Anti-aging hydrolysis-resistant reinforced nylon material

The chopped glass fibers treated with silane coupling are combined with high-end amino nylon resin, combined with heat stabilizer and lubricating dispersant, and the degradation problem of nylon materials in high-temperature hydrolysis environment is solved, and aging-resistant and hydrolysis-resistant reinforced nylon materials are prepared. It meets the strict conditions of automotive parts and realizes the high temperature, high strength and long-term stability of the material.

CN118931178APending Publication Date: 2024-11-12ANHUI ZHONGHAN POLYMER TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411238236.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Nylon materials are prone to degradation in high temperature and hydrolysis environments, resulting in a decrease in mechanical properties and it is difficult to meet the long-term use requirements of automotive engine peripherals and coolant contact parts. The existing hydrolysis-resistant nylon materials have poor performance and prices, and the domestic lack of compliance with strict requirements. Materials for conditions.

Method used

The chopped glass fibers treated with silane coupling are combined with high-end amino-content nylon resin. By adding heat stabilizers and lubricating dispersants, the thermal oxygen aging performance and fluidity of the material are improved. The same-directional parallel twin-screw extruder is used for processing. , reduce the structural damage of glass fibers, and prepare aging-resistant and hydrolysis-resistant reinforced nylon material.

Benefits of technology

It significantly improves the high temperature, hydrolysis and heat resistance of the material, extends the material life, meets the high temperature and high strength usage conditions of automotive parts, improves the stability and impact resistance of the material, and has long-term and stable performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005028389980000041
    Figure BDA0005028389980000041
  • Figure BDA0005028389980000051
    Figure BDA0005028389980000051
  • Figure BDA0005028389980000052
    Figure BDA0005028389980000052
Patent Text Reader

Abstract

The invention discloses an aging-resistant hydrolysis-resistant reinforced nylon material, and belongs to the technical field of nylon materials. Comprising the following raw materials in parts by weight: 45-85 parts of polyamide resin, 0-50 parts of modified glass fibers, 0-3 parts of a heat stabilizer, 0-5 parts of a lubricating dispersant, 0-0.3 part of an initiator and 0-15 parts of an auxiliary agent. Wherein the prepared auxiliary agent can greatly enhance the aging resistance, water resistance and heat resistance of the material to a certain extent, and the performance is long and stable. The nylon material prepared by the invention has stable and efficient aging resistance, water resistance and heat resistance, solves the technical problem of long-term use under harsh conditions such as impact resistance and capability of bearing high temperature and high strength required by a worm gear part in an automobile steering system, and has important application value in the technical field of nylon materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nylon materials, and in particular relates to an aging-resistant and hydrolysis-resistant reinforced nylon material. Background Art

[0002] At present, the development trends of energy conservation and emission reduction, replacing steel with plastics and new energy vehicles in the automotive field require that automotive engineering plastics have better stability and durability, while taking into account mechanical properties.

[0003] Nylon materials have high strength, excellent toughness, good fatigue strength, and good heat resistance, and are widely used in the automotive, transportation and other industries. However, when the temperature rises and it comes into contact with water or alcohol liquid environments, nylon materials are prone to hydrolysis or alcoholysis reactions, or even degradation, resulting in a sharp decline in mechanical properties, limiting its wide application in the field of engineering machinery. In theory, reinforcing and filling nylon materials with glass fiber materials can be used in more high-strength, high-toughness and other harsh environmental parts. However, the interface between nylon materials and glass fibers is not well bonded and the compatibility is poor, resulting in poor stability of glass fiber reinforced nylon composite materials, which are difficult to meet the technical requirements for long-term use under harsh conditions such as high temperatures around automobile engines and parts in contact with coolant.

[0004] Automobile engines and surrounding materials of water chambers are subjected to high temperature environment for a long time and are in contact with coolant or water for a long time. Related parts and water pipe joints need to be able to withstand the corrosion of coolant and should not crack or change the surface during application. At the same time, these parts are often large parts, and the materials used need to have good flow properties and should not degrade during high temperature and high pressure injection molding.

[0005] Reinforced nylon composite materials with aging resistance and hydrolysis resistance are one of the research hotspots and cutting-edge technologies in the development of world automobile technology, with broad application prospects. In the existing technology, hydrolysis-resistant nylon materials for domestic high-end automobiles and large trucks are mainly imported. Some domestic material companies have also developed related hydrolysis-resistant nylon materials, but the performance and price vary greatly, and there is a certain gap with imported materials.

[0006] Therefore, designing reasonable combinations and processes, and using appropriate raw materials and processing aids to prepare glass fiber reinforced nylon materials that are resistant to aging and hydrolysis is an important direction for future development. Summary of the invention

[0007] The purpose of the present invention is to overcome the defects of the prior art and provide a reinforced nylon material which is resistant to aging and hydrolysis.

[0008] The purpose of the present invention can be achieved through the following technical solutions:

[0009] A reinforced nylon material resistant to aging and hydrolysis is prepared by the following steps:

[0010] A1, drying the polyamide resin to obtain a dry polyamide resin;

[0011] A2, adding the dried polyamide resin, heat stabilizer, lubricating dispersant, initiator and auxiliary agent obtained in step A1 into a high-speed mixer and stirring evenly to obtain a premix;

[0012] A3. The premix obtained in step A2 is added from the main feeding port of the extruder, and the modified glass fiber is added through the side feeding port, the processing temperature of the plasticizing melting zone and the melt conveying zone is controlled, and the aging-resistant and hydrolysis-resistant reinforced nylon material is obtained by vacuum extraction, extrusion and granulation.

[0013] Furthermore, the raw materials are calculated in parts by weight as follows: 45-85 parts of polyamide resin, 0-50 parts of modified glass fiber, 0-3 parts of heat stabilizer, 0-5 parts of lubricating dispersant, 0-0.3 parts of initiator, and 0-15 parts of auxiliary agent.

[0014] Furthermore, the polyamide resin is one of nylon 66 with a terminal amino content of more than 40 mmol / kg and a relative viscosity of 2.0-2.8 and nylon 6 with a relative viscosity of 2.0-2.8.

[0015] Furthermore, the drying conditions are 80-100° C., drying for 3-8 hours, and controlling the moisture content to be below 0.02%.

[0016] Furthermore, the heat stabilizer is a mixture of potassium bromide, cuprous iodide and N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenedicarbamide in a mass ratio of 1:1:2.

[0017] Furthermore, the initiator is one of potassium persulfate and azobisisobutyronitrile.

[0018] Furthermore, the lubricating dispersant includes any one or a combination of several of montan wax, polyethylene wax, polypropylene wax, erucamide, oleamide, calcium stearate, and zinc stearate.

[0019] Furthermore, the extruder is a co-rotating parallel twin-screw extruder; the aspect ratio of the extruder is 32:1-52:1, the melt blending extrusion temperature is 240°C-300°C, wherein the first stage temperature is controlled below 120°C; the feeding speed is 10-75rpm / min, the screw speed is 100-600rpm / min, and the screw aspect ratio is 32:1-48:1.

[0020] The addition of lubricating dispersant improves the processing fluidity of glass fiber reinforced nylon material, reduces the friction coefficient, and improves the dispersion effect of modified glass fiber and heat stabilizer in nylon material; heat stabilizer can improve the thermal oxidation aging performance of the material, improve the high temperature resistance of the material to extend the life of the product, and provide long-term stability for high-rigidity nylon composite materials to resist premature mechanical fatigue caused by aging under the highest working temperature pressure, and delay the degradation of the material; high-end amino content nylon resin is selected to make the material have a higher decomposition temperature and heat resistance, and the terminal amino group can destroy the hydroperoxide generated by the oxidation degradation of nylon resin, prevent the material from cracking after aging in a high temperature environment, and improve the long-term hydrolysis resistance of the material; finally, the premix is ​​added from the main feeding port of the extruder, and the glass fiber is added through the side feeding port according to the weight, thereby greatly reducing the structural damage problem of the glass fiber.

[0021] Furthermore, the modified glass fiber is prepared by the following steps:

[0022] The chopped glass fiber was soaked in acetone for 24 hours, washed with distilled water, dried, placed in an ethanol aqueous solution, and γ-aminopropyltriethoxysilane (silane coupling agent KH-550) was added. The temperature was controlled at 80°C. After stirring for 6 hours, the pH value was adjusted to 5 with glacial acetic acid, and vacuum dried for 2 hours to obtain modified glass fiber.

[0023] Furthermore, the ratio of the chopped glass fiber, acetone, ethanol aqueous solution, and γ-aminopropyltriethoxysilane is 1 g:100 mL:100 mL:4.5 g.

[0024] Furthermore, the chopped glass fiber monofilaments have an average diameter of 5-20 μm and a length of 3-8 mm.

[0025] Chopped glass fibers have good reinforcing effects and effective filling effects. Treating the chopped glass fibers with silane coupling agents can change the interfacial effect of the chopped glass fibers, improve their hydrophobicity, and thereby enhance their compatibility with the nylon matrix, improve the bonding between the glass fibers and the surface of the nylon matrix, reduce the voids in the composite material, and greatly improve the strength and heat resistance of the material.

[0026] Furthermore, the auxiliary agent is prepared by the following steps:

[0027] S1. In a three-necked flask equipped with a thermometer, an electromagnetic stirrer and a spherical condenser, a drying tube is added to the outlet of the condenser, and the drying tube is connected to a tail gas absorption device to absorb the generated hydrogen chloride gas. After pentaerythritol and benzene are mixed, phosphorus trichloride is slowly added dropwise under stirring, and the temperature is controlled not to exceed 30° C. After the addition is completed, the temperature is raised to 70° C., and the reaction is refluxed for 4 hours. After the reaction is completed, the solvent benzene and excess phosphorus trichloride are distilled off to obtain dichloropentaerythritol phosphite; the ratio of pentaerythritol, benzene and phosphorus trichloride is 13.6g:100mL:27.8g;

[0028] Pentaerythritol reacts with phosphorus trichloride to obtain dichloropentaerythritol phosphite; the specific reaction is as follows:

[0029]

[0030] S2. In a three-necked flask equipped with a stirring device, dichloropentaerythritol phosphite, 3,5-di-tert-butyl-4-hydroxybenzyl alcohol, potassium carbonate (acid binding agent) and N,N-dimethylformamide (DMF) were mixed and stirred uniformly, the reaction temperature was controlled to 70°C, and the reaction was kept warm for 8 hours. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by rotary evaporation. The mixture was then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 2:3), and the eluent was removed by rotary evaporation to obtain intermediate 1; the ratio of dichloropentaerythritol phosphite, 3,5-di-tert-butyl-4-hydroxybenzyl alcohol, potassium carbonate and N,N-dimethylformamide was 29.1 g:23.6 g:15 mL:100 mL;

[0031] Under the catalysis of potassium carbonate, dichloropentaerythritol phosphite and 3,5-di-tert-butyl-4-hydroxybenzyl alcohol react, and by controlling the molar ratio of the two to be close to 1:1 and the dichloropentaerythritol phosphite to be slightly excessive, only one chlorine group on the dichloropentaerythritol phosphite participates in the reaction to obtain intermediate 1; the specific reaction process is as follows:

[0032]

[0033] S3. In a three-necked flask equipped with a stirring device, tetrafluorobutanediol, allyl acetic acid and N,N-dimethylformamide (DMF) were mixed and stirred uniformly, and then dibutyltin oxide (catalyst) and dicyclohexylcarbodiimide (DCC) were added, and the temperature was raised to 85°C for reaction for 4 hours. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by rotary evaporation. The mixture was purified by column chromatography (the eluent was a mixed solvent of ethyl acetate / methanol in a volume ratio of 3:2), and the eluent was removed by rotary evaporation to obtain intermediate 2; the ratio of the amount of tetrafluorobutanediol, allyl acetic acid, N,N-dimethylformamide, dibutyltin oxide and dicyclohexylcarbodiimide was 17.4 g:10.1 g:100 mL:0.2 g:20.6 g;

[0034] Under the catalysis of dibutyltin oxide and DCC, the hydroxyl group on tetrafluorobutanediol and the carboxyl group on allyl acetic acid undergo esterification reaction. By controlling the molar ratio of the two to be close to 1:1 and the tetrafluorobutanediol to be slightly excessive, only one hydroxyl group on tetrafluorobutanediol participates in the reaction to obtain intermediate 2. The specific reaction process is as follows:

[0035]

[0036] S4, in a three-necked flask equipped with a stirring device, intermediate 2, intermediate 1, triethylamine (acid binding agent) and toluene were mixed and stirred uniformly, the reaction temperature was controlled to 75 ° C, the reaction was kept warm for 8 hours, the reaction was completed, triethylamine hydrochloride was filtered out, part of the solvent was removed by rotary evaporation, and then purified by column chromatography (eluent using a mixed solvent of benzene / ethyl acetate, the volume ratio of the two is 5:3), the eluent was removed by rotary evaporation to obtain an auxiliary agent; the ratio of the amount of intermediate 2, intermediate 1, triethylamine, toluene is 23.1g:46.4g:15mL:150mL;

[0037] Triethylamine is used as an acid-binding agent to remove the hydrogen chloride generated by the reaction, and intermediate 2 and intermediate 1 undergo a nucleophilic substitution reaction to obtain an auxiliary agent; the structure of the auxiliary agent is shown below:

[0038]

[0039] The prepared auxiliary agent molecule contains phosphite, hindered phenol and CF bond structure, wherein the introduced phosphite can be used as a kind of auxiliary antioxidant, which can decompose the hydroperoxide generated in the polymer due to oxidative aging and make it inactive, thereby achieving the purpose of terminating or delaying the oxidative degradation of the polymer; moreover, the hindered phenol group belongs to phenolic antioxidants, and the structure of this type of antioxidant contains -OH functional group, which is easier to provide H atoms in the reaction, and the occurrence of this process is achieved through proton donation, so that the free radical auto-oxidation in the chain reaction is destroyed, achieving the antioxidant effect, and can play a synergistic role with phosphite, greatly enhancing the aging resistance of the nylon matrix; in addition, the introduced CF bond has a small polarity and a strong bond energy. The higher the chemical bond energy, the better the stability, which not only improves the heat resistance of the matrix, but also gives the matrix excellent waterproof performance. Moreover, the CF bond can well coat the CC main chain, shield it, and improve the stability;

[0040] It should be noted that one end of the additive molecule also contains a carbon-carbon double bond, which can be cross-linked with the matrix, thereby improving the migration and exudation resistance of the additive small molecule and making the performance of the additive long-term and stable.

[0041] Beneficial effects of the present invention:

[0042] 1. The present invention uses short-cut glass fibers treated with silane coupling, which have a small diameter and can play a good reinforcing effect and an effective filling role, improve the interface bonding between the glass fiber and the surface of the nylon matrix, make the voids in the composite material smaller, and have better hydrolysis resistance, strength and stability. The material's bearing strength and heat resistance are improved to meet the harsh operating conditions of high temperature and hydrolysis resistant parts of automobiles.

[0043] 2. The present invention improves the thermal oxidative aging performance of the composite material by adding a thermal stabilizer, thereby improving the high temperature resistance of the material.

[0044] 3. Choose nylon resin with high-end amino content, which has higher decomposition temperature and heat resistance. At the same time, the terminal amino group can destroy the hydroperoxide generated by the oxidative degradation of nylon resin, prevent the material from cracking after aging in a high-temperature environment, and improve the long-term hydrolysis resistance of the material.

[0045] 4. During processing, the twin-screw module combination is adjusted to minimize the damage of the screw shear force to the glass fiber structure, while increasing the surface contact energy and bonding strength between the glass fiber and the nylon material, giving full play to the high performance of the glass fiber material and achieving a better composite effect with the nylon material.

[0046] 5. The prepared additives can greatly enhance the material's aging resistance, water resistance and a certain degree of heat resistance, and the performance is long-lasting and stable.

[0047] Therefore, the nylon material prepared by the present invention has stable and efficient aging resistance, water resistance and heat resistance, solves the technical problems of the worm gear parts in the automobile steering system required to be impact-resistant and able to withstand long-term use under harsh conditions such as high temperature and high strength, and has important application value in the field of nylon material technology. DETAILED DESCRIPTION

[0048] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Example 1

[0050] Preparation of modified glass fiber:

[0051] 1 g of chopped glass fiber with a single fiber diameter of 5 μm and a length of 3 mm was soaked in 100 mL of acetone for 24 h, washed with distilled water, dried, placed in an ethanol aqueous solution, and 4.5 g of γ-aminopropyltriethoxysilane was added. The temperature was controlled at 80 ° C. After stirring for 6 h, the pH value was adjusted to 5 with glacial acetic acid, and vacuum dried for 2 h to obtain modified glass fiber.

[0052] Example 2

[0053] Preparation of modified glass fiber:

[0054] 2 g of chopped glass fiber with a single fiber diameter of 20 μm and a length of 8 mm was soaked in 200 mL of acetone for 24 h, washed with distilled water, dried, placed in an ethanol aqueous solution, and 9 g of γ-aminopropyltriethoxysilane was added. The temperature was controlled at 80 ° C. After stirring for 6 h, the pH value was adjusted to 5 with glacial acetic acid, and vacuum dried for 2 h to obtain modified glass fiber.

[0055] Example 3

[0056] Preparation aids:

[0057] S1. In a three-necked flask equipped with a thermometer, an electromagnetic stirrer and a spherical condenser, a drying tube is added to the outlet of the condenser, and the drying tube is connected to a tail gas absorption device to absorb the generated hydrogen chloride gas. After mixing 13.6 g of pentaerythritol and 100 mL of benzene, 27.8 g of phosphorus trichloride is slowly added dropwise under stirring, and the temperature is controlled not to exceed 30° C. After the addition is completed, the temperature is raised to 70° C., and the reaction is refluxed for 4 hours. After the reaction is completed, the solvent benzene and excess phosphorus trichloride are removed by distillation to obtain dichloropentaerythritol phosphite;

[0058] S2. In a three-necked flask equipped with a stirring device, 29.1 g of dichloropentaerythritol phosphite, 23.6 g of 3,5-di-tert-butyl-4-hydroxybenzyl alcohol, 15 mL of potassium carbonate and 100 mL of N,N-dimethylformamide (DMF) were mixed and stirred uniformly, the reaction temperature was controlled to 70° C., and the reaction was kept warm for 8 hours. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by rotary evaporation. The mixture was then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 2:3), and the eluent was removed by rotary evaporation to obtain intermediate 1.

[0059] S3, in a three-necked flask equipped with a stirring device, 17.4 g of tetrafluorobutanediol, 10.1 g of allyl acetic acid and 100 mL of N, N-dimethylformamide were mixed and stirred evenly, and then 0.2 g of dibutyltin oxide and 20.6 g of dicyclohexylcarbodiimide were added, and the temperature was raised to 85°C for reaction for 4 h. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by rotary evaporation. Then, the mixture was purified by column chromatography (the eluent was a mixed solvent of ethyl acetate / methanol in a volume ratio of 3:2), and the eluent was removed by rotary evaporation to obtain intermediate 2;

[0060] S4. In a three-necked flask equipped with a stirring device, 23.1 g of intermediate 2, 46.4 g of intermediate 1, 15 mL of triethylamine and 150 mL of toluene were mixed and stirred evenly, the reaction temperature was controlled to 75°C, and the reaction was kept warm for 8 hours. After the reaction was completed, the triethylamine hydrochloride was filtered out, and part of the solvent was removed by rotary evaporation. Then, it was purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 5:3), and the eluent was removed by rotary evaporation to obtain an auxiliary agent.

[0061] Example 4

[0062] Preparation aids:

[0063] S1. In a three-necked flask equipped with a thermometer, an electromagnetic stirrer and a spherical condenser, a drying tube is added to the outlet of the condenser, and the drying tube is connected to a tail gas absorption device to absorb the generated hydrogen chloride gas. After mixing 27.2 g of pentaerythritol and 200 mL of benzene, 55.6 g of phosphorus trichloride is slowly added dropwise under stirring, and the temperature is controlled not to exceed 30° C. After the addition is completed, the temperature is raised to 70° C., and the reaction is refluxed for 4 hours. After the reaction is completed, the solvent benzene and excess phosphorus trichloride are removed by distillation to obtain dichloropentaerythritol phosphite;

[0064] S2, in a three-necked flask equipped with a stirring device, 58.2 g of dichloropentaerythritol phosphite, 47.2 g of 3,5-di-tert-butyl-4-hydroxybenzyl alcohol, 30 mL of potassium carbonate and 200 mL of N,N-dimethylformamide (DMF) were mixed and stirred uniformly, the reaction temperature was controlled to 70° C., and the reaction was kept warm for 8 hours. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by rotary evaporation. The mixture was then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 2:3), and the eluent was removed by rotary evaporation to obtain intermediate 1;

[0065] S3, in a three-necked flask equipped with a stirring device, 34.8g of tetrafluorobutanediol, 20.2g of allyl acetic acid and 200mL of N,N-dimethylformamide were mixed and stirred evenly, and then 0.4g of dibutyltin oxide and 41.2g of dicyclohexylcarbodiimide were added, and the temperature was raised to 85°C for reaction for 4h, and stirring was continued during the reaction. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of ethyl acetate / methanol, and the volume ratio of the two was 3:2), and the eluent was removed by rotary evaporation to obtain intermediate 2;

[0066] S4. In a three-necked flask equipped with a stirring device, 46.2 g of intermediate 2, 92.8 g of intermediate 1, 30 mL of triethylamine and 300 mL of toluene were mixed and stirred evenly, the reaction temperature was controlled to 75°C, and the reaction was kept warm for 8 hours. After the reaction was completed, the triethylamine hydrochloride was filtered out, and part of the solvent was removed by rotary evaporation. Then, it was purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 5:3), and the eluent was removed by rotary evaporation to obtain an auxiliary agent.

[0067] Example 5

[0068] A1. Dry 66 g of nylon 66 having a relative viscosity of 2.6 and an amino terminal content of 110 mmol / kg at 100° C. for 6 h to obtain dry nylon 66;

[0069] A2, the dried nylon 66 obtained in step A1, 0.5g of a heat stabilizer (a mixture of potassium bromide, cuprous iodide and N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenedicarbamide in a mass ratio of 1:1:2), 1g of montan wax, 0.1g of potassium persulfate and 2.5g of the auxiliary agent obtained in Example 3, added into a high-speed mixer and stirred evenly to obtain a premix;

[0070] A3, adding the premix obtained in step A2 from the main feeding port of the extruder, and adding 30g of the modified glass fiber obtained in Example 1 through the side feeding port, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, vacuum extraction, extrusion, and granulation to obtain an aging-resistant and hydrolysis-resistant reinforced nylon material;

[0071] Among them, the extruder is a co-rotating parallel twin-screw extruder; the aspect ratio of the extruder is 32:1, the melt blending extrusion temperature is 240°C, of ​​which the first stage temperature is 120°C; the feeding speed is 10rpm / min, the screw speed is 100rpm / min, and the screw aspect ratio is 32:1.

[0072] Example 6

[0073] A1. Dry 72 g of nylon 66 with a relative viscosity of 2.7 and an amino terminal content of 85 mmol / kg at 100° C. for 6 h to obtain dry nylon 66;

[0074] A2, the dried nylon 66 obtained in step A1, 0.4g of a heat stabilizer (a mixture of potassium bromide, cuprous iodide and N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenedicarbamide in a mass ratio of 1:1:2), 1g of polyethylene wax, 0.1g of azobisisobutyronitrile and 1.9g of the auxiliary agent obtained in Example 3, added into a high-speed mixer and stirred evenly to obtain a premix;

[0075] A3, adding the premix obtained in step A2 from the main feeding port of the extruder, and adding 25g of the modified glass fiber obtained in Example 1 through the side feeding port, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, vacuum extraction, extrusion, and granulation to obtain an aging-resistant and hydrolysis-resistant reinforced nylon material;

[0076] Among them, the extruder is a co-rotating parallel twin-screw extruder; the aspect ratio of the extruder is 42:1, the melt blending extrusion temperature is 260°C, of ​​which the first stage temperature is 110°C; the feed speed is 45rpm / min, the screw speed is 300rpm / min, and the screw aspect ratio is 40:1.

[0077] Example 7

[0078] A1. Dry 66 g of nylon 66 with a relative viscosity of 2.7 and an amino terminal content of 85 mmol / kg at 100°C for 6 hours to obtain dry nylon 66;

[0079] A2, the dried nylon 66 obtained in step A1, 0.5g of a heat stabilizer (a mixture of potassium bromide, cuprous iodide and N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenedicarbamide in a mass ratio of 1:1:2), 1g of montan wax, 0.1g of potassium persulfate and 2.3g of the auxiliary agent obtained in Example 3, added into a high-speed mixer and stirred evenly to obtain a premix;

[0080] A3, adding the premix obtained in step A2 from the main feeding port of the extruder, and adding 30g of the modified glass fiber obtained in Example 1 through the side feeding port, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, vacuum extraction, extrusion, and granulation to obtain an aging-resistant and hydrolysis-resistant reinforced nylon material;

[0081] Among them, the extruder is a co-rotating parallel twin-screw extruder; the aspect ratio of the extruder is 52:1, the melt blending extrusion temperature is 300°C, of ​​which the first stage temperature is 110°C; the feed speed is 75rpm / min, the screw speed is 600rpm / min, and the screw aspect ratio is 48:1.

[0082] Example 8

[0083] A1. Dry 59 g of nylon 66 with a relative viscosity of 2.7 and an amino terminal content of 85 mmol / kg at 100° C. for 6 h to obtain dry nylon 66;

[0084] A2, the dried nylon 66 obtained in step A1, 0.6 g of a heat stabilizer (a mixture of potassium bromide, cuprous iodide and N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenedicarbamide in a mass ratio of 1:1:2), 1.5 g of montan wax, 0.3 g of potassium persulfate and 3.8 g of the auxiliary agent obtained in Example 4, added to a high-speed mixer and stirred evenly to obtain a premix;

[0085] A3, adding the premix obtained in step A2 from the main feeding port of the extruder, and adding 35g of the modified glass fiber obtained in Example 2 through the side feeding port, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, vacuum extraction, extrusion, and granulation to obtain an aging-resistant and hydrolysis-resistant reinforced nylon material;

[0086] Among them, the extruder is a co-rotating parallel twin-screw extruder; the aspect ratio of the extruder is 52:1, the melt blending extrusion temperature is 300°C, of ​​which the first stage temperature is 110°C; the feed speed is 75rpm / min, the screw speed is 600rpm / min, and the screw aspect ratio is 48:1.

[0087] Example 9

[0088] A1. Dry 54 g of nylon 66 having a relative viscosity of 2.7 and an end amino content of 110 mmol / kg at 100° C. for 6 h to obtain dry nylon 66;

[0089] A2, the dried nylon 66 obtained in step A1, 0.7g of a heat stabilizer (a mixture of potassium bromide, cuprous iodide and N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenedicarbamide in a mass ratio of 1:1:2), 2g of oleic acid amide, 0.3g of potassium persulfate and 3.3g of the auxiliary agent obtained in Example 4, added into a high-speed mixer and stirred evenly to obtain a premix;

[0090] A3, adding the premix obtained in step A2 from the main feeding port of the extruder, and adding 40g of the modified glass fiber obtained in Example 2 through the side feeding port, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, vacuum extraction, extrusion, and granulation to obtain an aging-resistant and hydrolysis-resistant reinforced nylon material;

[0091] Among them, the extruder is a co-rotating parallel twin-screw extruder; the aspect ratio of the extruder is 52:1, the melt blending extrusion temperature is 300°C, of ​​which the first stage temperature is 110°C; the feed speed is 75rpm / min, the screw speed is 600rpm / min, and the screw aspect ratio is 48:1.

[0092] Example 10

[0093] A1. Dry 66 g of nylon 6 with a relative viscosity of 2.8 at 100°C for 6 hours to obtain dry nylon 6;

[0094] A2, the dried nylon 6 obtained in step A1, 0.5g of a heat stabilizer (a mixture of potassium bromide, cuprous iodide and N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenedicarbamide in a mass ratio of 1:1:2), 1g of zinc stearate, 0.1g of potassium persulfate and 2.3g of the auxiliary agent obtained in Example 4, added to a high-speed mixer and stirred evenly to obtain a premix;

[0095] A3, adding the premix obtained in step A2 from the main feeding port of the extruder, and adding 30g of the modified glass fiber obtained in Example 2 through the side feeding port, controlling the processing temperature of the plasticizing melting zone and the melt conveying zone, vacuum extraction, extrusion, and granulation to obtain an aging-resistant and hydrolysis-resistant reinforced nylon material;

[0096] Among them, the extruder is a co-rotating parallel twin-screw extruder; the aspect ratio of the extruder is 52:1, the melt blending extrusion temperature is 300°C, of ​​which the first stage temperature is 110°C; the feed speed is 75rpm / min, the screw speed is 600rpm / min, and the screw aspect ratio is 48:1.

[0097] Comparative Example 1

[0098] This embodiment provides an aging-resistant and hydrolysis-resistant reinforced nylon material, the components and preparation process of which are substantially the same as those of embodiment 10, except that:

[0099] The main ingredients used in this comparative example include the following raw materials in parts by weight: 69g nylon resin, 30g glass fiber, 1.0g lubricating dispersant, and 2.3g commercially available antioxidant;

[0100] The nylon resin is commercially available nylon 66 with a relative viscosity of 2.7 and a terminal amino group content of 42 mmol / kg.

[0101] Comparative Example 2

[0102] This embodiment provides an aging-resistant and hydrolysis-resistant reinforced nylon material, the components and preparation process of which are substantially the same as those of embodiment 10, except that:

[0103] The main ingredients used in this comparative example include the following raw materials in parts by weight: 64g nylon resin, 35g glass fiber, and 2.3g commercially available antioxidant;

[0104] The nylon resin is commercially available nylon 66 with a relative viscosity of 2.7 and a terminal amino group content of 42 mmol / kg.

[0105] Comparative Example 3

[0106] This embodiment provides an aging-resistant and hydrolysis-resistant reinforced nylon material, the components and preparation process of which are substantially the same as those of embodiment 10, except that:

[0107] The main ingredients used in this comparative example include the following raw materials in parts by weight: 69g nylon resin, 30g glass fiber, and 2.3g commercially available antioxidant;

[0108] The nylon resin is commercially available nylon 6 having a relative viscosity of 2.8.

[0109] Comparative Example 4

[0110] Commercially available hydrolysis-resistant 35% glass fiber reinforced nylon 66 material is used.

[0111] The following performance tests were performed on Examples 5-10 and Comparative Examples 1-4, as follows:

[0112] The prepared pellets were placed in a blast oven and dried at 110°C for 8 hours. The dried pellets were then injection molded in an injection molding machine to prepare test specimens. The injection molding mold temperature was 70°C.

[0113] The tensile properties test was carried out according to ISO 527, with a tensile speed of 50 mm / min;

[0114] The bending performance test was carried out according to ISO 178, with a bending speed of 2 mm / min and a span of 64 mm;

[0115] The simply supported beam impact strength was carried out according to ISO 179.

[0116] The comprehensive performance of the composite material is evaluated by the tensile strength, flexural strength and impact strength values ​​obtained by testing. At the same time, the injection-molded specimens need to be placed in a sealed tank filled with 100% coolant at 135°C, immersed for 48 hours and 1000 hours respectively, and then taken out and tested within half an hour after being dried.

[0117] The measured results are shown in the following table:

[0118]

[0119]

[0120] It can be seen from the above table that the aging-resistant and hydrolysis-resistant reinforced nylon materials prepared in Examples 5-10 of the present invention have better anti-coolant aging performance than other comparative examples, and can meet the technical requirements of TL52682 (bending strength ≥ 25MPa after soaking in 100% antifreeze, 135°C constant temperature sealed conditions for 1000h) and TL-VW774 (i.e., the surface is smooth and crack-free after soaking in 100% antifreeze, 135°C constant temperature sealed conditions for 48h, and stress cracking does not occur during assembly), indicating that the aging-resistant and hydrolysis-resistant glass fiber reinforced nylon composite material prepared by the present invention has good reinforcement and aging-resistant and hydrolysis-resistant modification effects. Among them, the tensile strength and impact strength of Examples 5 and 7 with a glass fiber content of 30 parts are matched, and the comprehensive performance is the best. Compared with the representative comparative example 4 on the market, Example 8 has significant advantages in impact performance, aging resistance and hydrolysis resistance, and the appearance is smooth and complete after 1000 hours of cooling liquid resistance, indicating that it can withstand high-temperature injection molding and still maintain good mechanical properties. By adding a heat stabilizer, a lubricant and a suitable processing technology, the grain size is miniaturized, and the impact resistance of the nylon material of the present invention is improved. The additive has a positive effect on the retention rate of the nylon composite material of the present invention after aging and hydrolysis in coolant. The material performance can meet the use of parts around automobile engines and water chambers.

[0121] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0122] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. An aging-resistant and hydrolysis-resistant reinforced nylon material, characterized in that: The invention comprises the following raw materials in parts by weight: 45-85 parts of polyamide resin, 0-50 parts of modified glass fiber, 0-3 parts of heat stabilizer, 0-5 parts of lubricating dispersant, 0-0.3 parts of initiator and 0-15 parts of auxiliary agent.

2. The aging-resistant and hydrolysis-resistant reinforced nylon material according to claim 1, characterized in that: The auxiliary agent is prepared by the following steps: S1. After pentaerythritol and benzene are mixed, phosphorus trichloride is slowly added dropwise under stirring, and the temperature is controlled not to exceed 30° C. After the addition is completed, reflux reaction is carried out at 70° C. for 4 hours. After the reaction is completed, distillation is performed to obtain dichloropentaerythritol phosphite; S2, dichloropentaerythritol phosphite, 3,5-di-tert-butyl-4-hydroxybenzyl alcohol, potassium carbonate and N,N-dimethylformamide were mixed and stirred evenly, reacted at 70° C. for 8 h, and after the reaction was completed, filtered, evaporated, purified by column chromatography, and evaporated to obtain intermediate 1; S3, tetrafluorobutanediol, allyl acetic acid and N,N-dimethylformamide were mixed and stirred evenly, and then dibutyltin oxide and dicyclohexylcarbodiimide were added, and the mixture was reacted at 85° C. for 4 h, with continuous stirring during the reaction. After the reaction was completed, the mixture was filtered, rotary evaporated, purified by column chromatography, and rotary evaporated to obtain intermediate 2; S4. Mix and stir the intermediate 2, intermediate 1, triethylamine and toluene evenly, control the reaction temperature to 75°C, and keep the reaction warm for 8 hours. After the reaction is completed, filter, rotary evaporate, purify by column chromatography, and rotary evaporate to obtain an auxiliary agent.

3. The aging-resistant and hydrolysis-resistant reinforced nylon material according to claim 2, characterized in that: In step S1, the ratio of pentaerythritol, benzene and phosphorus trichloride is 13.6 g:100 mL:27.8 g.

4. The aging-resistant and hydrolysis-resistant reinforced nylon material according to claim 2, characterized in that: In step S2, the ratio of the amount of dichloropentaerythritol phosphite, 3,5-di-tert-butyl-4-hydroxybenzyl alcohol, potassium carbonate and N,N-dimethylformamide is 29.1 g:23.6 g:15 mL:100 mL.

5. The aging-resistant and hydrolysis-resistant reinforced nylon material according to claim 2, characterized in that: In step S3, the ratio of the amount of tetrafluorobutanediol, allyl acetic acid, N,N-dimethylformamide, dibutyltin oxide, and dicyclohexylcarbodiimide is 17.4 g: 10.1 g: 100 mL: 0.2 g: 20.6 g.

6. The aging-resistant and hydrolysis-resistant reinforced nylon material according to claim 2, characterized in that: In step S4, the ratio of the amount of intermediate 2, intermediate 1, triethylamine and toluene is 23.1 g:46.4 g:15 mL:150 mL.

7. The aging-resistant and hydrolysis-resistant reinforced nylon material according to claim 1, characterized in that: The modified glass fiber is prepared by the following steps: The chopped glass fibers were soaked in acetone for 24 hours, washed, dried, placed in an ethanol aqueous solution, and γ-aminopropyltriethoxysilane was added. The temperature was controlled at 80°C, stirred for 6 hours, adjusted to a pH of 5, and vacuum dried for 2 hours to obtain modified glass fibers.

8. The aging-resistant and hydrolysis-resistant reinforced nylon material according to claim 7, characterized in that: The ratio of the chopped glass fibers, acetone, ethanol aqueous solution, and γ-aminopropyltriethoxysilane is 1 g:100 mL:100 mL:4.5 g.

9. The aging-resistant and hydrolysis-resistant reinforced nylon material according to claim 7, characterized in that: The chopped glass fiber monofilaments have an average diameter of 5-20 μm and a length of 3-8 mm.

Citation Information

Cited By

  • Sound-insulation and pressure-resistant PE pipe and preparation method thereof

    CN119661921A