claims 1 to 7, characterized in that The isocyanate index R of the aqueous polyurethane dispersion is 1.05 to 1.6; the number average molecular weight Mn of the aqueous polyurethane dispersion is 10,000 to 150,000; the acid value of the aqueous polyurethane dispersion is 5 to 12 mgKOH / g; the viscosity of the aqueous polyurethane dispersion is 10 to 2000 mPa.s; and the solid content of the aqueous polyurethane dispersion is 20 to 60%.
9. A method for preparing the aqueous polyurethane dispersion according to any one of claims 1 to 8, characterized in that: include: S1. After removing water from the polymer diol in vacuum, add isocyanate at 45-55°C, raise the temperature to 80-90°C, react; then add a hydrophilic chain extender and a catalyst, continue the reaction; then add an epoxy resin and continue the reaction; S2, cooling to 30-50°C, adding a neutralizing agent to react for 10 minutes to 1 hour, and then adding deionized water to disperse evenly under strong shearing conditions; then adding a post-chain extender, and continuing to stir and disperse for 10 minutes to 2 hours; to obtain the aqueous polyurethane dispersion.
10. Use of the aqueous polyurethane dispersion according to any one of claims 1 to 8 in the preparation of aqueous mid-coat or aqueous metallic basecoat for automobiles.