PVC (polyvinyl chloride) composite material for pipes and preparation method of PVC composite material
By using functional fibers and high-temperature resistant components in PVC pipes, the high temperature and toughness of PVC pipes are improved, the problems of softening and deformation under high temperature conditions are solved, and the application safety and reliability of their power pipes are improved in the field of power pipes. .
Patent Information
- Application Number
- CN202411239317.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-12
AI Technical Summary
PVC pipes are not durable under high temperature conditions, are prone to softening and deforming, and have poor toughness, which limits their application scope, especially in the field of power pipes.
Using functional fibers and high-temperature resistant components, grafting of pineapple leaf fibers with chloroether rubber through ultrasonic dispersion, combined with the modification of polyaramide, enhance the mechanical and high-temperature resistance of PVC composite materials, and utilize chloroether rubber and silicon structures. Improve resilience.
It significantly improves the high temperature resistance and toughness of PVC pipes, extends the service life, avoids softening deformation and impact rupture under high temperature conditions, broadens the application field, and ensures safe and reliable operation.
Smart Images

Figure CN118931067A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a PVC composite material for pipes and a preparation method thereof. Background Art
[0002] Polyvinyl chloride (PVC) is an amorphous long-chain polymer formed by the polymerization of vinyl chloride monomer under the action of an initiator. It is one of the commonly used thermoplastics. Due to the advantages of PVC such as corrosion resistance, insulation, flame retardancy, and easy processing, it plays a very important role in industrial production and is widely used in agriculture, electricity, construction, transportation, packaging and other industries. Preparing PVC composite materials into pipes can give the pipes good physical and chemical properties.
[0003] With the rapid development of polymer materials in recent years and the new application environment requirements for PVC pipes, the performance requirements for PVC pipes are getting higher and higher. When PVC pipes are used as power pipes, they have the defect of insufficient high temperature resistance. When used for a long time under high temperature conditions, the pipes are prone to softening, deformation and other problems, and cannot work for a long time, which greatly reduces the service life of PVC pipes and limits their application scope. In addition, PVC pipes have poor toughness and are prone to cracking when subjected to strong impacts, affecting the normal use of the pipes. PVC pipes need to withstand a certain amount of pressure to ensure that the pipes are not easy to break or deform when subjected to external forces, so as to ensure the safe and stable operation of the system.
[0004] In the prior art, the performance of PVC pipes is mostly improved by adding various functional additives to the matrix to improve the performance of PVC composite materials, thereby giving PVC pipes excellent high temperature resistance and mechanical properties. For example, the invention patent with publication number CN108219326B discloses a high-impact PVC pipe formula and its preparation method. The invention modifies PVC by using MBS resin and ACR resin to form a composite toughening agent. The two can form a so-called "sea-island" structure with the continuous phase of polyvinyl chloride in the form of a dispersed phase, which effectively improves the toughness of PVC pipes. However, there is no improvement in the high temperature resistance of PVC pipes, which has certain limitations in the field of power pipes. Based on this, it is of great significance to develop a PVC composite material with excellent high temperature resistance and mechanical properties. Summary of the invention
[0005] In order to solve the problems mentioned in the background technology, the object of the present invention is to provide a PVC composite material for pipes and a preparation method thereof.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A PVC composite material for pipes comprises the following raw materials in parts by weight: 60-80 parts of polyvinyl chloride, 4-8 parts of functionalized fibers, 3-6 parts of high temperature resistant components, 5-15 parts of fillers, 2-4 parts of plasticizers, 3-5 parts of stabilizers, 0.5-1.5 parts of lubricants, and 1-2 parts of antioxidants.
[0008] Furthermore, the method for preparing the functionalized fiber comprises the following steps:
[0009] A1: ultrasonically disperse pineapple leaf fiber in N,N-dimethylformamide solution, pass nitrogen, add p-dimethylaminobenzoic acid and catalyst, after addition, raise the system temperature to 90-110°C under stirring, keep warm for 4-8 hours, and then discharge the material to obtain modified pineapple leaf fiber;
[0010] A2: The modified pineapple leaf fiber is mixed with toluene solution, and ultrasonicated to form a uniform suspension. Then, chloroether rubber is added to the suspension, and mechanically stirred to be uniform. The suspension is treated at a temperature of 60 to 70°C for 5 to 10 hours, and the solid material is separated by filtration to obtain functionalized fiber.
[0011] Furthermore, in step A1, the catalyst is any one of calcium methanesulfonate, aminosulfonic acid, trifluoromethanesulfonic acid or p-toluenesulfonic acid.
[0012] Furthermore, in step A2, the number average molecular weight of the chloroether rubber is 9000 to 15000.
[0013] Furthermore, the preparation method of the high temperature resistant component comprises the following steps:
[0014] AA1: Add polyaromatic amide and dimethyl sulfoxide to a reactor filled with nitrogen in sequence, stir evenly, add alkali metal hydride, stir at room temperature for 12 to 36 hours, then add 3-chloropropylene, turn on the heating until the temperature in the reactor reaches 65 to 75°C, keep warm and stir for 15 to 25 hours, wait for the material to cool naturally, discharge the material, and obtain modified polyaromatic amide;
[0015] AA2: Under nitrogen protection, add the modified polyaromatic amide to the N-methylpyrrolidone solution, stir evenly, add bis(dimethylsilyl)amine, raise the system temperature to 75-85°C under stirring, continue to add platinum catalyst, stir for 3-7 hours after addition, stop heating and remove nitrogen, cool to room temperature and then discharge to obtain a high temperature resistant component.
[0016] Furthermore, in step AA1, the alkali metal hydride is any one of potassium hydride, sodium hydride or lithium hydride.
[0017] Furthermore, in step AA2, the mass ratio of the modified polyaromatic amide to bis(dimethylsilyl)amine is 1:0.1-0.4.
[0018] Furthermore, the filler is either talcum powder or titanium dioxide; the plasticizer is either dibutyl phthalate or diisononyl phthalate; the stabilizer is either barium zinc stabilizer or calcium zinc stabilizer; the lubricant is either paraffin wax or polyethylene wax; and the antioxidant is either antioxidant 1076 or antioxidant 2246.
[0019] A method for preparing a PVC composite material for pipes comprises the following steps:
[0020] (1) adding polyvinyl chloride, functionalized fiber, high temperature resistant component, filler, plasticizer, stabilizer, lubricant and antioxidant into a high-speed mixer, raising the system temperature to 110-120° C., stirring evenly, placing the mixed material into a cold mixing device, and continuing to mix at 300-500 r / min until the material temperature drops to 40-50° C., discharging the material, and obtaining a blend;
[0021] (2) feeding the blend obtained in step (1) into a twin-screw extruder, setting the speed of the extruder to 400-600 r / min and the melting temperature to 180-220° C., and performing melt extrusion granulation to obtain a PVC composite material.
[0022] Beneficial effects of the present invention:
[0023] (1) The present invention effectively improves the mechanical properties and high temperature resistance of the PVC composite material by adding functionalized fibers and high temperature resistant components into the matrix. The composite material is used to prepare PVC pipes, which is beneficial to improving the service life of the PVC pipes, broadening the application areas of the PVC pipes, and meeting the quality requirements of PVC pipes in multiple fields.
[0024] (2) The present invention utilizes a chemical connection method to graft epichlorohydrin rubber onto the surface of pineapple leaf fiber to obtain functionalized fiber. By modifying the surface of the pineapple leaf fiber, good affinity between the pineapple leaf fiber and the polyvinyl chloride substrate can be achieved, so that the pineapple leaf fiber is evenly dispersed in the polyvinyl chloride substrate. In addition, the pineapple leaf fiber has high strength and a large aspect ratio, and is an excellent reinforcement material. It can significantly enhance the strength of the PVC composite material and prevent the PVC pipe from being deformed, broken, or having reduced durability when subjected to external forces. In addition, the rubber segment in the epichlorohydrin rubber can absorb stress, which can improve the toughness of the PVC composite material and prevent the pipe from cracking when subjected to a strong impact.
[0025] (3) The present invention prepares a high temperature resistant component as a modifier for a PVC composite material. On the one hand, the imino group in the high temperature resistant component structure can generate hydrogen bonds with the C-Cl in the polyvinyl chloride structure, thereby enhancing the interface interaction between the high temperature resistant component and the matrix, which is beneficial to improving the high temperature resistance of the PVC composite material and further improving the toughness of the PVC composite material. On the other hand, the high temperature resistant component structure contains a large amount of silicon and rigid benzene ring structure, which can effectively improve the high temperature resistance of the PVC composite material and give the PVC pipe excellent high temperature resistance, thereby avoiding the softening and deformation of the PVC pipe under long-term use under high temperature conditions, thereby ensuring the safety and reliability of its use.
[0026] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0028] Figure 1 This is a scanning electron microscope image of the pineapple leaf fiber and the functionalized fiber prepared in the present invention.
[0029] Figure 2 This is an infrared spectrum test chart of the polyaromatic amide, modified polyaromatic amide and high temperature resistant component prepared by the present invention. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The functionalized fibers and high temperature resistant components in the examples and comparative examples of the present invention are prepared by the following method:
[0032] 1. Preparation of functionalized fibers
[0033] A1: 5 g of pineapple leaf fiber was ultrasonically dispersed in N,N-dimethylformamide solution, nitrogen was passed through, and after the air was exhausted, 1.2 g of p-dimethylaminobenzoic acid and 0.05 g of p-toluenesulfonic acid were added. After the addition was completed, the system temperature was raised to 100°C under stirring conditions, and the temperature was kept for 6 hours, and then the material was discharged, washed, and dried to obtain modified pineapple leaf fiber;
[0034] A2: Mix 3g of modified pineapple leaf fiber with toluene solution, and ultrasonicate to form a uniform suspension. Then add 2.4g of chloroether rubber to the suspension, stir it mechanically, and treat it at 65°C for 8h. Filter and separate the solid material, wash and vacuum dry it to obtain functionalized fiber.
[0035] The morphology of pineapple leaf fibers and functionalized fibers was analyzed using a ZEISS Gemin i 300 scanning electron microscope produced by Zeiss, Germany. The test results are shown in Figure 1 ,It can be observed from the figure that the surface of pineapple leaf fiber is relatively smooth and flat, while the surface of functionalized fiber is rough. This is because chloroether rubber is grafted onto the surface of pineapple leaf fiber.
[0036] Technical principle: The surface of pineapple leaf fiber contains active hydroxyl groups. Under the action of p-toluenesulfonic acid, it can react with the carboxyl groups in the structure of p-dimethylaminobenzoic acid, thereby modifying the tertiary amine groups on the surface of the pineapple leaf fiber to obtain modified pineapple leaf fiber. The tertiary amine groups on its surface are used as active sites. The mechanism that the tertiary amine groups can react with the halogen functional groups in the structure of chloroether rubber to undergo quaternization reaction is utilized to graft chloroether rubber onto the surface of the pineapple leaf fiber to obtain functionalized fibers.
[0037] 2. Preparation of high temperature resistant components
[0038] AA1: 10 g of polyaromatic amide and dimethyl sulfoxide were added to a reactor filled with nitrogen in sequence, and after stirring evenly, 5 g of sodium hydride was added, and stirred at room temperature for 24 h. Then, 2.6 g of 3-chloropropylene was added, and heating was started until the temperature in the reactor reached 70°C. The mixture was stirred for 20 h at this temperature, and the material was cooled naturally and discharged to obtain modified polyaromatic amide;
[0039] AA2: Under nitrogen protection, add 6 g of modified polyaromatic amide to N-methylpyrrolidone solution, stir evenly, add 1.8 g of bis(dimethylsilyl)amine, raise the system temperature to 80°C under stirring, continue to add 0.02 g of 2% mass fraction of chloroplatinic acid in isopropanol solution, stir for 5 hours, stop heating and remove nitrogen, cool to room temperature and then discharge to obtain a high temperature resistant component.
[0040] The infrared spectroscopy analysis of polyaramid, modified polyaramid and high temperature resistant components was performed using TENSOR 27 Fourier transform infrared spectrometer produced by Bruker, Germany. Figure 2 As shown by Figure 2 It can be seen that in the infrared spectrum of polyaramid, 3315cm -1 The characteristic absorption peak of NH on the amide bond appears at 1655cm -1The characteristic absorption peak of C=O in the amide bond appears at 1245 cm -1 The characteristic absorption peak of CN in the amide bond appears at 1650cm -1 The characteristic absorption peak of C=O in the amide bond appears at 3021cm -1 The characteristic absorption peak of the carbon-hydrogen bond in the carbon-carbon double bond appears at 1241 cm -1 The characteristic absorption peak of CN appears at 1646cm -1 The characteristic absorption peak of C=O appears at 1270cm -1 The absorption peak of C-Si appears at 945cm -1 The characteristic absorption peak of SiN appears at the position where the carbon-hydrogen bond in the carbon-carbon double bond disappears.
[0041] Technical principle: After the amide bond in the polyaromatic amide structure undergoes a metallization reaction with sodium hydride, it can undergo a substitution reaction with the halogen functional group in the 3-chloropropylene structure to obtain a modified polyaromatic amide with an unsaturated alkenyl functional group in the structure. Under the catalysis of an isopropanol solution of chloroplatinic acid, the alkenyl group in the modified polyaromatic amide structure can undergo a silylation reaction with the SiH in the bis(dimethylsilyl)amine structure to obtain a high temperature resistant component.
[0042] Example 1
[0043] Preparation of PVC composite materials
[0044] (1) 60 g of polyvinyl chloride, 4 g of functionalized fiber, 3 g of high temperature resistant component, 5 g of titanium dioxide, 2 g of dibutyl phthalate, 3 g of calcium zinc stabilizer, 0.5 g of paraffin wax and 1 g of antioxidant 1076 were added to a high-speed mixer, the system temperature was raised to 110° C., and after being stirred evenly, the mixture was placed in a cold mixing device, and continued to be mixed at 300 r / min until the material temperature dropped to 40° C., and the mixture was discharged to obtain a blend;
[0045] (2) feeding the blend obtained in step (1) into a twin-screw extruder, setting the speed of the extruder to 400 r / min and the melting temperature to 180° C., and performing melt extrusion granulation to obtain a PVC composite material.
[0046] Example 2
[0047] Preparation of PVC composite materials
[0048] (1) 70 g of polyvinyl chloride, 6 g of functionalized fiber, 5 g of high temperature resistant component, 10 g of titanium dioxide, 3 g of dibutyl phthalate, 4 g of calcium zinc stabilizer, 1 g of paraffin wax and 1.5 g of antioxidant 1076 were added to a high-speed mixer, the system temperature was raised to 115° C., and after being stirred evenly, the mixture was placed in a cold mixing device, and continued to be mixed at 400 r / min until the material temperature dropped to 45° C., and the material was discharged to obtain a blend;
[0049] (2) The blend obtained in step (1) is fed into a twin-screw extruder, the speed of the extruder is set to 500 r / min, the melting temperature is set to 200° C., and melt extrusion granulation is performed to obtain a PVC composite material.
[0050] Example 3
[0051] Preparation of PVC composite materials
[0052] (1) 80 g of polyvinyl chloride, 8 g of functionalized fiber, 6 g of high temperature resistant component, 15 g of titanium dioxide, 4 g of dibutyl phthalate, 5 g of calcium zinc stabilizer, 1.5 g of paraffin wax and 2 g of antioxidant 1076 were added to a high-speed mixer, the system temperature was raised to 120° C., and after being stirred evenly, the mixed material was placed in a cold mixing device, and continued to be mixed at 500 r / min until the material temperature dropped to 50° C., and the material was discharged to obtain a blend;
[0053] (2) The blend obtained in step (1) is fed into a twin-screw extruder, the speed of the extruder is set to 600 r / min, the melting temperature is set to 220° C., and melt extrusion granulation is performed to obtain a PVC composite material.
[0054] Comparative Example 1
[0055] Preparation of PVC composite materials
[0056] (1) 70 g of polyvinyl chloride, 6 g of functionalized fiber, 10 g of titanium dioxide, 3 g of dibutyl phthalate, 4 g of calcium zinc stabilizer, 1 g of paraffin wax and 1.5 g of antioxidant 1076 were added to a high-speed mixer, the system temperature was raised to 115° C., and after being stirred evenly, the mixture was placed in a cold mixing device and continued to be mixed at 400 r / min until the material temperature dropped to 45° C., and the mixture was discharged to obtain a blend;
[0057] (2) The blend obtained in step (1) is fed into a twin-screw extruder, the speed of the extruder is set to 500 r / min, the melting temperature is set to 200° C., and melt extrusion granulation is performed to obtain a PVC composite material.
[0058] Comparative Example 2
[0059] Preparation of PVC composite materials
[0060] (1) 70 g of polyvinyl chloride, 5 g of a high temperature resistant component, 10 g of titanium dioxide, 3 g of dibutyl phthalate, 4 g of a calcium zinc stabilizer, 1 g of paraffin wax and 1.5 g of an antioxidant 1076 were added to a high-speed mixer, the system temperature was raised to 115° C., and after being stirred evenly, the mixture was placed in a cold mixing device, and continued to be mixed at 400 r / min until the material temperature dropped to 45° C., and the mixture was discharged to obtain a blend;
[0061] (2) The blend obtained in step (1) is fed into a twin-screw extruder, the speed of the extruder is set to 500 r / min, the melting temperature is set to 200° C., and melt extrusion granulation is performed to obtain a PVC composite material.
[0062] Comparative Example 3
[0063] Preparation of PVC composite materials
[0064] (1) 70 g of polyvinyl chloride, 4 g of pineapple leaf fiber, 2 g of chloroether rubber, 5 g of high temperature resistant component, 10 g of titanium dioxide, 3 g of dibutyl phthalate, 4 g of calcium zinc stabilizer, 1 g of paraffin and 1.5 g of antioxidant 1076 were added to a high-speed mixer, the system temperature was raised to 115 ° C, and after stirring evenly, the mixture was placed in a cold mixing device, and continued to mix at 400 r / min until the material temperature dropped to 45 ° C, and the material was discharged to obtain a blend;
[0065] (2) The blend obtained in step (1) is fed into a twin-screw extruder, the speed of the extruder is set to 500 r / min, the melting temperature is set to 200° C., and melt extrusion granulation is performed to obtain a PVC composite material.
[0066] Comparative Example 4
[0067] Preparation of PVC composite materials
[0068] (1) 70 g of polyvinyl chloride, 10 g of titanium dioxide, 3 g of dibutyl phthalate, 4 g of calcium zinc stabilizer, 1 g of paraffin wax and 1.5 g of antioxidant 1076 were added to a high-speed mixer, the system temperature was raised to 115° C., and after being stirred evenly, the mixed material was placed in a cold mixing device and continued to be mixed at 400 r / min until the material temperature dropped to 45° C., and the material was discharged to obtain a blend;
[0069] (2) The blend obtained in step (1) is fed into a twin-screw extruder, the speed of the extruder is set to 500 r / min, the melting temperature is set to 200° C., and melt extrusion granulation is performed to obtain a PVC composite material.
[0070] Performance testing:
[0071] The PVC composite materials prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 4 were made into samples that met the specifications. The samples were tested for tensile properties and elongation at break according to GB / T 1040.1-2018 "Determination of tensile properties of plastics Part 1: General Principles"; the samples were tested for impact properties according to GB / T 1843-2008 "Determination of cantilever impact strength of plastics"; the samples were tested for Vicat softening temperature according to GB / T 1633-2000 "Determination of Vicat softening temperature (VST) of thermoplastics". The specific test results are shown in Table 1:
[0072] Table 1 - Performance Test
[0073]
[0074] From the test results in Table 1, it can be seen that the PVC composite materials prepared in Examples 1 to 3 all have excellent toughness, strength and high temperature resistance; in the PVC composite material prepared in Comparative Example 1, only functionalized fibers are added, and the toughness and strength of the PVC composite material are good, and its Vicat softening temperature is 97°C. Compared with the embodiment, the high temperature resistance is average; in the PVC composite material prepared in Comparative Example 2, no functionalized fibers are added, so the toughness and strength are not as good as the embodiment, but because the high temperature resistant component is added therein, the Vicat softening temperature is 105°C, and the high temperature resistance is good; in the PVC composite material prepared in Comparative Example 3, pineapple leaf fiber, chloroether rubber and high temperature resistant component are added, and compared with the embodiment, the toughness and high temperature resistance of the PVC composite material are good, but the strength is average. It is speculated that this may be because the surface of the pineapple leaf fiber is not modified, and agglomeration occurs in the matrix, resulting in the weakening of the strength of the PVC composite material; in the PVC composite material prepared in Comparative Example 4, neither functionalized fibers nor high temperature resistant components are added, so the toughness, strength and high temperature resistance of the PVC composite material are poor.
[0075] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A PVC composite material for pipes, It is characterized in that The invention comprises the following raw materials in parts by weight: 60 to 80 parts of polyvinyl chloride, 4 to 8 parts of functionalized fibers, 3 to 6 parts of high temperature resistant components, 5 to 15 parts of fillers, 2 to 4 parts of plasticizers, 3 to 5 parts of stabilizers, 0.5 to 1.5 parts of lubricants and 1 to 2 parts of antioxidants.
2. The PVC composite material for pipes according to claim 1, It is characterized in that The method for preparing the functionalized fiber comprises the following steps: A1: ultrasonically disperse pineapple leaf fiber in N,N-dimethylformamide solution, pass nitrogen, add p-dimethylaminobenzoic acid and catalyst, after addition, raise the system temperature to 90-110°C under stirring, keep warm for 4-8 hours, and then discharge the material to obtain modified pineapple leaf fiber; A2: The modified pineapple leaf fiber is mixed with toluene solution, and ultrasonicated to form a uniform suspension. Then, chloroether rubber is added to the suspension, and mechanically stirred to be uniform. The suspension is treated at a temperature of 60 to 70°C for 5 to 10 hours, and the solid material is separated by filtration to obtain functionalized fiber.
3. The PVC composite material for pipes according to claim 2, It is characterized in that In step A1, the catalyst is any one of calcium methanesulfonate, aminosulfonic acid, trifluoromethanesulfonic acid or p-toluenesulfonic acid.
4. The PVC composite material for pipes according to claim 2, It is characterized in that In step A2, the number average molecular weight of the chloroether rubber is 9000-15000.
5. The PVC composite material for pipes according to claim 1, It is characterized in that The preparation method of the high temperature resistant component comprises the following steps: AA1: Add polyaromatic amide and dimethyl sulfoxide to a reactor filled with nitrogen in sequence, stir evenly, add alkali metal hydride, stir at room temperature for 12 to 36 hours, then add 3-chloropropylene, turn on the heating until the temperature in the reactor reaches 65 to 75°C, keep warm and stir for 15 to 25 hours, wait for the material to cool naturally, discharge the material, and obtain modified polyaromatic amide; AA2: Under nitrogen protection, add the modified polyaromatic amide to the N-methylpyrrolidone solution, stir evenly, add bis(dimethylsilyl)amine, raise the system temperature to 75-85°C under stirring, continue to add platinum catalyst, stir for 3-7 hours after addition, stop heating and remove nitrogen, cool to room temperature and then discharge to obtain a high temperature resistant component.
6. The PVC composite material for pipes according to claim 5, It is characterized in that In step AA1, the alkali metal hydride is any one of potassium hydride, sodium hydride or lithium hydride.
7. The PVC composite material for pipes according to claim 5, It is characterized in that In step AA2, the mass ratio of the modified polyaromatic amide to bis(dimethylsilyl)amine is 1:0.1-0.
4.
8. The PVC composite material for pipes according to claim 1, It is characterized in that The filler is either talcum powder or titanium dioxide; the plasticizer is either dibutyl phthalate or diisononyl phthalate; the stabilizer is either barium zinc stabilizer or calcium zinc stabilizer; the lubricant is either paraffin wax or polyethylene wax; and the antioxidant is either antioxidant 1076 or antioxidant 2246.
9. A method for preparing the PVC composite material for pipes as claimed in claim 1, It is characterized in that The following steps are involved: (1) adding polyvinyl chloride, functionalized fiber, high temperature resistant component, filler, plasticizer, stabilizer, lubricant and antioxidant into a high-speed mixer, raising the system temperature to 110-120° C., stirring evenly, placing the mixed material into a cold mixing device, and continuing to mix at 300-500 r / min until the material temperature drops to 40-50° C., discharging the material, and obtaining a blend; (2) feeding the blend obtained in step (1) into a twin-screw extruder, setting the speed of the extruder to 400-600 r / min and the melting temperature to 180-220° C., and performing melt extrusion granulation to obtain a PVC composite material.