Surface-modified crosslinked polystyrene insulator and preparation method thereof

By grafting high-voltage resistance characteristic molecular groups on the surface of crosslinked polystyrene insulators to form a flexible two-dimensional molecular film structure, the problem of low vacuum along the plane flashover voltage in the prior art is solved, and significant increase and stability of the withstand voltage is achieved , suitable for a variety of electric field conditions.

CN118930939APending Publication Date: 2024-11-12NORTHWEST INST OF NUCLEAR TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411043792.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing surface modification methods cannot prepare chemical components with high vacuum along-plane flashover voltage on the surface of crosslinked polystyrene insulators, and the voltage resistance level is low and unstable.

Method used

Using high pressure resistance characteristics molecular groups, such as long-chain alkyl, carbon fluorogen or delocalized electron groups, grafting onto the surface of cross-linked polystyrene insulators through nitration, reductive amination and acylation reactions, to form a flexible two-dimensional The molecular membrane structure reduces the secondary electron emission coefficient and gas adsorption amount.

Benefits of technology

It significantly improves the vacuum pressure resistance performance of cross-linked polystyrene insulators, and the pressure resistance improvement level is high and stable. It is suitable for various electric field conditions. The chemical connection between molecular groups and the insulator body is stable, avoiding the Reduced mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972990100000101
    Figure BDA0004972990100000101
  • Figure BDA0004972990100000111
    Figure BDA0004972990100000111
  • Figure HDA0004972990110000011
    Figure HDA0004972990110000011
Patent Text Reader

Abstract

The invention provides a surface-modified crosslinked polystyrene insulator and a preparation method thereof, and can solve the problems that chemical components with high vacuum surface flashover voltage cannot be prepared on the surface of the crosslinked polystyrene insulator by the existing surface modification method, and the voltage resistance improvement level is low and unstable. The insulator comprises a cross-linked polystyrene insulator body and a high-voltage-resistant molecular group grafted on the surface of the cross-linked polystyrene insulator body, the high-voltage-resistant molecular groups form a flexible two-dimensional molecular film structure on the surface of the crosslinked polystyrene insulator body, and the flexible two-dimensional molecular film structure is used for reducing the secondary electron emission coefficient and the gas adsorption capacity of the surface of the crosslinked polystyrene insulator body. The preparation method of the insulator comprises the following steps: preparing the crosslinked polystyrene insulator body, and then sequentially carrying out nitration reaction, reductive amination reaction and acylation reaction. Or preparing a crosslinked polystyrene insulator body, and then directly carrying out acylation reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an insulator and a preparation method thereof, in particular to a surface-modified cross-linked polystyrene insulator and a preparation method thereof. Background Art

[0002] As a vacuum insulation material with low dielectric constant, low dielectric loss, high bulk breakdown voltage and excellent mechanical properties, cross-linked polystyrene is widely used in high voltage devices. However, the interface between cross-linked polystyrene and vacuum will experience breakdown discharge at a voltage far lower than the voltage between the insulator bulk and vacuum, resulting in insulation failure. This phenomenon is called vacuum surface flashover. Vacuum surface flashover will greatly reduce the withstand voltage of the insulating material surface, making it the most vulnerable area in high voltage devices. In addition, vacuum surface flashover is also a bottleneck problem faced by high voltage vacuum devices. At present, it is generally believed that the emission and multiplication of secondary electrons on the insulator surface and the desorption of gas adsorbed on the surface stimulated by electrons are important processes in the formation of surface flashover. Reducing the emission of secondary electrons and the amount of gas adsorbed on the insulator surface can effectively increase the surface flashover voltage (see: Li S, Nie Y, Min D, et al. Research Progress on Vacuum Surface Flashover of Solid Dielectrics[J]. Transactions of China Electrotechnical Society. 2017, 32(8): 1-9. Zhang GJ, Zhao WB, Zheng N, et al. Research Progress on Surface Flashover Phenomena Across Solid Insulation in Vacuum[J]. High Voltage Engineering. 2007, 33(30): 30-35.). Since the secondary electron emission coefficient (SEY) and the amount of surface gas adsorption are determined by the surface state of the insulator, in order to reduce the secondary electron emission coefficient and the amount of gas adsorption and increase the vacuum surface flashover voltage, the method of chemical modification on the surface of the insulator is usually adopted to change the surface state of the insulator, thereby changing the secondary electron emission coefficient and the amount of gas adsorption.

[0003] Commonly used methods for chemical modification of vacuum insulator surfaces include fluorination (including direct gas fluorination, plasma-assisted fluorination, and fluorination of fluorine-containing organic molecules), coating preparation, plasma treatment, ion implantation, etc. (see: Zhang C, Ma Y, Kong F, et al. Atmospheric pressure plasmas and direct fluorination treatment of Al2O3-filled epoxy resin: A comparison of surface charge dissipation [J]. Surface & Coatings Technology. 2019, 362: 1-11. Xie, Dongri, Lin, et al. Surface flashover performance of epoxy resin microcomposites improved by electron beam irradiation [J]. Applied Surface Science. 2017.). Through these methods, a variety of chemical components are modified onto the surface of vacuum insulators. However, since the relationship between the surface molecular structure and the vacuum surface withstand voltage characteristics of the insulator has not yet been established, it is unknown which surface chemical composition can effectively improve the vacuum surface flashover voltage of the insulator. Therefore, the existing surface modification methods cannot prepare chemical compositions with high vacuum surface flashover voltage on the surface of cross-linked polystyrene insulators, and the withstand voltage improvement level is low and unstable. Summary of the invention

[0004] The purpose of the present invention is to solve the technical problems that the existing surface modification method cannot prepare chemical components with high vacuum surface flashover voltage on the surface of cross-linked polystyrene insulators, and the withstand voltage improvement level is low and unstable, and to provide a surface modified cross-linked polystyrene insulator and a preparation method thereof.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] A surface-modified cross-linked polystyrene insulator, which is special in that:

[0007] It comprises a cross-linked polystyrene insulator body and a high voltage-withstand molecular group grafted on the surface of the cross-linked polystyrene insulator body; the high voltage-withstand molecular group is a high voltage-withstand molecular group that can be grafted on the surface of the cross-linked polystyrene insulator body according to the chemical reaction characteristics of the cross-linked polystyrene; the high voltage-withstand molecular group forms a flexible two-dimensional molecular film structure on the surface of the cross-linked polystyrene insulator body, which is used to reduce the secondary electron emission coefficient and gas adsorption amount on the surface of the cross-linked polystyrene insulator body.

[0008] Furthermore, the high voltage resistance molecular group is a long-chain alkyl group, a carbon fluoride group or a delocalized electron group.

[0009] At the same time, the present invention also provides a method for preparing the surface-modified cross-linked polystyrene insulator, which is special in that it comprises the following steps:

[0010] Step 1, preparing a cross-linked polystyrene insulator body;

[0011] Step 2: Nitration reaction

[0012] Step 2.1, according to the volume ratio of concentrated HNO3 to concentrated H2SO4 of 10:2 to 10:3, respectively measure 65% by mass of concentrated HNO3 and 98% by mass of concentrated H2SO4, add concentrated H2SO4 to concentrated HNO3, stir until the mixture is uniform, and prepare a mixed acid;

[0013] Step 2.2, placing the cross-linked polystyrene insulator body prepared in step 1 into the mixed acid prepared in step 2.1, stirring and reacting at room temperature for at least 1 hour to obtain a nitrated cross-linked polystyrene insulator;

[0014] Step 2.3, washing and drying the cross-linked polystyrene insulator after nitration in step 2.2;

[0015] Step 3: Reductive amination reaction

[0016] Step 3.1, placing the dried cross-linked polystyrene insulator in step 2.3 into a reaction container, adding concentrated hydrochloric acid with a mass fraction of 36% to 38% into the reaction container, weighing zinc particles or iron powder and adding them into the reaction container in a ratio of 4g to 6g of mass volume of zinc particles or iron powder to concentrated hydrochloric acid: 25mL, stirring and reacting for 4h to 6h at room temperature to obtain a cross-linked polystyrene insulator after reductive amination;

[0017] Step 3.2, washing and drying the cross-linked polystyrene insulator after reductive amination in step 3.1;

[0018] Step 4: Acylation reaction

[0019] Step 4.1, placing the cross-linked polystyrene insulator dried in step 3.2 into a non-polar organic solvent, adding an acylating agent in a ratio of 1 g to 2 g of the mass volume of the non-polar organic solvent to 100 mL, stirring and reacting for at least 30 minutes at room temperature, to obtain a cross-linked polystyrene insulator with a high withstand voltage molecular group grafted on the surface;

[0020] Step 4.2: Wash and dry the cross-linked polystyrene insulator obtained in step 4.1 to complete the preparation of the surface-modified cross-linked polystyrene insulator.

[0021] Further, in step 2.1, concentrated H2SO4 is added dropwise to concentrated HNO3;

[0022] In step 2.2, the reaction is stirred for 1 h to 4 h using a magnetic stirrer;

[0023] Step 2.3 is specifically as follows: placing the cross-linked polystyrene insulator after nitration in step 2.2 into deionized water, ultrasonically washing for at least 30 minutes, and then drying at 50° C. to 80° C. for at least 12 hours;

[0024] In step 3.1, the volume of the concentrated hydrochloric acid is the same as the volume of the mixed acid; the zinc particles are weighed and added to the reaction container one by one according to a mass volume ratio of zinc particles to concentrated hydrochloric acid of 4 g to 6 g: 25 mL;

[0025] In step 3.2, the specific process of cleaning and drying is the same as the specific process of cleaning and drying in step 2.3.

[0026] Furthermore, step 1 specifically includes, by means of mechanical processing, making the cross-linked polystyrene insulating material into a cross-linked polystyrene insulator body with a preset geometric structure and size;

[0027] In step 4.1, the reaction is stirred for at least 30 minutes and then allowed to stand for at least 6 hours; the volume of the non-polar organic solvent is the same as the volume of the mixed acid;

[0028] The non-polar organic solvent is n-octane, toluene or chloroform; the acylating agent is octadecyl chloride, perfluoroundecyl chloride, perfluorooctyl chloride or phenethyl chloride;

[0029] Step 4.2 specifically comprises washing the cross-linked polystyrene insulator obtained in step 4.1 with tap water, placing it in deionized water, ultrasonically washing it for at least 30 minutes, and then drying it at 50° C. to 80° C. for at least 12 hours to complete the preparation of the surface-modified cross-linked polystyrene insulator.

[0030] Further, in step 2.1, the volume ratio of concentrated HNO3 to concentrated H2SO4 is 10:2.5;

[0031] In step 2.2, the reaction was stirred for 3 h using a magnetic stirrer;

[0032] Step 2.3 is specifically as follows: placing the cross-linked polystyrene insulator after nitration in step 2.2 into deionized water, ultrasonically washing for 30 minutes, and then drying at 80° C. for 12 hours;

[0033] In step 3.1, the mass fraction of the concentrated hydrochloric acid is 36.5%; the mass volume ratio of the zinc particles to the concentrated hydrochloric acid is 4g:25mL; the stirring reaction time is 5h;

[0034] Step 4.1 is specifically as follows: putting the cross-linked polystyrene insulator dried in step 3.2 into n-octane with the same volume as the mixed acid, adding phenethyl chloride in a ratio of 1 g:100 mL by mass volume of phenethyl chloride to n-octane, stirring the reaction for 30 min at room temperature and then standing for 6 h to obtain a cross-linked polystyrene insulator with phenethyl grafted on the surface;

[0035] In step 4.2, the ultrasonic washing time is 30 min, the drying temperature is 80° C., and the drying time is 12 h.

[0036] At the same time, the present invention also provides another method for preparing the surface-modified cross-linked polystyrene insulator, which is special in that it comprises the following steps:

[0037] Step 1, preparing a cross-linked polystyrene insulator body;

[0038] Step 2: Acylation reaction

[0039] Step 2.1, placing the cross-linked polystyrene insulator body prepared in step 1 into a non-polar organic solvent, adding an acylating agent according to a mass volume ratio of 1g to 2g of the acylating agent to the non-polar organic solvent: 100mL, adding anhydrous aluminum chloride according to a mass volume ratio of 1g to 2g of anhydrous aluminum chloride to the non-polar organic solvent: 50mL, stirring the reaction at room temperature for at least 2h, and obtaining a cross-linked polystyrene insulator with a high withstand voltage molecular group grafted on the surface;

[0040] Step 2.2: Wash and dry the cross-linked polystyrene insulator obtained in step 2.1 to complete the preparation of the surface-modified cross-linked polystyrene insulator.

[0041] Further, in step 2.1, the reaction is stirred for at least 2 hours and then allowed to stand for at least 12 hours;

[0042] The non-polar organic solvent is n-octane, toluene or chloroform; the acylating agent is octadecyl chloride, perfluoroundecyl chloride, perfluorooctyl chloride or phenethyl chloride;

[0043] Step 2.2 specifically comprises washing the cross-linked polystyrene insulator obtained in step 2.1 with tap water, placing it in deionized water, ultrasonically washing it for at least 30 minutes, and then drying it at 50° C. to 80° C. for at least 12 hours to complete the preparation of the surface-modified cross-linked polystyrene insulator.

[0044] Further, step 2.1 is specifically, placing the cross-linked polystyrene insulator body prepared in step 1 into n-octane, adding octadecyl chloride in a ratio of 1 g: 100 mL of mass volume of octadecyl chloride to n-octane, adding anhydrous aluminum chloride in a ratio of 1 g: 50 mL of mass volume of anhydrous aluminum chloride to n-octane, stirring the reaction for 2 hours at room temperature and then standing for 12 hours to obtain a cross-linked polystyrene insulator with octadecyl grafted on the surface;

[0045] In step 2.2, the ultrasonic washing time is 30 min, the drying temperature is 80° C., and the drying time is 12 h.

[0046] Furthermore, step 1 is specifically as follows:

[0047] The cross-linked polystyrene insulating material is made into a cross-linked polystyrene insulator body with a preset geometric structure and size by mechanical processing.

[0048] Beneficial effects of the present invention:

[0049] 1. The present invention provides a surface-modified cross-linked polystyrene insulator. High-voltage withstand molecular groups are grafted on the surface of the insulator body, which can improve the vacuum surface withstand voltage performance of the cross-linked polystyrene insulator. The voltage resistance improvement level is high and stable, which can be regarded as improving the intrinsic withstand voltage performance of the insulator. The insulator is suitable for insulators under various electric field conditions.

[0050] 2. The present invention also provides a method for preparing surface-modified cross-linked polystyrene insulators. According to the chemical reaction characteristics of cross-linked polystyrene, a suitable molecular modification path is adopted to directly graft high-voltage-withstand molecular groups onto the surface of the cross-linked polystyrene insulator body to improve the vacuum surface voltage-withstand performance of the cross-linked polystyrene insulator. The method has strong purpose and high voltage-withstand strength improvement.

[0051] 3. In the present invention, the high withstand voltage molecular group is chemically connected to the insulator body, the combination is firm, will not change over time, and has high stability.

[0052] 4. The present invention adopts liquid phase reaction conditions, and chemical reactions can occur at the contact positions between the cross-linked polystyrene insulator body and the liquid phase, so that the grafted high-voltage molecular groups are evenly distributed and the flashover voltage is stably increased; in addition, the liquid phase reaction conditions are applicable to insulators of various shapes.

[0053] 5. In the present invention, the molecular groups with high withstand voltage characteristics are grafted onto the surface of the cross-linked polystyrene insulator body without destroying the bulk structure of the insulator, and the mechanical strength of the insulator can be ensured. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 This is a schematic diagram of a reaction route of a preparation method of the surface-modified cross-linked polystyrene insulator of the present invention (R represents a molecular group with high withstand voltage characteristics);

[0055] Figure 2 This is a schematic diagram of the reaction route of another preparation method of the surface-modified cross-linked polystyrene insulator of the present invention (R represents a molecular group with high withstand voltage characteristics). DETAILED DESCRIPTION

[0056] Embodiment 1

[0057] A surface-modified cross-linked polystyrene insulator comprises a cross-linked polystyrene insulator body and a high-voltage-withstand molecular group grafted on the surface of the cross-linked polystyrene insulator body. The high-voltage-withstand molecular group is a high-voltage-withstand molecular group that can be grafted on the surface of the cross-linked polystyrene insulator body according to the chemical reaction characteristics of the cross-linked polystyrene. Driven by intermolecular forces, the high-voltage-withstand molecular group is regularly arranged on the surface of the cross-linked polystyrene insulator body to form a flexible two-dimensional molecular film structure. Since the molecular groups of the structure can swing and adjust spontaneously within a certain range, it has a certain flexibility. The flexible two-dimensional molecular film structure can give the insulator surface higher stability and reduce the adsorption of gas molecules, that is, it can reduce the secondary electron emission coefficient and gas adsorption amount on the surface of the cross-linked polystyrene insulator body, thereby inhibiting the development of vacuum surface flashover on the surface of the cross-linked polystyrene insulator and improving the vacuum surface withstand voltage performance of the cross-linked polystyrene insulator. The high-voltage-withstand molecular group is a molecular group such as a long-chain alkyl group, a carbon fluoride group or a delocalized electron group that can reduce the secondary electron emission coefficient and gas adsorption amount on the surface of the insulator and improve the vacuum surface withstand voltage characteristics of the insulator. In this embodiment, the high voltage resistance molecular group is a delocalized electron group.

[0058] like Figure 1 As shown, a method for preparing the above-mentioned surface-modified cross-linked polystyrene insulator comprises the following steps:

[0059] Step 1: By means of mechanical processing, the cross-linked polystyrene insulating material is made into a cross-linked polystyrene insulator body with a thickness of 5 mm and a diameter of 30 mm.

[0060] Step 2: Nitration reaction

[0061] Step 2.1, according to the volume ratio of concentrated HNO3 to concentrated H2SO4 of 10:2.5, respectively measure 40mL of concentrated HNO3 with a mass fraction of 65% and 10mL of concentrated H2SO4 with a mass fraction of 98%, add the concentrated H2SO4 dropwise into the concentrated HNO3, stirring while adding until the mixture is uniform, to obtain a mixed acid;

[0062] Step 2.2, placing the cross-linked polystyrene insulator body prepared in step 1 into the mixed acid prepared in step 2.1, stirring and reacting for 3 hours at room temperature using a magnetic method, to obtain a nitrated cross-linked polystyrene insulator;

[0063] Step 2.3: Place the cross-linked polystyrene insulator after nitration in step 2.2 into deionized water, perform ultrasonic washing for 30 minutes, and then dry it in an oven at 80° C. for 12 hours.

[0064] Step 3: Reductive amination reaction

[0065] Step 3.1, putting the cross-linked polystyrene insulator dried in step 2.3 into a reaction container, adding 50 mL of concentrated hydrochloric acid with a mass fraction of 36.5% into the reaction container, weighing 8 g of zinc particles and adding them into the reaction container one by one according to the mass volume ratio of zinc particles to concentrated hydrochloric acid of 4 g: 25 mL, stirring and reacting for 5 hours at room temperature to obtain a cross-linked polystyrene insulator after reductive amination;

[0066] Step 3.2, cleaning and drying the cross-linked polystyrene insulator after reductive amination in step 3.1; the specific process of cleaning and drying in this step is the same as the specific process of cleaning and drying in step 2.3.

[0067] Step 4: Acylation reaction

[0068] Step 4.1, placing the cross-linked polystyrene insulator dried in step 3.2 into 50 mL of n-octane, adding 0.5 g of phenethyl chloride in a ratio of 1 g:100 mL of mass volume of phenethyl chloride to n-octane, stirring the reaction for 30 min at room temperature and then standing for 6 h to obtain a cross-linked polystyrene insulator with phenethyl grafted on the surface;

[0069] Step 4.2: Wash the cross-linked polystyrene insulator obtained in step 4.1 with a large amount of tap water to quench the phenylethyl chloride, then put it into deionized water, ultrasonically wash it for 30 minutes, and use an oven at 80°C for 12 hours to complete the preparation of the surface-modified cross-linked polystyrene insulator, which is recorded as "phenylethyl grafted cross-linked polystyrene insulator 1".

[0070] Embodiment 2

[0071] The difference between the surface-modified cross-linked polystyrene insulator in this embodiment and the surface-modified cross-linked polystyrene insulator in the first embodiment is that the molecular group with high withstand voltage characteristics is a long-chain alkyl group.

[0072] like Figure 2 As shown, this embodiment also provides another method for preparing a surface-modified cross-linked polystyrene insulator, comprising the following steps:

[0073] Step 1: By means of mechanical processing, the cross-linked polystyrene insulating material is made into a cross-linked polystyrene insulator body with a thickness of 5 mm and a diameter of 30 mm.

[0074] Step 2: Acylation reaction

[0075] Step 2.1, the cross-linked polystyrene insulator body prepared in step 1 is placed in 50 mL of n-octane, 0.5 g of octadecyl chloride is added according to the mass volume ratio of octadecyl chloride to n-octane of 1 g: 100 mL, and 1 g of anhydrous aluminum chloride is added according to the mass volume ratio of anhydrous aluminum chloride to n-octane of 1 g: 50 mL for catalysis, and the reaction is stirred for 2 hours at room temperature and then allowed to stand for 12 hours, and the phenyl groups on the cross-linked polystyrene molecular chain are directly acylated to obtain a cross-linked polystyrene insulator with octadecyl grafted on the surface;

[0076] Step 2.2, wash the cross-linked polystyrene insulator obtained in step 2.1 with a large amount of tap water, quench anhydrous aluminum chloride and octadecyl chloride, then put it into deionized water, ultrasonically wash it for 30 minutes, and dry it at 80°C for 12 hours; complete the preparation of the surface-modified cross-linked polystyrene insulator, recorded as "octadecyl grafted cross-linked polystyrene insulator 2".

[0077] Embodiment 3

[0078] The difference between the surface-modified cross-linked polystyrene insulator in this embodiment and the surface-modified cross-linked polystyrene insulator in the first embodiment is that the molecular group with high withstand voltage characteristics is a long-chain alkyl group.

[0079] The difference between the preparation method of the surface-modified cross-linked polystyrene insulator in this embodiment and the preparation method of the surface-modified cross-linked polystyrene insulator in the first embodiment is that:

[0080] In step 2.1, the volume ratio of concentrated HNO3 to concentrated H2SO4 is 10:2, the volume of concentrated HNO3 is 40 mL, and the volume of concentrated H2SO4 is 8 mL.

[0081] In step 2.2, the stirring reaction time is 1 h.

[0082] In step 2.3, the ultrasonic washing time is 35 min, the temperature is 65° C., and the drying time is 12.5 h.

[0083] Step 3.1 is specifically as follows: the cross-linked polystyrene insulator dried in step 2.3 is placed in a reaction container, 48 mL of concentrated hydrochloric acid with a mass fraction of 37.5% is added to the reaction container, and 9.6 g of iron powder is weighed and added to the reaction container at one time according to the mass volume ratio of iron powder to concentrated hydrochloric acid of 5 g:25 mL. Under room temperature conditions, the reaction is stirred for 6 hours to obtain the cross-linked polystyrene insulator after reductive amination.

[0084] Step 4.1 is specifically as follows: the cross-linked polystyrene insulator dried in step 3.2 is placed in 48 mL of toluene, 0.72 g of octadecyl chloride is added in a ratio of 1.5 g:100 mL of octadecyl chloride to toluene by mass volume, and the reaction is stirred for 35 min at room temperature and then allowed to stand for 6.5 h to obtain a cross-linked polystyrene insulator with octadecyl grafted on the surface.

[0085] In step 4.2, the ultrasonic washing time is 35 min, the temperature is 65° C., and the drying time is 12.5 h, which is recorded as “octadecyl grafted cross-linked polystyrene insulator 3”.

[0086] Embodiment 4

[0087] The difference between the surface-modified cross-linked polystyrene insulator in this embodiment and the surface-modified cross-linked polystyrene insulator in the first embodiment is that the molecular group with high withstand voltage characteristics is a carbon-fluorine group.

[0088] The difference between the preparation method of the surface-modified cross-linked polystyrene insulator in this embodiment and the preparation method of the surface-modified cross-linked polystyrene insulator in the first embodiment is that:

[0089] In step 2.1, the volume ratio of concentrated HNO3 to concentrated H2SO4 is 10:3, the volume of concentrated HNO3 is 40 mL, and the volume of concentrated H2SO4 is 12 mL.

[0090] In step 2.2, the stirring reaction time is 4 h.

[0091] In step 2.3, the temperature is 50°C and the drying time is 13h.

[0092] Step 3.1 is specifically as follows: the cross-linked polystyrene insulator dried in step 2.3 is placed in a reaction container, 52 mL of concentrated hydrochloric acid with a mass fraction of 38% is added to the reaction container, 12.48 g of zinc particles are weighed and added to the reaction container one by one according to the mass volume ratio of iron powder to concentrated hydrochloric acid of 6 g:25 mL, and the reaction is stirred for 4 hours at room temperature to obtain the cross-linked polystyrene insulator after reductive amination.

[0093] Step 4.1 is specifically as follows: the cross-linked polystyrene insulator dried in step 3.2 is placed in 52 mL of chloroform, 1.04 g of perfluorooctyl chloride is added in a ratio of 2 g:100 mL of mass volume of perfluorooctyl chloride to chloroform, and the reaction is stirred for 30 min at room temperature and then allowed to stand for 6 h to obtain a cross-linked polystyrene insulator with perfluorooctyl grafted on the surface. In other embodiments, the perfluorooctyl chloride in this step can be replaced by perfluoroundecyl chloride.

[0094] In step 4.2, the temperature is 50° C. and the drying time is 13 h, which is recorded as “perfluorooctyl grafted cross-linked polystyrene insulator 4”.

[0095] Embodiment 5

[0096] The difference between the surface-modified cross-linked polystyrene insulator in this embodiment and the surface-modified cross-linked polystyrene insulator in the second embodiment is that the molecular group with high withstand voltage characteristics is a carbon-fluorine group.

[0097] The difference between the preparation method of the surface-modified cross-linked polystyrene insulator in this embodiment and the preparation method of the surface-modified cross-linked polystyrene insulator in the second embodiment is that:

[0098] Step 2.1 is specifically as follows: the cross-linked polystyrene insulator body prepared in step 1 is placed in 50 mL of toluene, 0.75 g of perfluoroundecyl chloride is added in a ratio of 1.5 g:100 mL of the mass volume ratio of perfluoroundecyl chloride to toluene, 1.5 g of anhydrous aluminum chloride is added for catalysis in a ratio of 1.5 g:50 mL of the mass volume ratio of anhydrous aluminum chloride to toluene, and the reaction is stirred for 2.5 hours at room temperature and then allowed to stand for 12.5 hours to directly acylate the phenyl groups on the cross-linked polystyrene molecular chain to obtain a cross-linked polystyrene insulator with perfluoroundecyl grafted on the surface. In other embodiments, the perfluoroundecyl chloride in this step can be replaced by perfluorooctyl chloride.

[0099] In step 2.2, the ultrasonic washing time is 35 min, the temperature is 65° C., and the drying time is 12.5 h, which is recorded as “perfluoroundecyl grafted cross-linked polystyrene insulator 5”.

[0100] Embodiment 6

[0101] The difference between the surface-modified cross-linked polystyrene insulator in this embodiment and the surface-modified cross-linked polystyrene insulator in the second embodiment is that the molecular group with high withstand voltage characteristic is a delocalized electron group.

[0102] The difference between the preparation method of the surface-modified cross-linked polystyrene insulator in this embodiment and the preparation method of the surface-modified cross-linked polystyrene insulator in the second embodiment is that:

[0103] Step 2.1 is specifically as follows: the cross-linked polystyrene insulator body prepared in step 1 is placed in 50 mL of chloroform, 1 g of phenethyl chloride is added in a ratio of 2 g:100 mL of the mass volume ratio of phenethyl chloride to chloroform, and 2 g of anhydrous aluminum chloride is added for catalysis in a ratio of 2 g:50 mL of the mass volume ratio of anhydrous aluminum chloride to chloroform. Under room temperature conditions, the reaction is stirred for 2 hours and then allowed to stand for 12 hours to directly acylate the phenyl groups on the cross-linked polystyrene molecular chain to obtain a cross-linked polystyrene insulator with phenethyl grafted on the surface.

[0104] In step 2.2, the temperature is 50° C. and the drying time is 13 h, which is recorded as “phenylethyl grafted cross-linked polystyrene insulator 6”.

[0105] The cross-linked polystyrene insulators with high withstand voltage molecular groups grafted on the surface prepared in the above examples 1 to 6 and the cross-linked polystyrene insulator bodies were subjected to vacuum surface flashover voltage tests on a vacuum surface flashover voltage test bench with a pulse width of 500ns. The flashover voltage test results are shown in Table 1.

[0106] Table 1

[0107]

[0108]

[0109] As can be seen from Table 1, the flashover voltage of the insulator grafted with high-voltage-withstand molecular groups of the present invention is increased by 30% to 40% compared with the cross-linked polystyrene insulator body, which shows that the high-voltage-withstand molecular groups of the present invention are grafted on the surface of the cross-linked polystyrene insulator body, which can effectively increase the flashover voltage of the cross-linked polystyrene insulator.

[0110] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A surface-modified cross-linked polystyrene insulator, characterized in that: It comprises a cross-linked polystyrene insulator body and a high voltage-withstand molecular group grafted on the surface of the cross-linked polystyrene insulator body; the high voltage-withstand molecular group is a high voltage-withstand molecular group that can be grafted on the surface of the cross-linked polystyrene insulator body according to the chemical reaction characteristics of the cross-linked polystyrene; the high voltage-withstand molecular group forms a flexible two-dimensional molecular film structure on the surface of the cross-linked polystyrene insulator body, which is used to reduce the secondary electron emission coefficient and gas adsorption amount on the surface of the cross-linked polystyrene insulator body.

2. The surface-modified cross-linked polystyrene insulator according to claim 1, characterized in that: The high voltage resistance molecular group is a long-chain alkyl group, a carbon fluoride group or a delocalized electron group.

3. A method for preparing the surface-modified cross-linked polystyrene insulator according to claim 1 or 2, characterized in that: The following steps are involved: Step 1, preparing a cross-linked polystyrene insulator body; Step 2: Nitration reaction Step 2.1, according to the volume ratio of concentrated HNO3 to concentrated H2SO4 of 10:2 to 10:3, respectively measure 65% by mass of concentrated HNO3 and 98% by mass of concentrated H2SO4, add concentrated H2SO4 to concentrated HNO3, stir until the mixture is uniform, and prepare a mixed acid; Step 2.2, placing the cross-linked polystyrene insulator body prepared in step 1 into the mixed acid prepared in step 2.1, stirring and reacting at room temperature for at least 1 hour to obtain a nitrated cross-linked polystyrene insulator; Step 2.3, washing and drying the cross-linked polystyrene insulator after nitration in step 2.2; Step 3: Reductive amination reaction Step 3.1, placing the dried cross-linked polystyrene insulator in step 2.3 into a reaction container, adding concentrated hydrochloric acid with a mass fraction of 36% to 38% into the reaction container, weighing zinc particles or iron powder and adding them into the reaction container in a ratio of 4g to 6g of mass volume of zinc particles or iron powder to concentrated hydrochloric acid: 25mL, stirring and reacting for 4h to 6h at room temperature to obtain a cross-linked polystyrene insulator after reductive amination; Step 3.2, washing and drying the cross-linked polystyrene insulator after reductive amination in step 3.1; Step 4: Acylation reaction Step 4.1, placing the cross-linked polystyrene insulator dried in step 3.2 into a non-polar organic solvent, adding an acylating agent in a ratio of 1 g to 2 g of the mass volume of the non-polar organic solvent to 100 mL, stirring and reacting for at least 30 minutes at room temperature, to obtain a cross-linked polystyrene insulator with a high withstand voltage molecular group grafted on the surface; Step 4.2: Wash and dry the cross-linked polystyrene insulator obtained in step 4.1 to complete the preparation of the surface-modified cross-linked polystyrene insulator.

4. The method for preparing the surface-modified cross-linked polystyrene insulator according to claim 3, characterized in that: In step 2.1, concentrated H2SO4 is added dropwise to concentrated HNO3; In step 2.2, the reaction is stirred for 1 h to 4 h using a magnetic stirrer; Step 2.3 is specifically as follows: placing the cross-linked polystyrene insulator after nitration in step 2.2 into deionized water, ultrasonically washing for at least 30 minutes, and then drying at 50° C. to 80° C. for at least 12 hours; In step 3.1, the volume of the concentrated hydrochloric acid is the same as the volume of the mixed acid; the zinc particles are weighed and added to the reaction container one by one according to a mass volume ratio of zinc particles to concentrated hydrochloric acid of 4 g to 6 g: 25 mL; In step 3.2, the specific process of cleaning and drying is the same as the specific process of cleaning and drying in step 2.

3.

5. The method for preparing the surface-modified cross-linked polystyrene insulator according to claim 4, characterized in that: Step 1 specifically includes, by means of mechanical processing, making the cross-linked polystyrene insulating material into a cross-linked polystyrene insulator body with a preset geometric structure and size; In step 4.1, the reaction is stirred for at least 30 minutes and then allowed to stand for at least 6 hours; the volume of the non-polar organic solvent is the same as the volume of the mixed acid; The non-polar organic solvent is n-octane, toluene or chloroform; the acylating agent is octadecyl chloride, perfluoroundecyl chloride, perfluorooctyl chloride or phenethyl chloride; Step 4.2 specifically comprises washing the cross-linked polystyrene insulator obtained in step 4.1 with tap water, placing it in deionized water, ultrasonically washing it for at least 30 minutes, and then drying it at 50° C. to 80° C. for at least 12 hours to complete the preparation of the surface-modified cross-linked polystyrene insulator.

6. The method for preparing the surface-modified cross-linked polystyrene insulator according to claim 5, characterized in that: In step 2.1, the volume ratio of concentrated HNO3 to concentrated H2SO4 is 10:2.5; In step 2.2, the reaction was stirred for 3 h using a magnetic stirrer; Step 2.3 is specifically as follows: placing the cross-linked polystyrene insulator after nitration in step 2.2 into deionized water, ultrasonically washing for 30 minutes, and then drying at 80° C. for 12 hours; In step 3.1, the mass fraction of the concentrated hydrochloric acid is 36.5%; the mass volume ratio of the zinc particles to the concentrated hydrochloric acid is 4g:25mL; the stirring reaction time is 5h; Step 4.1 is specifically as follows: putting the cross-linked polystyrene insulator dried in step 3.2 into n-octane with the same volume as the mixed acid, adding phenethyl chloride in a ratio of 1 g:100 mL by mass volume of phenethyl chloride to n-octane, stirring the reaction for 30 min at room temperature and then standing for 6 h to obtain a cross-linked polystyrene insulator with phenethyl grafted on the surface; In step 4.2, the ultrasonic washing time is 30 min, the drying temperature is 80° C., and the drying time is 12 h.

7. A method for preparing the surface-modified cross-linked polystyrene insulator according to claim 1 or 2, characterized in that: The following steps are involved: Step 1, preparing a cross-linked polystyrene insulator body; Step 2: Acylation reaction Step 2.1, placing the cross-linked polystyrene insulator body prepared in step 1 into a non-polar organic solvent, adding an acylating agent according to a mass volume ratio of 1g to 2g of the acylating agent to the non-polar organic solvent: 100mL, adding anhydrous aluminum chloride according to a mass volume ratio of 1g to 2g of anhydrous aluminum chloride to the non-polar organic solvent: 50mL, stirring the reaction at room temperature for at least 2h, and obtaining a cross-linked polystyrene insulator with a high withstand voltage molecular group grafted on the surface; Step 2.2: Wash and dry the cross-linked polystyrene insulator obtained in step 2.1 to complete the preparation of the surface-modified cross-linked polystyrene insulator.

8. The method for preparing the surface-modified cross-linked polystyrene insulator according to claim 7, characterized in that: In step 2.1, the reaction was stirred for at least 2 h and then allowed to stand for at least 12 h; The non-polar organic solvent is n-octane, toluene or chloroform; the acylating agent is octadecyl chloride, perfluoroundecyl chloride, perfluorooctyl chloride or phenethyl chloride; Step 2.2 specifically comprises washing the cross-linked polystyrene insulator obtained in step 2.1 with tap water, placing it in deionized water, ultrasonically washing it for at least 30 minutes, and then drying it at 50° C. to 80° C. for at least 12 hours to complete the preparation of the surface-modified cross-linked polystyrene insulator.

9. The method for preparing the surface-modified cross-linked polystyrene insulator according to claim 8, characterized in that: Step 2.1 is specifically, placing the cross-linked polystyrene insulator body prepared in step 1 into n-octane, adding octadecyl chloride in a ratio of 1 g:100 mL by mass volume of octadecyl chloride to n-octane, adding anhydrous aluminum chloride in a ratio of 1 g:50 mL by mass volume of anhydrous aluminum chloride to n-octane, stirring the reaction for 2 hours at room temperature and then standing for 12 hours to obtain a cross-linked polystyrene insulator with octadecyl grafted on the surface; In step 2.2, the ultrasonic washing time is 30 min, the drying temperature is 80° C., and the drying time is 12 h.

10. The method for preparing the surface-modified cross-linked polystyrene insulator according to claim 9, characterized in that: Step 1 is as follows: The cross-linked polystyrene insulating material is made into a cross-linked polystyrene insulator body with a preset geometric structure and size by mechanical processing.