Quick-drying water-based ink and preparation method thereof

By using aqueous acrylic emulsion and homemade aqueous alkyd resin, and combining emulsion technology to design the core-shell structure, the problem of slow drying speed of water-based ink is solved, and the rapid drying and high adhesion fastness of ink are achieved.

CN118931256AActive Publication Date: 2024-11-12深圳市深赛尔股份有限公司
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411155397.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The drying rate of water-based inks is slow, affecting production efficiency, requiring additional drying equipment or longer drying time.

Method used

Use aqueous acrylic emulsion and homemade aqueous alkyd resin as the connecting material, and conduct esterification reactions through specific mixed ratios of dry vegetable oil, crystalline polyols and aromatic polyacids or anhydrides. The core-shell structure is designed in combination with emulsion technology to improve the drying of ink Speed ​​and heat resistance.

Benefits of technology

It significantly improves the drying speed and heat resistance of the ink, improves storage stability and adhesion fastness, and solves the problem of slow drying speed of water-based inks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931256A_ABST
    Figure CN118931256A_ABST
Patent Text Reader

Abstract

The invention discloses quick-drying water-based ink and a preparation method thereof. The quick-drying water-based ink is prepared from the following components in percentage by weight: 40 to 50 percent of water-based acrylic emulsion, 15 to 20 percent of water-based alkyd resin, 1 to 2 percent of polyethylene wax, 10 to 30 percent of pigment, 0.1 to 0.3 percent of defoaming agent, 0.2 to 0.5 percent of flatting agent, 0.1 to 0.5 percent of dispersing agent, 0.1 to 1 percent of coupling agent and the balance of water. The water-based ink is prepared by taking a water-based acrylic emulsion and water-based alkyd resin as connecting materials; the water-based alkyd resin adopts dry vegetable oil, crystalline polyhydric alcohol and aromatic polybasic acid or acid anhydride in a specific mixing ratio as main raw materials; the introduction of the dry vegetable oil can accelerate the drying of the ink, the crystalline polyol can improve the cross-linking speed and density of the water-based alkyd resin, and the aromatic polyacid or anhydride introduces an aromatic ring into the water-based alkyd resin so as to improve the heat resistance of the polymer. The drying speed and the heat resistance of the prepared water-based ink are obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a quick-drying water-based ink and a preparation method thereof. Background Art

[0002] Ink is an important material used in printing. It is a uniform mixture of colored bodies (such as pigments), binders (resins), fillers, additives and solvents. It is a colored, fluid slurry adhesive. Ink can express patterns and texts on substrates through printing or spraying. It is widely used in various printings such as books and periodicals, packaging and decoration, and architectural decoration. With the increase of social demand, the variety and output of inks have also expanded and increased accordingly.

[0003] Water-based ink is an ink that uses water as a solvent or dispersant, referred to as "water-based ink". It uses water-based polymer resin as a binder, does not contain harmful organic solvents, can reduce pollution to the environment and harm to the human body, and is undoubtedly more in line with environmental protection requirements. Water-based acrylic emulsion not only has the advantages of organic solvent-based resins such as excellent gloss, acid and alkali resistance, good weather resistance, and pollution resistance, but also has the characteristics of low price, safe use, energy saving, and reduced environmental pollution and public hazards. It is a low-VOC green and environmentally friendly material, and has become the best choice for water-based ink binders with its diversity and good physical and chemical properties. However, compared with traditional solvent-based inks, water-based inks have a relatively slow drying speed, which means that production efficiency may be affected and often require additional drying equipment or longer drying time.

[0004] Therefore, it is necessary to further develop water-based inks with fast drying properties. Summary of the invention

[0005] In order to overcome the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a quick-drying water-based ink.

[0006] Another object of the present invention is to provide a method for preparing the quick-drying water-based ink.

[0007] The purpose of the present invention is achieved through the following technical solutions: A quick-drying water-based ink, comprising the following components by weight percentage: Water-based acrylic emulsion 40-50%, Water-based alkyd resin 15-20%, Polyethylene wax 1-2%, Pigment 10-30%, Defoaming agent 0.1-0.3%, Leveling agent 0.2-0.5%, Dispersant 0.1-0.5%, Coupling agent 0.1-1%, The balance is water; The preparation of the waterborne alkyd resin comprises the following steps: (1) In a nitrogen or rare gas atmosphere, 10-15 parts by weight of vegetable oil, 0.2-0.5 parts by weight of catalyst, 2-5 parts by weight of diglycerol, 15-20 parts by weight of crystalline polyol, 20-25 parts by weight of polyacid or anhydride, and 40-80 parts by weight of xylene are added to a reaction kettle, and heated to 190-210° C. and refluxed to carry out esterification reaction; (2) Sampling and measuring the acid value of the reaction system. When the acid value is 25-30 mgKOH / g, heating is stopped and xylene is removed by vacuum distillation. (3) Adding a neutralizing agent to the reaction system to adjust the pH to 7-8 to obtain the waterborne alkyd resin.

[0008] Preferably, the vegetable oil is safflower oil and walnut oil in a mass ratio of 1:(3-5).

[0009] Preferably, the catalyst is at least one of antimony oxide, antimony acetate, tin oxide, lithium hydroxide, monobutyltin oxide, dibutyltin oxide, and dibutyltin dilaurate.

[0010] Preferably, the crystalline polyol is at least one of neopentyl glycol, pentaerythritol and erythritol.

[0011] Preferably, the polyacid is at least one of phthalic acid, isophthalic acid, terephthalic acid, and 2,6-naphthalene dicarboxylic acid.

[0012] Preferably, the acid anhydride is at least one of phthalic anhydride, benzoic anhydride and trimellitic anhydride.

[0013] Preferably, the dispersant is at least one of oleamide, sodium lignin sulfonate, sodium tripolyphosphate, sodium pyrophosphate, and sodium silicate.

[0014] Preferably, the defoamer is an organosilicon defoamer. In some embodiments of the present invention, the organosilicon defoamer includes but is not limited to at least one of BYK-020, BYK-077 and BYK-085 produced by BYK in Germany.

[0015] In some embodiments of the present invention, the leveling agent includes but is not limited to at least one of EFKA-3033, EFKA-3777, EFKA-3236, and EFKA-3288 produced by BASF of Germany.

[0016] Preferably, the coupling agent is a silane coupling agent. In some embodiments of the present invention, the silane coupling agent includes but is not limited to at least one of KH550, KH560, KH570, and KH792 produced by Shanghai Aladdin Biochemical Technology Co., Ltd.

[0017] Preferably, the preparation of the aqueous acrylic emulsion comprises the following steps: S1, adding 30-40 parts by weight of methyl methacrylate, 5-10 parts by weight of acrylic acid, 10-15 parts by weight of N-hydroxymethyl acrylamide, and 2-3 parts by weight of an emulsifier to 15-20 parts by weight of water and mixing evenly to obtain an emulsion; S2, the emulsion obtained in step S1 and 8-10 parts by weight of an aqueous solution of an initiator with a concentration of 5-8wt% are simultaneously added dropwise to 90-100 parts by weight of water at 85-95° C., and the mixture is kept warm for 1-2 hours after the addition is completed to obtain a first reaction solution; S3, taking 1 / 4 of the amount of methyl methacrylate, acrylic acid, and N-hydroxymethyl acrylamide used in step S1, and preparing a mixed solution with 2-3 parts by weight of hydroxyethyl methacrylate and 0.5-1 parts by weight of thioacetic acid; S4, synchronously adding the mixed solution prepared in step S3 and 8-10 parts by weight of an aqueous solution of an initiator with a concentration of 5-8wt% to the first reaction solution obtained in step S2, and keeping the mixture at 85-95° C. for 1-2 hours after the addition is completed to obtain a second reaction solution; S5. After the temperature of the second reaction liquid is reduced to 55-60° C., 0.5-1 parts by weight of a mixture of tert-butyl hydroperoxide and sodium isoascorbate and 8-10 parts by weight of water are added thereto, and the mixture is kept at 55-60° C. for 1-2 hours, and then naturally cooled to room temperature and a neutralizing agent is added to adjust the pH to 7-8, thereby obtaining the aqueous acrylic emulsion.

[0018] Preferably, the neutralizing agent is at least one of triethanolamine, triethylamine, N,N-dimethylethanolamine, ammonia water, sodium carbonate and sodium hydroxide.

[0019] Preferably, the emulsifier is at least one of alkylphenol polyoxyethylene ether, sodium dodecyl sulfate and sodium dodecylbenzene sulfonate.

[0020] Preferably, the initiator is at least one of ammonium persulfate, sodium persulfate and potassium persulfate.

[0021] Preferably, in step S5, the mass ratio of tert-butyl hydroperoxide to sodium isoascorbate is 1:(1-2).

[0022] The method for preparing the quick-drying water-based ink comprises the following steps: (1) Weigh all components by weight and mix them at room temperature and a speed of 400-600 r / min for 30-45 min; (2) The mixed materials are sent to a ball mill and ground to a fineness of less than 15 μm to obtain the quick-drying water-based ink.

[0023] Compared with the prior art, the present invention has the following advantages and effects: (1) The present invention uses water-based acrylic emulsion and self-made water-based alkyd resin as binders to prepare water-based ink. The self-made water-based alkyd resin uses dry vegetable oil (palm kernel oil and perilla seed oil), crystalline aliphatic polyol and aromatic polyacid or anhydride in a specific mixing ratio as main raw materials; wherein the introduction of dry vegetable oil can accelerate the drying of ink, crystalline aliphatic polyol can improve the crosslinking speed and crosslinking density of water-based alkyd resin, and aromatic polyacid or anhydride introduces aromatic rings into water-based alkyd resin to improve the heat resistance of polymer. After the water-based alkyd resin is blended with water-based acrylic emulsion and other additives, the drying speed and heat resistance of the obtained ink are significantly improved. At the same time, the self-made water-based alkyd resin also introduces diglycerol, whose hydroxyl group can participate in the reaction and can increase the main chain length and reduce the degree of branching, thereby improving the water resistance and adhesion of the prepared ink.

[0024] (2) The present invention further adopts emulsion technology and designs a core-shell structure by a two-step dropping method to prepare an aqueous acrylic emulsion, which can improve the dispersibility of the prepared ink, which is beneficial to improving the storage stability of the ink. At the same time, it can also make the ink better bond with the surface of the substrate, further improving the adhesion strength of the ink. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 These are the test results of initial drying, heat resistance and scratch resistance of the water-based inks prepared in the examples and comparative examples.

[0027] Figure 2 The test results of water resistance, storage stability and adhesion fastness of the water-based inks prepared in the examples and comparative examples are shown. DETAILED DESCRIPTION

[0028] The embodiments of the present invention will be clearly and completely described below in conjunction with the examples, and the described examples are only some examples of the present invention, rather than all examples. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the examples in the present invention, all other examples obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0029] The reagents or instruments used in the present invention, if the manufacturer is not specified, are all conventional products that can be purchased from the market. For process parameters not specifically specified, conventional techniques can be used.

[0030] The commercially available water-based acrylic emulsion used in the specific embodiment of the present invention was purchased from Guangzhou Xinlian New Materials Co., Ltd., CAS: 25085-34-1; The polyethylene wax used was purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number: P816883; The commercially available waterborne alkyd resin used was purchased from Pandex (Shanghai) International Trading Co., Ltd.; The safflower oil used was purchased from Tianjin Xiensi Biochemical Technology Co., Ltd., product number: S-00600; The walnut oil used was purchased from Shanghai Dingfen Chemical Technology Co., Ltd., product number: P032987; The permanent orange pigment used was purchased from Lily Group Co., Ltd.

[0031] Example 1 This embodiment provides a quick-drying water-based ink, which includes the following components by weight percentage: Water-based acrylic emulsion 45%, Water-based alkyd resin 15%, Polyethylene wax 2%, Pigment (Permanent Orange) 20%, Defoamer (BYK-077) 0.2%, Leveling agent (EFKA-3033) 0.4%, Dispersant (oleamide) 0.2%, Coupling agent (KH550) 0.3%, The balance was deionized water.

[0032] The aqueous acrylic emulsion used in this embodiment is prepared according to the following steps: S1, adding 40 parts by weight of methyl methacrylate, 6 parts by weight of acrylic acid, 10 parts by weight of N-hydroxymethyl acrylamide, and 2 parts by weight of alkylphenol polyoxyethylene ether into 20 parts by weight of deionized water and mixing evenly to obtain an emulsion; S2, the emulsion obtained in step S1 and 8 parts by weight of an aqueous solution of ammonium persulfate having a concentration of 5 wt% are simultaneously added dropwise to 100 parts by weight of deionized water at 90° C., and after the addition is completed, the mixture is kept warm for 2 hours to obtain a first reaction solution; S3, taking 1 / 4 of the amount of methyl methacrylate, acrylic acid, and N-hydroxymethyl acrylamide used in step S1, and preparing a mixed solution with 2 parts by weight of hydroxyethyl methacrylate and 0.8 parts by weight of thioacetic acid; S4, synchronously adding the mixed solution prepared in step S3 and 8 parts by weight of an aqueous solution of ammonium persulfate having a concentration of 5 wt% to the first reaction solution obtained in step S2, and after the addition is completed, keeping the mixture at 90° C. for 1 hour to obtain a second reaction solution; S5. After the temperature of the second reaction liquid is reduced to 60° C., a solution prepared by adding 0.9 parts by weight of a mixture of tert-butyl hydroperoxide and sodium isoascorbate in a mass ratio of 1:2 and 10 parts by weight of deionized water is added thereto, and the mixture is kept warm at 60° C. for 1.5 hours, and then naturally cooled to room temperature and sodium carbonate is added to adjust the pH to 7.5, thereby obtaining the aqueous acrylic emulsion.

[0033] The water-based alkyd resin used in this embodiment was prepared as follows: (1) In a nitrogen atmosphere, 10 parts by weight of safflower oil and walnut oil in a mass ratio of 1:4, 0.2 parts by weight of antimony acetate, 3 parts by weight of diglycerol, 15 parts by weight of pentaerythritol, 25 parts by weight of trimellitic anhydride, and 60 parts by weight of xylene were added to a reaction kettle, and the mixture was heated to 190° C. and refluxed for esterification reaction; (2) Sampling and measuring the acid value of the reaction system. When the acid value is 25 mgKOH / g, heating is stopped and xylene is removed by vacuum distillation. (3) Sodium carbonate is added to the reaction system to adjust the pH to 7.5 to obtain the water-based alkyd resin.

[0034] The quick-drying water-based ink of this embodiment is prepared according to the following steps: (1) Weigh all components by weight and mix them at room temperature and 500 r / min for 40 min; (2) The mixed materials are sent to a ball mill and ground to a fineness of less than 15 μm to obtain the quick-drying water-based ink.

[0035] Example 2 This embodiment provides a quick-drying water-based ink, which includes the following components by weight percentage: Water-based acrylic emulsion 40%, Water-based alkyd resin 15%, Polyethylene wax 2%, Pigment (Permanent Orange) 25%, Defoamer (BYK-085) 0.1%, Leveling agent (EFKA-3236) 0.2%, Dispersant (sodium lignin sulfonate) 0.2%, Coupling agent (KH792) 0.2%, The balance was deionized water.

[0036] The aqueous acrylic emulsion used in this embodiment is prepared according to the following steps: S1, adding 36 parts by weight of methyl methacrylate, 8 parts by weight of acrylic acid, 12 parts by weight of N-hydroxymethyl acrylamide, and 2 parts by weight of sodium lauryl sulfate to 18 parts by weight of deionized water and mixing evenly to obtain an emulsion; S2, the emulsion obtained in step S1 and 8 parts by weight of a 5 wt% sodium persulfate aqueous solution are simultaneously added dropwise to 90 parts by weight of deionized water at 95° C., and after the addition is completed, the mixture is kept warm for 1 hour to obtain a first reaction solution; S3, taking 1 / 4 of the amount of methyl methacrylate, acrylic acid, and N-hydroxymethyl acrylamide used in step S1, and preparing a mixed solution with 3 parts by weight of hydroxyethyl methacrylate and 0.6 parts by weight of thioacetic acid; S4, synchronously adding the mixed solution prepared in step S3 and 8 parts by weight of a 5 wt% sodium persulfate aqueous solution to the first reaction solution obtained in step S2, and keeping the mixture at 95° C. for 1.5 h after the addition is complete to obtain a second reaction solution; S5. After the temperature of the second reaction liquid is reduced to 60° C., 0.6 parts by weight of a mixture of tert-butyl hydroperoxide and sodium isoascorbate in a mass ratio of 1:1 and 8 parts by weight of deionized water are added thereto, and the mixture is kept at 60° C. for 2 hours, then naturally cooled to room temperature, and ammonia water is added to adjust the pH to 7, thereby obtaining the aqueous acrylic emulsion.

[0037] The water-based alkyd resin used in this embodiment was prepared as follows: (1) In a nitrogen atmosphere, 12 parts by weight of safflower oil and walnut oil in a mass ratio of 1:3, 0.5 parts by weight of dibutyltin oxide, 3 parts by weight of diglycerol, 18 parts by weight of erythritol, 25 parts by weight of benzoic anhydride, and 60 parts by weight of xylene were added to a reaction kettle, and the mixture was heated to 200° C. and refluxed for esterification reaction; (2) Sampling and measuring the acid value of the reaction system. When the acid value is 27 mgKOH / g, heating is stopped and xylene is removed by vacuum distillation. (3) Adding ammonia water to the reaction system to adjust the pH to 7 to obtain the waterborne alkyd resin.

[0038] The quick-drying water-based ink of this embodiment is prepared according to the following steps: (1) Weigh all the components by weight and mix them at room temperature and 500 r / min for 45 min; (2) The mixed materials are sent to a ball mill and ground to a fineness of less than 15 μm to obtain the quick-drying water-based ink.

[0039] Example 3 This embodiment provides a quick-drying water-based ink, which includes the following components by weight percentage: Water-based acrylic emulsion 50%, Water-based alkyd resin 20%, Polyethylene wax 2%, Pigment (Permanent Orange) 15%, Defoamer (BYK-020) 0.3%, Leveling agent (EFKA-3777) 0.5%, Dispersant (sodium tripolyphosphate) 0.5%, Coupling agent (KH570) 0.5%, The balance was deionized water.

[0040] The aqueous acrylic emulsion used in this embodiment is prepared according to the following steps: S1, adding 32 parts by weight of methyl methacrylate, 6 parts by weight of acrylic acid, 12 parts by weight of N-hydroxymethyl acrylamide, and 3 parts by weight of sodium dodecylbenzene sulfonate to 15 parts by weight of deionized water and mixing evenly to obtain an emulsion; S2, the emulsion obtained in step S1 and 10 parts by weight of an aqueous solution of ammonium persulfate having a concentration of 6 wt% are simultaneously added dropwise to 90 parts by weight of deionized water at 85° C., and after the addition is completed, the mixture is kept warm for 1.5 hours to obtain a first reaction solution; S3, taking 1 / 4 of the amount of methyl methacrylate, acrylic acid, and N-hydroxymethyl acrylamide used in step S1, and preparing a mixed solution with 2 parts by weight of hydroxyethyl methacrylate and 0.5 parts by weight of thioacetic acid; S4, synchronously adding the mixed solution prepared in step S3 and 10 parts by weight of an aqueous solution of ammonium persulfate having a concentration of 6 wt % to the first reaction solution obtained in step S2, and after the addition is completed, keeping the mixture at 85° C. for 2 h to obtain a second reaction solution; S5. After the temperature of the second reaction liquid is reduced to 55° C., a solution prepared by adding 0.8 parts by weight of a mixture of tert-butyl hydroperoxide and sodium isoascorbate in a mass ratio of 1:1 and 10 parts by weight of deionized water is added thereto, and the mixture is kept warm at 55° C. for 1 hour, then naturally cooled to room temperature, and triethylamine is added to adjust the pH to 8, thereby obtaining the aqueous acrylic emulsion.

[0041] The water-based alkyd resin used in this embodiment was prepared as follows: (1) In a nitrogen atmosphere, 12 parts by weight of safflower oil and walnut oil in a mass ratio of 1:5, 0.4 parts by weight of tin oxide, 4 parts by weight of diglycerol, 20 parts by weight of neopentyl glycol, 25 parts by weight of 2,6-naphthalene dicarboxylic acid, and 60 parts by weight of xylene were added to a reaction kettle, and the mixture was heated to 200° C. and refluxed for esterification reaction; (2) Sampling and measuring the acid value of the reaction system. When the acid value is 30 mgKOH / g, heating is stopped and xylene is removed by vacuum distillation. (3) Add triethylamine to the reaction system to adjust the pH to 8 to obtain the waterborne alkyd resin.

[0042] The quick-drying water-based ink of this embodiment is prepared according to the following steps: (1) Weigh all components by weight and mix them at room temperature and 600 r / min for 35 min; (2) The mixed materials are sent to a ball mill and ground to a fineness of less than 15 μm to obtain the quick-drying water-based ink.

[0043] Example 4 The difference between this embodiment and embodiment 1 is that the water-based acrylic emulsion used is a commercially available water-based acrylic emulsion purchased from Guangzhou Xinlian New Materials Co., Ltd., CAS: 25085-34-1.

[0044] Comparative Example 1 The difference between this comparative example and Example 1 is that the water-based alkyd resin used is a commercially available water-based alkyd resin purchased from Pandex (Shanghai) International Trading Co., Ltd.

[0045] Comparative Example 2 The difference between this comparative example and Example 1 is that in the process of preparing the water-based alkyd resin, 10 parts by weight of the vegetable oil are all safflower oil.

[0046] Comparative Example 3 The difference between this comparative example and Example 1 is that in the process of preparing the water-based alkyd resin, 10 parts by weight of the vegetable oil are all walnut oil.

[0047] Comparative Example 4 The difference between this comparative example and Example 1 is that no diglycerol component is added during the preparation of the waterborne alkyd resin.

[0048] Performance Testing In order to further demonstrate the effect of the present invention, the water-based inks prepared in the above examples and comparative examples were subjected to the following performance tests: 1. Initial drying test The ink was printed on the surface of the polytetrafluoroethylene plate using a 250 mesh screen, and the initial drying of the water-based ink was tested according to GB / T13217.5-2008 "Test method for initial drying of liquid inks". The test results are as follows: Figure 1 shown.

[0049] 2. Heat resistance test The ink was printed on the surface of the polytetrafluoroethylene plate using a 250 mesh screen. After the ink was left to dry and solidify at room temperature, it was placed in a 200°C environment and baked for 12 hours. The surface condition of the ink layer was observed. The test results are as follows: Figure 1 shown.

[0050] 3. Water resistance test The ink was printed on the surface of a polytetrafluoroethylene plate using a 250-mesh screen. After the ink was left to dry and solidify at room temperature, the water resistance of the ink was tested according to GB / T1733-1993 "Determination of Water Resistance of Paint Films". The bubbling and shedding of the ink were observed. The test results are as follows: Figure 2 shown.

[0051] 4. Storage stability test The prepared ink was left standing for 3 months at room temperature and sealed, and the flocculation, precipitation and agglomeration of the ink were observed. The test results are as follows: Figure 2 shown.

[0052] 5. Adhesion fastness test The ink was printed on the surface of the polytetrafluoroethylene plate using a 250 mesh screen. After the ink was left to dry and solidify at room temperature, the ink adhesion was tested according to GB / T13217.7-2009 "Test Method for Adhesion Fastness of Liquid Inks". The test results are as follows: Figure 2 shown.

[0053] 6. Scratch resistance test The ink was printed on the surface of the polytetrafluoroethylene plate using a 250 mesh screen. After the ink was left to dry and solidify at room temperature, a 2019 version of a 1 yuan coin was used to apply a 100g load to the ink layer for a scratch test. The peeling condition was visually observed. The test results are as follows: Figure 1 shown.

[0054] Depend on Figure 1 and Figure 2From the test results, it can be seen that the ink of Example 4 has a more obvious decline in storage stability and adhesion than the ink of Examples 1-3 because it does not use the homemade water-based acrylic emulsion of the present invention, but its initial drying, heat resistance and water resistance still maintain better performance; the ink of Comparative Example 1 has a more obvious decline in many properties because it does not use the homemade water-based alkyd resin of the present invention; the inks of Comparative Examples 2 and 3 do not mix safflower oil and walnut oil in the process of preparing the water-based alkyd resin, and their initial drying has a more obvious decline, indicating that the simultaneous use of safflower oil and walnut oil in the present invention is beneficial to improving the drying performance of the ink; the ink of Comparative Example 4 does not add diglycerol component in the process of preparing the water-based alkyd resin, and its water resistance and adhesion are lower than those of the inks of Examples 1-4.

[0055] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A quick-drying water-based ink, characterized in that: The components include the following by weight percentage: Water-based acrylic emulsion 40-50%, Water-based alkyd resin 15-20%, Polyethylene wax 1-2%, Pigment 10-30%, Defoaming agent 0.1-0.3%, Leveling agent 0.2-0.5%, Dispersant 0.1-0.5%, Coupling agent 0.1-1%, The balance is water; The preparation of the waterborne alkyd resin comprises the following steps: (1) In a nitrogen or rare gas atmosphere, 10-15 parts by weight of vegetable oil, 0.2-0.5 parts by weight of catalyst, 2-5 parts by weight of diglycerol, 15-20 parts by weight of crystalline polyol, 20-25 parts by weight of polyacid or anhydride, and 40-80 parts by weight of xylene are added to a reaction kettle, and heated to 190-210° C. and refluxed to carry out esterification reaction; (2) Sampling and measuring the acid value of the reaction system. When the acid value is 25-30 mgKOH / g, heating is stopped and xylene is removed by vacuum distillation. (3) Adding a neutralizing agent to the reaction system to adjust the pH to 7-8 to obtain the waterborne alkyd resin.

2. The quick-drying water-based ink according to claim 1, characterized in that: The preparation of the aqueous acrylic emulsion comprises the following steps: S1, adding 30-40 parts by weight of methyl methacrylate, 5-10 parts by weight of acrylic acid, 10-15 parts by weight of N-hydroxymethyl acrylamide, and 2-3 parts by weight of an emulsifier to 15-20 parts by weight of water and mixing evenly to obtain an emulsion; S2, the emulsion obtained in step S1 and 8-10 parts by weight of an aqueous solution of an initiator with a concentration of 5-8wt% are simultaneously added dropwise to 90-100 parts by weight of water at 85-95° C., and the mixture is kept warm for 1-2 hours after the addition is completed to obtain a first reaction solution; S3, taking 1 / 4 of the amount of methyl methacrylate, acrylic acid, and N-hydroxymethyl acrylamide used in step S1, and preparing a mixed solution with 2-3 parts by weight of hydroxyethyl methacrylate and 0.5-1 parts by weight of thioacetic acid; S4, synchronously adding the mixed solution prepared in step S3 and 8-10 parts by weight of an aqueous solution of an initiator with a concentration of 5-8wt% to the first reaction solution obtained in step S2, and keeping the mixture at 85-95° C. for 1-2 hours after the addition is completed to obtain a second reaction solution; S5. After the temperature of the second reaction liquid is reduced to 55-60° C., 0.5-1 parts by weight of a mixture of tert-butyl hydroperoxide and sodium isoascorbate and 8-10 parts by weight of water are added thereto, and the mixture is kept at 55-60° C. for 1-2 hours, and then naturally cooled to room temperature and a neutralizing agent is added to adjust the pH to 7-8, thereby obtaining the aqueous acrylic emulsion.

3. The quick-drying water-based ink according to claim 1, characterized in that: The vegetable oils are safflower oil and walnut oil in a mass ratio of 1:(3-5).

4. The quick-drying water-based ink according to claim 1, characterized in that: The catalyst is at least one of antimony oxide, antimony acetate, tin oxide, lithium hydroxide, monobutyltin oxide, dibutyltin oxide, and dibutyltin dilaurate.

5. The quick-drying water-based ink according to claim 1, characterized in that: The crystalline polyol is at least one of neopentyl glycol, pentaerythritol and erythritol; the polyacid is at least one of phthalic acid, isophthalic acid, terephthalic acid and 2,6-naphthalene dicarboxylic acid; the acid anhydride is at least one of phthalic anhydride, benzoic anhydride and trimellitic anhydride.

6. The quick-drying water-based ink according to claim 1, characterized in that: The dispersant is at least one of oleamide, sodium lignin sulfonate, sodium tripolyphosphate, sodium pyrophosphate and sodium silicate.

7. The quick-drying water-based ink according to claim 1 or 2, characterized in that: The neutralizing agent is at least one of triethanolamine, triethylamine, N,N-dimethylethanolamine, ammonia water, sodium carbonate and sodium hydroxide.

8. The quick-drying water-based ink according to claim 2, characterized in that: The emulsifier is at least one of alkylphenol polyoxyethylene ether, sodium dodecyl sulfate, and sodium dodecylbenzene sulfonate; the initiator is at least one of ammonium persulfate, sodium persulfate, and potassium persulfate.

9. The quick-drying water-based ink according to claim 2, characterized in that: In step S5, the mass ratio of tert-butyl hydroperoxide to sodium isoascorbate is 1:(1-2).

10. The method for preparing the quick-drying water-based ink according to claim 1, characterized in that: The steps include: (1) Weigh all components by weight and mix them at room temperature and a speed of 400-600 r / min for 30-45 min; (2) The mixed materials are sent to a ball mill and ground to a fineness of less than 15 μm to obtain the quick-drying water-based ink.

Citation Information

Patent Citations

  • Preparing method of ethanol-soluble resin for printing ink and application thereof

    CN101525405A

  • Polymer emulsion, preparation method and re-dispersible latex powder

    CN101550218A

  • Aqueous acrylic acid-alkyd paint and preparation method thereof

    CN109337536A

  • Environmental-friendly water-based printing ink and preparation method thereof

    CN110204958A

  • High-solid-content high-performance glycidyl tertiary carboxylic ester modified alkyd resin and preparation method thereof

    CN111234126A