Waterborne polyurethane dipping emulsion as well as preparation method and application thereof

Through the specific ratio of water-based polyurethane impregnated latex, the problems of sewage discharge and organic solvent residue caused by water washing treatment in the production of traditional polyurethane gloves are solved, and the production of wear-resistant and environmentally friendly gloves is realized, simplifying the process flow and improving production efficiency.

CN118930804AActive Publication Date: 2024-11-12XUCHUAN CHEM SUZHOU

Patent Information

Application Number
CN202411180260.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The traditional polyurethane impregnated glove production process requires multiple washes, resulting in sewage discharge and organic solvent residue, affecting environmental protection and human health.

Method used

Using aqueous polyurethane impregnant emulsion, the emulsion with contact demulsification characteristics is formed through specific ratio prepolymers, amine-based pre-chain extenders, neutralizing agents and amine-based post-chain extenders, to avoid pretreatment of coagulants. Simplify the process flow.

Benefits of technology

The wear resistance and environmental protection of labor protection gloves are realized, the production process is simplified, and the harm of organic solvents to the human body and the environment is avoided, and the product has no odor and harmless solvent residues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930804A_ABST
    Figure CN118930804A_ABST
Patent Text Reader

Abstract

The invention provides a waterborne polyurethane dipping emulsion as well as a preparation method and application thereof. The waterborne polyurethane dipping emulsion is prepared from the following raw materials: a first prepolymer, an amine front chain extender, a neutralizer and an amine rear chain extender, the first prepolymer is prepared from the following raw material components in parts by weight: 100 parts of polytetrahydrofuran glycol, 100 to 200 parts of polypropylene oxide glycol, 5 to 7 parts of dihydroxyl-terminated polyoxyethylene polyol with a long EO side chain, 2 to 4 parts of a hydrophilic chain extender, 3 to 6 parts of a small molecule chain extender, 90 to 105 parts of diisocyanate and 0.0018 to 0.0025 part of a catalyst; the hydrophilic chain extender comprises dimethylolpropionic acid. The waterborne polyurethane dipping emulsion provided by the invention has the characteristic of contact demulsification, and the working gloves prepared from the waterborne polyurethane dipping emulsion have the characteristics of good wear resistance and environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane emulsions, and in particular relates to an aqueous polyurethane dipping emulsion and a preparation method and application thereof. Background Art

[0002] With the improvement of people's living standards, people have higher and higher requirements for the quality, comfort, and environmental protection of gloves. In recent years, polyurethane products have been recognized by people because of their lightness, softness, and wear resistance. However, the traditional polyurethane glove dipping mainly uses solvent-based polyurethane dipping to prepare labor protection gloves, and the preparation process includes dipping, washing, and drying. After the glove embryo is dipped in solvent-based polyurethane, it is necessary to replace the organic solvent in the glove embryo with water for many times. Reduce the content of organic solvents, thereby reducing the harm to the human body and the environment. However, experiments have shown that after multiple washings, DMF will still remain in the solvent-based polyurethane dipped labor protection gloves. As we all know, DMF is very harmful to the human body. Long-term contact will cause significant effects on human eyes, skin, and respiratory tract. At the same time, when washing with water, a large amount of sewage will be generated. The factory needs to recover DMF from the wastewater by distillation so that the sewage can reach the discharge index, which will undoubtedly cause a lot of energy consumption. Therefore, the production process of preparing labor protection gloves with solvent-based polyurethane dipping is a process with pollution properties and a production process with poor environmental friendliness.

[0003] As people pay more attention to the environment and health, waterborne polyurethane has gradually been recognized by people and has been widely used in many fields. Waterborne polyurethane uses water as a solvent and does not contain substances harmful to the human body. It is an environmentally friendly polymer material. Products made from waterborne polyurethane are wear-resistant, scratch-resistant, skin-friendly, and have good biocompatibility.

[0004] In the prior art, the process of preparing polyurethane dipped gloves using water-based polyurethane includes an acid coagulation process. For example, CN104479340A discloses a modified water-based polyurethane resin for labor protection gloves and a preparation method thereof. The modified water-based polyurethane resin for labor protection gloves is prepared from the following raw materials in weight percentage: 11.03% to 23.01% of a polyol compound, 3.17% to 7.06% of an isocyanate, 0.54% to 1.21% of a chain extender, 0.27% to 0.72% of a diamine, 25.21% to 45.56% of water, 0.35% to 0.91% of triethylamine, 20.83% to 42.06% of water-based acrylic acid, 1.71% to 4.54% of a modified wax emulsion, and 4.54% to 12.82% of silicon powder. This technical solution can prepare labor protection gloves by impregnating glove blanks with water-based polyurethane resin, but the glove blanks need to be pretreated with Ca(NO3)2 before impregnation, and still need to be washed with water after impregnation.

[0005] The acid coagulation process of using water-based polyurethane to produce polyurethane dipped gloves is to soak the glove blank in a layer of coagulant such as salt solution, acid solution or methanol solution in advance, so that when the glove blank is put into the water-based polyurethane for dipping, the water-based polyurethane can quickly demulsify and form a film on the surface of the glove blank, thereby preventing the water-based polyurethane from penetrating to the back of the glove and affecting the wearing comfort of the glove. In addition, after dipping, it still needs to be washed several times with water to wash out the pre-treated acid or salt, which will still produce a large amount of sewage, causing pollution to the environment and increasing costs.

[0006] Therefore, it is necessary to develop a safe and environmentally friendly water-based polyurethane dipping emulsion to solve the problem that the glove blank needs to be pretreated with a coagulant when preparing polyurethane dipped gloves with water-based polyurethane. Summary of the invention

[0007] In view of the deficiencies of the prior art, the present invention aims to provide an aqueous polyurethane dipping emulsion and a preparation method and application thereof. The aqueous polyurethane dipping emulsion has the characteristics of contact demulsification, and the labor protection gloves prepared with the aqueous polyurethane dipping emulsion have the characteristics of good wear resistance and green environmental protection, and when the labor protection gloves are prepared by dipping, it is not necessary to pre-treat the glove blank with a coagulant, and the glove blank will not penetrate into the back of the glove blank, which simplifies the preparation process of the labor protection gloves, improves production efficiency, and avoids the harm of organic solvents to the human body and the environment.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides an aqueous polyurethane dipping emulsion, wherein the raw materials for preparing the aqueous polyurethane dipping emulsion include a first prepolymer, an amine pre-chain extender, a neutralizer, and an amine post-chain extender;

[0010] The raw materials for preparing the first prepolymer include the following components in parts by weight: 100 parts of polytetrahydrofuran diol, 100-200 parts of polyoxypropylene diol (for example, 110 parts, 120 parts, 130 parts, 140 parts, 150 parts, 160 parts, 170 parts, 180 parts or 190 parts, etc.), 5-7 parts of polyoxyethylene polyol with a terminal dihydroxyl long EO side chain (for example, 5.2 parts, 5.4 parts, 5.6 parts, 5.8 parts, 6.0 parts, 6.2 parts, 6.4 parts, 6.6 parts or 6.8 parts, etc.), 2-4 parts of a hydrophilic chain extender (for example, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts, 3.0 parts, 3.2 parts, 3.4 parts, 3.6 parts or 3.8 parts, etc.), 3 to 6 parts of small molecule chain extenders (for example, 3.3 parts, 3.6 parts, 3.9 parts, 4.2 parts, 4.5 parts, 4.8 parts, 5.1 parts, 5.4 parts or 5.7 parts, etc.), 90 to 105 parts of diisocyanates (for example, 92 parts, 94 parts, 96 parts, 98 parts, 100 parts, 102 parts or 104 parts, etc.) and 0.0018 to 0.0025 parts of catalysts (for example, 0.0019 parts, 0.0020 parts, 0.0021 parts, 0.0022 parts, 0.0023 parts or 0.0024 parts, etc.); the hydrophilic chain extender includes dimethylol propionic acid (DMPA).

[0011] In the present invention, the amine pre-chain extender introduces a polyurea structure into the polyurethane molecular chain, and the polyurea structure provides certain wear resistance; the polyoxyethylene polyol with a terminal dihydroxy long EO side chain and the hydrophilic chain extender are matched with each other to form an ionic and non-ionic hydration layer, and a hydrophilic group is introduced to provide a hydrophilic effect; the specific proportion of the polyurea structure and the hydrophilic group in the aqueous polyurethane dipping emulsion ensures a certain stability of the aqueous polyurethane dipping emulsion under the condition of a large particle size, and reaches a semi-stable state, which can be packaged and stored, but the emulsification is not very stable, so that the aqueous polyurethane dipping emulsion has the characteristics of contact demulsification, and when it contacts the glove blank that has not been treated with a coagulant, it can quickly demulsify and form a membrane on the surface, thereby achieving the effect of not penetrating to the back side. The polyoxyethylene polyol or hydrophilic chain extender with dihydroxyl long EO side chain at the end of the waterborne polyurethane dipping latex is matched with each other. If the polyoxyethylene polyol or hydrophilic chain extender with dihydroxyl long EO side chain at the end is not added, the stability of the emulsion particle size will be poor. If the polyoxyethylene polyol with dihydroxyl long EO side chain at the end is not included, the stability of the emulsion particle size is very poor. In the case of large emulsion particle size, it is not enough to maintain its stability, and fusion between particles will occur. If the hydrophilic chain extender is not included, the molecular weight of the prepared polyurethane fluctuates greatly, which leads to fluctuations in the hydrophilicity of the water and layer, thereby causing fluctuations in the emulsion particle size. The emulsion particle size is unstable, sometimes the particle size is large, and sometimes the particle size is small, resulting in the emulsion's glue penetration being in an unstable state, and a waterborne polyurethane dipping latex with stable performance cannot be obtained.

[0012] In the present invention, the aqueous polyurethane dipping emulsion has the characteristics of good wear resistance and environmental protection when used for labor protection gloves, can simplify the preparation process of labor protection gloves, improve production efficiency, and avoid organic solvents from causing harm to human body and environment.

[0013] In the present invention, if the weight fraction of the polyoxyethylene polyol with dihydroxyl long EO side chain at the end is too much, the hydrophilic group content in the aqueous polyurethane dipping emulsion is too high, the emulsion particle size is small, the electric repulsion between molecules is strong, the emulsion is very stable, and the glove embryo will seep through when dipping. If the weight fraction of the polyoxyethylene polyol with dihydroxyl long EO side chain at the end is too low, the hydrophilic group content is low, the particle size is large, the electric repulsion between particles is very weak, the particles are easily fused, and the emulsion is in a very unstable state, and cannot be stably packaged and stored.

[0014] Preferably, the molar amount of the amine pre-chain extender is 20% to 60% of the molar amount of the remaining -NCO groups in the first prepolymer, such as 25%, 30%, 35%, 40%, 45%, 50% or 55%, more preferably 20% to 50%, and even more preferably 20% to 30%.

[0015] Preferably, the number average molecular weight of the polytetrahydrofuran diol is 1000-2000, for example, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800 or 1900 etc.

[0016] Preferably, the number average molecular weight of the polyoxypropylene glycol is 1000-2000, for example, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800 or 1900.

[0017] Preferably, the number average molecular weight of the polyoxyethylene polyol with terminal dihydroxy long EO side chains is 1000-2000, for example, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800 or 1900.

[0018] In the present invention, the long EO side chain means that the number average molecular weight of the EO side chain is 50 to 60, such as 51, 52, 53, 54, 55, 56, 57, 58 or 59.

[0019] Preferably, the small molecule chain extender comprises 1,4-butanediol (BDO).

[0020] Preferably, the diisocyanate includes any one of hydrogenated phenylmethane diisocyanate, 2,4-toluene diisocyanate trimer, isophorone diisocyanate or 4,4'-dicyclohexylmethane diisocyanate, or a combination of at least two thereof.

[0021] Preferably, the catalyst comprises stannous octoate.

[0022] Preferably, the amine front chain extender and the amine post chain extender each independently include an aliphatic diamine compound and / or an aliphatic polyamine compound.

[0023] Preferably, the aliphatic diamine compound includes ethylenediamine and / or isophoronediamine.

[0024] Preferably, the aliphatic polyamine compound includes diethylenetriamine and / or triethylenetetramine.

[0025] Preferably, the weight portion of the amine post-chain extender is 0.6 to 0.9 parts, such as 0.65 parts, 0.7 parts, 0.75 parts, 0.8 parts or 0.85 parts.

[0026] Preferably, the weight proportion of the neutralizing agent is 2 to 6 parts, for example, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts or 5.5 parts.

[0027] Preferably, the neutralizing agent comprises triethylamine.

[0028] Preferably, the raw materials for preparing the waterborne polyurethane dipping emulsion also include an antioxidant.

[0029] Preferably, based on the total mass of the aqueous polyurethane dipping emulsion as 100%, the mass of the antioxidant is 0.013% to 0.02%, for example, 0.014%, 0.015%, 0.016%, 0.017%, 0.018% or 0.019%.

[0030] Preferably, the raw materials for preparing the aqueous polyurethane dipping emulsion also include water.

[0031] Preferably, the water comprises deionized water.

[0032] Preferably, the solid content of the aqueous polyurethane dipping emulsion is 20% to 30%, for example, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28% or 29%, etc.

[0033] Preferably, the particle size of the aqueous polyurethane dipping emulsion is 1000-4000, for example, 1300, 1600, 1900, 2200, 2500, 2800, 3100, 3400 or 3700.

[0034] In the present invention, the emulsion particle size of the aqueous polyurethane dipping emulsion is preferably 1000-4000. If the emulsion particle size is too small, the stability of the aqueous polyurethane dipping emulsion is too good and glue penetration is likely to occur; if the emulsion particle size is too large, the stability of the aqueous polyurethane dipping emulsion is too poor, the production filterability is poor, and the production and storage stability requirements are not met.

[0035] In a second aspect, the present invention provides a method for preparing the aqueous polyurethane dipping emulsion as described in the first aspect, the preparation method comprising the following steps:

[0036] (1) mixing polytetrahydrofuran diol, polyoxypropylene diol, polyoxyethylene polyol with a terminal dihydroxyl long EO side chain, a hydrophilic chain extender, a small molecule chain extender, a diisocyanate and a catalyst, and reacting them to prepare a first prepolymer;

[0037] (2) mixing the first prepolymer obtained in step (1) and an amine pre-chain extender, and reacting them to obtain a second prepolymer;

[0038] (3) mixing the second prepolymer obtained in step (2) with a neutralizing agent, and reacting them to obtain a third prepolymer;

[0039] (4) mixing the third prepolymer obtained in step (3) and the amine post-chain extender, and reacting them to obtain the waterborne polyurethane dipped latex.

[0040] Preferably, the step (1) specifically comprises the following steps: mixing polytetrahydrofuran diol, polyoxypropylene diol, polyoxyethylene polyol with a terminal dihydroxy long EO side chain, and a hydrophilic chain extender, vacuum drying and dehydrating for 1 to 2 hours (for example, 1.1 hours, 1.2 hours, 1.3 hours, 1.4 hours, 1.5 hours, 1.6 hours, 1.7 hours, 1.8 hours, or 1.9 hours, etc.), adding a small molecule chain extender, an organic solvent, a diisocyanate, and a catalyst, and reacting at 60 to 65° C. (for example, 60.5° C., 61° C., 61.5° C., 62° C., 62.5° C., 63° C., 63.5° C., 64° C., or 64.5° C., etc.) for 2 to 3 hours (for example, 2.1 hours, 2.2 hours, 2.3 hours, 2.4 hours, 2.5 hours, 2.6 hours, 2.7 hours, 2.8 hours, or 2.9 hours, etc.), to prepare a first prepolymer.

[0041] Preferably, the vacuum drying and dehydration in step (1) is carried out under the conditions of 95-105°C (for example, 96°C, 97°C, 98°C, 99°C, 100°C, 101°C, 102°C, 103°C or 104°C, etc.) and 0.05-0.2MPa (for example, 0.07MPa, 0.09MPa, 0.011MPa, 0.013MPa, 0.015MPa, 0.017MPa or 0.019MPa, etc.).

[0042] Preferably, the mass ratio of the small molecule chain extender to the organic solvent in step (1) is 1:(10-15), for example, 1:10.5, 1:11, 1:11.5, 1:12, 1:12.5, 1:13, 1:13.5, 1:14 or 1:14.5, and more preferably 1:(10-12).

[0043] Preferably, the mixing in step (2) further comprises mixing with an organic solvent.

[0044] Preferably, the reaction temperature in step (2) is 40-45°C (e.g., 40.5°C, 41°C, 41.5°C, 42°C, 42.5°C, 43°C, 43.5°C, 44°C or 44.5°C, etc.), and the reaction time is 15-30 min (e.g., 17 min, 19 min, 21 min, 23 min, 25 min, 27 min or 29 min, etc.).

[0045] Preferably, the mass ratio of the organic solvent to the amine pre-chain extender in step (2) is 60:(0.9-10.1), for example 60:1, 60:2, 60:3, 60:4, 60:5, 60:6, 60:7, 60:8, 60:9 or 60:10, etc.

[0046] Preferably, the step (3) specifically comprises the following steps: cooling the second prepolymer obtained in step (2) to 15-35° C. (e.g., 17° C., 19° C., 21° C., 23° C., 25° C., 27° C., 29° C., 31° C., or 33° C., etc.), adding an organic solvent and a neutralizing agent to mix, reacting for 3-7 minutes (e.g., 3.5 minutes, 4 minutes, 4.5 minutes, 5 minutes, 5.5 minutes, 6 minutes, or 6.5 minutes, etc.), and then adding water to mix to obtain a third prepolymer;

[0047] Preferably, the mass ratio of the organic solvent to the neutralizer in step (3) is (40-50):(2-6), for example, 41:5, 42:5, 43:5, 44:4, 45:4, 46:4, 47:3, 48:3 or 49:3, etc.

[0048] Preferably, the mass ratio of water to neutralizing agent in step (3) is (1000-1300):(2-6), for example, 1000:5, 1050:5, 1100:4, 1150:4, 1200:4, 1250:4 or 1300:4, etc.

[0049] Preferably, the step (4) specifically comprises mixing an aqueous solution formed by mixing an amine post-chain extender and water, and then mixing and reacting with the third prepolymer obtained in step (3) to obtain the waterborne polyurethane dipping latex.

[0050] Preferably, the mass ratio of water to amine post-chain extender in the aqueous solution of step (4) is (15-25):(0.6-0.9), for example, 16:0.9, 17:0.9, 18:0.8, 19:0.8, 20:0.7, 21:0.7, 22:0.7, 23:0.6 or 24:0.6, etc.

[0051] Preferably, the reaction temperature in step (4) is 45-50°C (e.g., 45.5°C, 46°C, 46.5°C, 47°C, 47.5°C, 48°C, 48.5°C, 49°C or 49.5°C, etc.), and the reaction time is 20-40 min (e.g., 22 min, 24 min, 26 min, 28 min, 30 min, 32 min, 34 min, 36 min or 38 min, etc.).

[0052] Preferably, after the reaction in step (4), the process further comprises the steps of removing the organic solvent and adding water to adjust the solid content.

[0053] Preferably, the preparation method specifically comprises the following steps:

[0054] (1) Polytetrahydrofuran diol, polyoxypropylene diol, polyoxyethylene polyol with a terminal dihydroxyl long EO side chain, and a hydrophilic chain extender are mixed, vacuum dried and dehydrated at 95-105° C. and 0.05-0.2 MPa for 1-2 h, a small molecule chain extender, a diisocyanate, and a catalyst are added, and the mixture is reacted at 60-65° C. for 2-3 h to prepare a first prepolymer.

[0055] (2) The first prepolymer prepared in step (1), an amine pre-chain extender and an organic solvent are mixed at 40 to 45° C. for 15 to 30 minutes to obtain a second prepolymer.

[0056] (3) The second prepolymer prepared in step (2) is cooled to 15-35° C., an organic solvent and a neutralizing agent are added and mixed, and then water is added and mixed, and the mixture is reacted for 3-7 minutes to obtain a third prepolymer.

[0057] (4) mixing an aqueous solution formed by mixing an amine post-chain extender and water with the third prepolymer obtained in step (3), reacting at 45 to 50° C. for 20 to 40 minutes, removing the organic solvent, and adding water to adjust the solid content to obtain the aqueous polyurethane dipping latex.

[0058] Preferably, the organic solvent comprises acetone.

[0059] In the present invention, by adopting the preparation method and controlling the reaction conditions of steps (1) to (4), an aqueous polyurethane emulsion with moderate emulsion particle size and alkalinity can be prepared.

[0060] In a third aspect, the present invention provides a use of the aqueous polyurethane dipping emulsion as described in the first aspect in the preparation of labor protection gloves.

[0061] Compared with the prior art, the present invention has the following beneficial effects:

[0062] In the present invention, the components and contents of polytetrahydrofuran diol, polyoxypropylene diol, polyoxyethylene polyol with dihydroxyl long EO side chain at the end, hydrophilic chain extender, small molecule chain extender, diisocyanate, amine pre-chain extender, etc. are matched, so that the labor protection gloves prepared by the aqueous polyurethane dipping emulsion have the characteristics of softness and wear resistance, can meet the market demand for wear resistance level 4, and have durability and comfort. The aqueous polyurethane dipping emulsion has the characteristics of contact demulsification, and can quickly demulsify and form a film on the surface when contacting the glove embryo that has not been treated with a coagulant, and the glove embryo does not need to be pretreated with a coagulant, and the situation of glue penetration will not occur. After dipping, water washing is not required, which simplifies the preparation process of the labor protection gloves, improves production efficiency, and avoids the harm of organic solvents to the human body and the environment. The labor protection gloves made by dipping the aqueous polyurethane dipping emulsion are completely odorless, without any harmful solvent residue, and are healthier and safer. After the water-based polyurethane dipping emulsion is slightly thickened, the storage stability of the water-based polyurethane dipping emulsion can reach more than 6 months, and no premature demulsification will occur before the dipping construction, and the stability is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 The present invention provides a flow chart of preparing labor protection gloves using an aqueous polyurethane dipping emulsion according to a specific embodiment of the present invention. DETAILED DESCRIPTION

[0064] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0065] Example 1

[0066] The present embodiment provides an aqueous polyurethane dipped latex and a preparation method thereof. The raw materials for preparing the aqueous polyurethane dipped latex include the following components by weight: 100 parts of polytetrahydrofuran diol (number average molecular weight is 1000), 200 parts of polyoxypropylene diol (number average molecular weight is 2000), 5 parts of polyoxyethylene polyol with a terminal dihydroxyl long EO side chain (manufacturer is Pasto, brand name is ymer120), 5 parts of a hydrophilic chain extender ( The aqueous polyurethane dipping latex comprises 3 parts of dihydroxymethylpropionic acid), 5 parts of a small molecule chain extender (1,4-butanediol), 90 parts of hydrogenated phenylmethane diisocyanate, 5 parts of 2,4-toluene diisocyanate trimer, 0.0018 parts of a catalyst (stannous octoate), 3.34 parts of an amine pre-chain extender (isophoronediamine), 6 parts of a neutralizer (triethylamine), 0.9 parts of an amine post-chain extender (ethylenediamine) and deionized water, wherein the solid content of the aqueous polyurethane dipping latex is 25%.

[0067] The preparation method comprises the following steps:

[0068] (1) adding 100 parts by weight of polytetrahydrofuran diol, 200 parts by weight of polyoxypropylene diol, 5 parts by weight of polyoxyethylene polyol having a terminal dihydroxyl long EO side chain, and 3 parts by weight of a hydrophilic chain extender into a reaction kettle, heating the mixture to 100° C. while stirring, vacuum drying and dehydrating the mixture at 0.1 MPa for 2 h, then cooling the mixture to 50° C., adding 5 parts by weight of a small molecule chain extender, 50 parts by weight of acetone, 90 parts by weight of hydrogenated phenylmethane diisocyanate, 5 parts by weight of 2,4-toluene diisocyanate trimer, and 0.0018 parts by weight of a catalyst under normal pressure, and reacting the mixture at 62° C. for 3 h to prepare a first prepolymer;

[0069] (2) detecting the actual value of the molar amount of the remaining -NCO groups in the first prepolymer obtained in step (1), cooling the first prepolymer obtained in step (1) to 40° C., adding 3.34 parts by weight of an amine pre-chain extender and 60 parts by weight of acetone to the mixture, wherein the molar amount of the amine pre-chain extender is 20% of the molar amount of the remaining -NCO groups in the first prepolymer, and reacting for 30 minutes under stirring at 100 r / min to obtain a second prepolymer;

[0070] (3) cooling the second prepolymer obtained in step (2) to 30° C., adding 50 parts by weight of acetone and 6 parts by weight of a neutralizer, stirring at 100 r / min, reacting for 5 min, adding 1300 parts by weight of deionized water, stirring at 1500 r / min, and mixing to form a milky white emulsion, thereby obtaining a third prepolymer;

[0071] (4) adding an aqueous solution formed by mixing 0.9 parts by weight of an amine post-chain extender and 20 parts by weight of deionized water to the third prepolymer prepared in step (3), reacting at 45° C. and 800 r / min for 30 min to complete the chain extension reaction, and finally removing the acetone under vacuum under reduced pressure (the pressure is controlled at 0.05 MPa and the temperature is 50° C.), adding deionized water, and controlling the solid content to 25%, to obtain the aqueous polyurethane dipped latex.

[0072] Example 2

[0073] This embodiment provides an aqueous polyurethane dipped latex and a preparation method thereof, which differs from Embodiment 1 only in that the weight portion of the amine pre-chain extender (isophorone diamine) is adjusted to 5.01 parts, and the molar amount of the amine pre-chain extender in step (2) is 30% of the molar amount of the remaining -NCO groups in the first prepolymer, and other conditions are the same as in Embodiment 1.

[0074] Example 3

[0075] This embodiment provides an aqueous polyurethane dipped latex and a preparation method thereof, which differs from Embodiment 1 only in that the weight fraction of the amine pre-chain extender (isophorone diamine) is adjusted to 6.69 parts, and the molar amount of the amine pre-chain extender in step (2) is 40% of the molar amount of the remaining -NCO groups in the first prepolymer, and other conditions are the same as those in Embodiment 1.

[0076] Example 4

[0077] This embodiment provides an aqueous polyurethane dipped latex and a preparation method thereof, which differs from Embodiment 1 only in that the weight fraction of the amine pre-chain extender (isophorone diamine) is adjusted to 8.36 parts, and the molar amount of the amine pre-chain extender in step (2) is 50% of the molar amount of the remaining -NCO groups in the first prepolymer, and other conditions are the same as those in Embodiment 1.

[0078] Example 5

[0079] This embodiment provides an aqueous polyurethane dipped latex and a preparation method thereof, which differs from Embodiment 1 only in that the weight portion of the amine pre-chain extender (isophorone diamine) is adjusted to 10.03 parts, and the molar amount of the amine pre-chain extender in step (2) is 60% of the molar amount of the remaining -NCO groups in the first prepolymer, and other conditions are the same as in Embodiment 1.

[0080] Example 6

[0081] This embodiment provides an aqueous polyurethane dipping emulsion and a preparation method thereof, which is different from Example 1 only in that the weight fraction of the polyoxyethylene polyol with terminal dihydroxy long EO side chain is adjusted to 6 parts, and other conditions are the same as Example 1.

[0082] Example 7

[0083] This embodiment provides an aqueous polyurethane dipping emulsion and a preparation method thereof, which is different from Example 1 only in that the weight fraction of the polyoxyethylene polyol with terminal dihydroxy long EO side chain is adjusted to 7 parts, and other conditions are the same as Example 1.

[0084] Example 8

[0085] This embodiment provides an aqueous polyurethane dipping emulsion and a preparation method thereof, which differs from Example 1 only in that 3.34 parts by weight of an amine pre-chain extender (isophorone diamine) is replaced with 1.178 parts by weight of an amine pre-chain extender (ethylene diamine) of the same molar amount, and other conditions are the same as in Example 1.

[0086] Example 9

[0087] This embodiment provides an aqueous polyurethane dipping emulsion and a preparation method thereof, which is different from Embodiment 1 only in that the weight fraction of polyoxypropylene glycol is adjusted to 100 parts, and other conditions are the same as those of Embodiment 1.

[0088] Example 10

[0089] The present embodiment provides an aqueous polyurethane dipping emulsion and a preparation method thereof. The raw materials for preparing the aqueous polyurethane dipping emulsion include the following components in parts by weight: 100 parts of polytetrahydrofuran diol (number average molecular weight of 1000), 150 parts of polyoxypropylene diol (number average molecular weight of 2000), 5 parts of polyoxyethylene polyol with a terminal dihydroxy long EO side chain (manufacturer is Pasto, brand name is ymer120), 3 parts of a hydrophilic chain extender (dimethylol propionic acid), 4 parts of a small molecule chain extender (1,4-butanediol), 95 parts of isophorone diisocyanate, 0.0018 parts of a catalyst (stannous octoate), 4 parts of an amine pre-chain extender (isophorone diamine), 2.26 parts of a neutralizer (triethylamine), 0.9 parts of an amine post-chain extender (ethylenediamine) and deionized water. The solid content of the aqueous polyurethane dipping emulsion is 20%.

[0090] The preparation method comprises the following steps:

[0091] (1) adding 100 parts by weight of polytetrahydrofuran diol, 150 parts by weight of polyoxypropylene diol, 5 parts by weight of polyoxyethylene polyol having a terminal dihydroxyl long EO side chain, and 3 parts by weight of a hydrophilic chain extender into a reaction kettle, heating the mixture to 100° C. under stirring, vacuum drying and dehydration at 0.1 MPa for 2 h, then cooling the mixture to 50° C., adding 4 parts by weight of a small molecule chain extender, 50 parts by weight of acetone, 95 parts by weight of isophorone diisocyanate, and 0.0018 parts by weight of a catalyst under normal pressure, and reacting the mixture at 65° C. for 2 h to prepare a first prepolymer;

[0092] (2) detecting the actual value of the molar amount of the remaining -NCO groups in the first prepolymer obtained in step (1), cooling the first prepolymer obtained in step (1) to 45° C., adding 4 parts by weight of an amine pre-chain extender and 60 parts by weight of acetone to the mixture, wherein the molar amount of the amine pre-chain extender is 20% of the molar amount of the remaining -NCO groups in the first prepolymer, and reacting for 15 minutes under stirring at 100 r / min to obtain a second prepolymer;

[0093] (3) cooling the second prepolymer obtained in step (2) to 25° C., adding 50 parts by weight of acetone and 2.26 parts by weight of a neutralizer, stirring at 100 r / min, reacting for 5 min, adding 1300 parts by weight of deionized water, stirring at 1500 r / min, and mixing to form a milky white emulsion, thereby obtaining a third prepolymer;

[0094] (4) adding an aqueous solution of 0.9 parts by weight of an amine post-chain extender and 20 parts by weight of deionized water to the third prepolymer obtained in step (3), reacting at 45° C. and 800 r / min for 30 min under stirring to complete the post-chain extension reaction, and finally removing the acetone under vacuum under reduced pressure (the pressure was controlled at 0.05 MPa and the temperature was 50° C.), adding deionized water, and controlling the solid content to 20%, thereby obtaining the aqueous polyurethane dipped latex.

[0095] Embodiment 11

[0096] The present embodiment provides an aqueous polyurethane dipped latex and a preparation method thereof. The raw materials for preparing the aqueous polyurethane dipped latex include the following components in parts by weight: 100 parts of polytetrahydrofuran diol (number average molecular weight is 2000), 150 parts of polyoxypropylene diol (number average molecular weight is 1000), 5 parts of polyoxyethylene polyol with a terminal dihydroxyl long EO side chain (manufacturer is Pasto, brand name is ymer120), 4 parts of a hydrophilic chain extender (dimethylol propionic acid), and 100 parts of polyoxyethylene glycol (number average molecular weight is 1000). 6 parts of molecular chain extender (1,4-butanediol), 100 parts of isophorone diisocyanate, 5 parts of 2,4-toluene diisocyanate trimer, 0.002 parts of catalyst (stannous octoate), 5.01 parts of amine pre-chain extender (isophorone diamine), 3.02 parts of neutralizer (triethylamine), 0.68 parts of amine post-chain extender (diethylenetriamine), 0.2 parts of antioxidant (antioxidant 62TP) and deionized water, the solid content of the aqueous polyurethane dipping emulsion is 30%.

[0097] The preparation method comprises the following steps:

[0098] (1) adding 100 parts by weight of polytetrahydrofuran diol, 150 parts by weight of polyoxypropylene diol, 5 parts by weight of polyoxyethylene polyol having a terminal dihydroxyl long EO side chain, and 4 parts by weight of a hydrophilic chain extender into a reaction kettle, heating the mixture to 100° C. under stirring, vacuum drying and dehydration at 0.1 MPa for 2 h, then cooling the mixture to 50° C., adding 6 parts by weight of a small molecule chain extender, 60 parts by weight of acetone, 100 parts by weight of isophorone diisocyanate, 5 parts by weight of 2,4-toluene diisocyanate trimer, and 0.002 parts by weight of a catalyst under normal pressure, and reacting the mixture at 65° C. for 2 h to prepare a first prepolymer;

[0099] (2) detecting the actual value of the molar amount of the remaining -NCO groups in the first prepolymer obtained in step (1), cooling the first prepolymer obtained in step (1) to 45° C., adding 5.01 parts by weight of an amine pre-chain extender and 60 parts by weight of acetone to the mixture, wherein the molar amount of the amine pre-chain extender is 30% of the molar amount of the remaining -NCO groups in the first prepolymer, and reacting for 20 minutes under stirring at 100 r / min to obtain a second prepolymer;

[0100] (3) cooling the second prepolymer obtained in step (2) to 25° C., adding 50 parts by weight of acetone and 3.02 parts by weight of a neutralizer, stirring at 100 r / min, reacting for 5 min, adding 1000 parts by weight of deionized water, stirring at 1500 r / min, and mixing to form a milky white emulsion, thereby obtaining a third prepolymer;

[0101] (4) adding an aqueous solution of 0.68 parts by weight of an amine post-chain extender and 20 parts by weight of deionized water to the third prepolymer obtained in step (3), reacting at 50° C. and 800 r / min for 30 min under stirring to complete the post-chain extension reaction, and finally removing the acetone under vacuum under reduced pressure (the pressure was controlled at 0.05 MPa and the temperature was 50° C.), adding deionized water and an antioxidant, and controlling the solid content to 30%, thereby obtaining the aqueous polyurethane dipped latex.

[0102] Comparative Example 1

[0103] This comparative example provides an aqueous polyurethane dipping emulsion and a preparation method thereof, which differs from Example 1 only in that the weight fraction of the polyoxyethylene polyol with terminal dihydroxy long EO side chains is adjusted to 8 parts, and other conditions are the same as those in Example 1.

[0104] Comparative Example 2

[0105] This comparative example provides an aqueous polyurethane dipping emulsion and a preparation method thereof, which is different from Example 1 only in that no amine pre-chain extender is added, and other conditions are the same as those in Example 1.

[0106] Comparative Example 3

[0107] This comparative example provides an aqueous polyurethane dipping emulsion and a preparation method thereof, which differs from Example 1 only in that the hydrophilic chain extender (dihydroxymethylpropionic acid) is replaced with a hydrophilic chain extender (dihydroxymethylbutyric acid) of the same mass, and other conditions are the same as those in Example 1.

[0108] Comparative Example 4

[0109] This comparative example provides a water-based polyurethane dipping emulsion, manufactured by Asahikawa Chemical, with a brand name of XCWB-8510.

[0110] Comparative Example 5

[0111] This comparative example provides an aqueous polyurethane dipping emulsion and a preparation method thereof, which differs from Example 1 only in that no polyoxyethylene polyol with a terminal dihydroxy long EO side chain is added, the weight portion of the hydrophilic chain extender (dihydroxymethylpropionic acid) is adjusted to 8 parts, and other conditions are the same as Example 1.

[0112] The aqueous polyurethane dipping emulsions provided in the above embodiments and comparative examples were tested, and the specific testing method is as follows:

[0113] (1) Emulsion particle size: Dilute the water-based polyurethane latex with water at a ratio of 1:100, and then use a laser particle size analyzer to measure the emulsion particle size.

[0114] (2) Production filterability: Use a 150-mesh filter to filter. If 1 kg of emulsion can be filtered within 1 minute, it is recorded as filterable. If 1 kg of emulsion can be filtered within 1-2 minutes, it is recorded as barely filterable. If 1 kg of emulsion cannot be filtered within 1-2 minutes, it is recorded as unfilterable.

[0115] (3) Glue penetration: The woven polyester glove blank (13-gauge) was placed in an oven and heated to 60°C. It was then directly immersed in a water-based polyurethane dipping emulsion to observe whether the glove blank would undergo glue penetration. If there was a large area of ​​glue inside the glove core, it was recorded as glue penetration. If there were only a few glue spots inside the glove core, it was recorded as slight glue penetration. If there was no glue inside the glove core, it was recorded as no glue penetration.

[0116] (4) Young's modulus: The aqueous polyurethane latex was scraped onto a flat release paper with a coating thickness of 30 μm and dried to prepare a polyurethane film. The Young's modulus was measured according to GB / T 1040.3-2006.

[0117] (5) Wear resistance test and hand feel evaluation: The woven polyester glove blank (13 needles) was preheated in an 80°C oven. When the woven polyester glove blank was preheated to 40°C, it was immersed in the water-based polyurethane dipping emulsion and homogenized for 10 seconds. Then, it was placed in an 80°C oven and heated for 30 minutes. Finally, it was placed in a 100°C oven and heated for 65 minutes to fix the shape. The labor protection gloves were obtained. The process flow chart is shown in the figure. Figure 1As shown, then the wear resistance test and hand feel evaluation were carried out;

[0118] Abrasion test: According to EN388:2003 standard, Martindale abrasion tester is used for testing;

[0119] Feel evaluation: 5 testers judge the softness of the gloves and give scores respectively. The softness score is 1-3 points. The higher the softness, the higher the score, and the harder the feel, the lower the score. After scoring, the average score is taken as the final score n. 0≤n<1 is recorded as hard, 1≤n<2 is recorded as relatively hard, and 2≤n<3 is recorded as soft.

[0120] (6) Stability: Use thickener 220 (manufacturer Huashengyuan) to thicken the water-based polyurethane latex to a viscosity of 2000 mPa·s (25°C), and then use a release machine to centrifuge it at 3000 r / min for 15 minutes. If there is no material-water separation phenomenon, the storage time is considered to be ≥ 6 months, otherwise the storage time is < 6 months.

[0121] The test results are shown in Table 1 below.

[0122] Table 1

[0123]

[0124] In Table 1, “-” means that the test was not performed.

[0125] As can be seen from the contents of Table 1, the aqueous polyurethane dipping emulsions provided in Examples 1-11 have the characteristics of contact demulsification. When contacting the glove blanks that have not been treated with a coagulant, they can quickly demulsify and form a film on the surface, without or only slightly penetrating the glue, and the glove blanks do not need to be pretreated with a coagulant, which can meet the market demand for wear resistance level 4. After a slight amount of thickening, the storage stability of the aqueous polyurethane dipping emulsion can reach more than 6 months, and premature demulsification will not occur before dipping construction.

[0126] Compared with Example 1, it can be seen that if the molar amount of the amine pre-chain extender is too large as a percentage of the molar amount of the remaining -NCO group in the first prepolymer (Example 5), the molecular weight of the polyurethane in the obtained aqueous polyurethane dipping emulsion is large, and the proportion of hydrophilic groups in the polyurethane is reduced, resulting in a poor emulsification effect, which makes it impossible to filter and does not meet the production requirements.

[0127] Compared with Example 1, it can be seen that if the weight fraction of the polyoxyethylene polyol with terminal dihydroxy long EO side chain is too large (Comparative Example 1), the particle size of the prepared aqueous polyurethane dipping emulsion is small and the glue is permeable.

[0128] Compared with Example 1, it can be seen that if no amine pre-chain extender is added (Comparative Example 2), then at the same hydrophilic group content, the emulsion particle size is small and the glue is transparent. Although it feels soft, the abrasion resistance is very low and does not meet the requirements.

[0129] Compared with Example 1, it can be seen that if dimethylolpropionic acid is replaced with dimethylolbutyric acid of the same mass (Comparative Example 3), the obtained water-based polyurethane dipping emulsion is permeable to the glue because the hydrophilicity of dimethylolbutyric acid is better than that of dimethylolpropionic acid.

[0130] Compared with Comparative Example 4, the gloves prepared by the aqueous polyurethane dipping emulsion provided in Examples 1-11 of the present invention have higher wear resistance. The reason is that the polyurea structure introduced by the amine pre-chain extender provides good wear resistance. The present invention makes the hard segment and the soft segment ratio reasonably matched by matching the components in the aqueous polyurethane dipping emulsion, so that the feel of the prepared labor protection gloves is basically the same as the feel of the labor protection gloves prepared by the aqueous polyurethane dipping emulsion sold on the market.

[0131] Compared with Example 1, it can be seen that if the polyoxyethylene polyol with a terminal dihydroxy long EO side chain is not added (Comparative Example 5), the stability of the prepared aqueous polyurethane dipping emulsion is very poor. When the particle size is large, it is not enough to maintain its stability, fusion between ions will occur, and the storage stability cannot reach 6 months.

[0132] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A water-based polyurethane dipping emulsion, characterized in that: The raw materials for preparing the waterborne polyurethane dipped latex include a first prepolymer, an amine pre-chain extender, a neutralizer and an amine post-chain extender; The raw materials for preparing the first prepolymer include the following components in parts by weight: 100 parts of polytetrahydrofuran diol, 100-200 parts of polyoxypropylene diol, 5-7 parts of polyoxyethylene polyol with terminal dihydroxy long EO side chain, 2-4 parts of hydrophilic chain extender, 3-6 parts of small molecule chain extender, 90-105 parts of diisocyanate and 0.0018-0.0025 parts of catalyst; the hydrophilic chain extender includes dimethylol propionic acid.

2. The aqueous polyurethane dipping emulsion according to claim 1, characterized in that: The molar amount of the amine pre-chain extender is 20% to 60% of the molar amount of the remaining -NCO groups in the first prepolymer; Preferably, the number average molecular weight of the polytetrahydrofuran diol is 1000 to 2000; Preferably, the number average molecular weight of the polyoxypropylene glycol is 1000 to 2000; Preferably, the number average molecular weight of the polyoxyethylene polyol having a terminal dihydroxy long EO side chain is 1000-2000.

3. The aqueous polyurethane dipping emulsion according to claim 1 or 2, characterized in that: The small molecule chain extender includes 1,4-butanediol; Preferably, the diisocyanate includes any one or a combination of at least two of hydrogenated phenylmethane diisocyanate, 2,4-toluene diisocyanate trimer, isophorone diisocyanate or 4,4'-dicyclohexylmethane diisocyanate; Preferably, the catalyst comprises stannous octoate.

4. The aqueous polyurethane dipping emulsion according to any one of claims 1 to 3, characterized in that: The amine front chain extender and the amine post chain extender each independently include an aliphatic diamine compound and / or an aliphatic polyamine compound; Preferably, the aliphatic diamine compound includes ethylenediamine and / or isophoronediamine; Preferably, the aliphatic polyamine compound includes diethylenetriamine and / or triethylenetetramine; Preferably, the weight portion of the amine post-chain extender is 0.6 to 0.9 parts; Preferably, the weight proportion of the neutralizing agent is 2 to 6 parts; Preferably, the neutralizing agent comprises triethylamine.

5. The aqueous polyurethane dipping emulsion according to any one of claims 1 to 4, characterized in that: The raw materials for preparing the waterborne polyurethane dipping latex also include an antioxidant; Preferably, based on the total mass of the aqueous polyurethane dipping emulsion being 100%, the mass of the antioxidant is 0.013% to 0.02%; Preferably, the raw materials for preparing the waterborne polyurethane dipping emulsion also include water; Preferably, the water comprises deionized water; Preferably, the solid content of the aqueous polyurethane dipping emulsion is 20% to 30%; Preferably, the particle size of the aqueous polyurethane dipping emulsion is 1000-4000 nm.

6. A method for preparing the aqueous polyurethane dipping emulsion according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) mixing polytetrahydrofuran diol, polyoxypropylene diol, polyoxyethylene polyol with a terminal dihydroxyl long EO side chain, a hydrophilic chain extender, a small molecule chain extender, a diisocyanate and a catalyst, and reacting them to prepare a first prepolymer; (2) mixing the first prepolymer obtained in step (1) and an amine pre-chain extender, and reacting them to obtain a second prepolymer; (3) mixing the second prepolymer obtained in step (2) with a neutralizing agent, and reacting them to obtain a third prepolymer; (4) mixing the third prepolymer obtained in step (3) and the amine post-chain extender, and reacting them to obtain the waterborne polyurethane dipped latex.

7. The preparation method according to claim 6, characterized in that: The step (1) specifically comprises the following steps: mixing polytetrahydrofuran diol, polyoxypropylene diol, polyoxyethylene polyol with a terminal dihydroxyl long EO side chain, and a hydrophilic chain extender, vacuum drying and dehydrating for 1 to 2 hours, adding a small molecule chain extender, an organic solvent, a diisocyanate and a catalyst, and reacting at 60 to 65° C. for 2 to 3 hours to prepare a first prepolymer; Preferably, the vacuum drying and dehydration in step (1) is carried out at 95-105° C. and 0.05-0.2 MPa; Preferably, the mass ratio of the small molecule chain extender to the organic solvent in step (1) is 1:(10-15); Preferably, the mixing in step (2) further comprises mixing with an organic solvent; Preferably, the reaction temperature in step (2) is 40-45°C and the reaction time is 15-30 min; Preferably, the mass ratio of the organic solvent to the amine pre-chain extender in step (2) is 60:(0.9-10.1).

8. The preparation method according to claim 6 or 7, characterized in that: The step (3) specifically comprises the following steps: cooling the second prepolymer obtained in step (2) to 15-35° C., adding an organic solvent and a neutralizing agent, mixing, reacting for 3-7 minutes, and then adding water and mixing to obtain a third prepolymer; Preferably, the mass ratio of the organic solvent to the neutralizing agent in step (3) is (40-50):(2-6); Preferably, the mass ratio of water to neutralizing agent in step (3) is (1000-1300):(2-6); Preferably, the step (4) specifically comprises mixing an aqueous solution formed by mixing an amine post-chain extender and water, and then mixing and reacting with the third prepolymer obtained in step (3) to obtain the aqueous polyurethane dipped latex; Preferably, the mass ratio of water to amine post-chain extender in the aqueous solution of step (4) is (15-25): (0.6-0.9); Preferably, the reaction temperature in step (4) is 45-50°C and the reaction time is 20-40 min; Preferably, after the reaction in step (4), the process further comprises the steps of removing the organic solvent and adding water to adjust the solid content.

9. The preparation method according to any one of claims 6 to 8, characterized in that: The preparation method specifically comprises the following steps: (1) mixing polytetrahydrofuran diol, polyoxypropylene diol, polyoxyethylene polyol with a terminal dihydroxyl long EO side chain, and a hydrophilic chain extender, vacuum drying and dehydrating for 1 to 2 hours at 95 to 105° C. and 0.05 to 0.2 MPa, adding a small molecule chain extender, a diisocyanate, and a catalyst, and reacting at 60 to 65° C. for 2 to 3 hours to prepare a first prepolymer; (2) mixing the first prepolymer obtained in step (1), an amine pre-chain extender and an organic solvent, and reacting at 40 to 45° C. for 15 to 30 minutes to obtain a second prepolymer; (3) cooling the second prepolymer obtained in step (2) to 15-35° C., adding an organic solvent and a neutralizing agent, mixing, reacting for 3-7 minutes, and then adding water and mixing to obtain a third prepolymer; (4) mixing an aqueous solution formed by mixing an amine post-chain extender and water with the third prepolymer obtained in step (3), reacting at 45 to 50° C. for 20 to 40 minutes, removing the organic solvent, and adding water to adjust the solid content to obtain the aqueous polyurethane dipped latex; Preferably, the organic solvent comprises acetone.

10. Use of the aqueous polyurethane dipping emulsion according to any one of claims 1 to 5 in the preparation of labor protection gloves.

Citation Information

Patent Citations

  • Production method for liner gloves aqueous polyurethane coating connection material

    CN101328383A

  • Aqueous polyurethane-polyurea polyol dispersion and preparation method thereof

    CN107955126A

  • Water-based polyurethane dispersion and preparation method and application thereof

    CN108192072A

  • Poly(carbonic ester-ether) type polyurethane emulsion for printing paste and preparation method thereof

    CN108330712A

  • Cationic polyurethane-polyurea water dispersion, and preparation method and application thereof

    CN109957087A

Cited By

  • Narrow-particle-size high-crystallinity nonionic waterborne polyurethane and preparation method thereof

    CN121824912A

  • Coagulant-free aqueous polyurethane emulsion for rubber-impregnated work protective equipment and method for producing the same

    JP7898791B1