Preparation method of aramid fiber product
By using super acid to crack and disperse aramid fibers and add nanomaterials, the problem of structural hydrolysis of aramid fibers during alkaline cracking is solved, and aramid nanofiber bundles with high elongation of fracture and fracture toughness are prepared. The film fully reflects its excellent performance.
Patent Information
- Application Number
- CN202411252367.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-12
AI Technical Summary
The structural hydrolysis of existing aramid fibers during alkaline cracking leads to a decrease in fracture elongation and fracture toughness, which fails to fully reflect their excellent performance.
Use super acids such as trifluoromethylsulfonic acid or chlorosulfonic acid to crack and disperse aramid fibers to prepare mixed liquids or mixed colloids, and prepare high-quality products through washing, drying, nanomaterial addition, emulsification, wet spinning and other steps. Performance of aramid nanofiber bundles or films.
The elongation and fracture toughness of aramid fibers are improved, and the performance space is broadened, so that the prepared aramid nanofiber bundles and films have high strength and good processing properties.
Smart Images

Figure CN118932707A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of aramid fiber processing and molding, and in particular to a method for preparing aramid fiber products. Background Art
[0002] In the related technology, in order to achieve new aramid fiber properties and related industrial development, aramid nanofibers can be prepared by a stripping method, that is, aramid is cracked using potassium hydroxide and dimethyl sulfoxide to prepare well-dispersed aramid nanofibers.
[0003] However, during the alkaline lysis process, the structure of the material undergoes a certain degree of hydrolysis, so the elongation at break and the fracture toughness of the prepared aramid nanofibers are significantly reduced, and the excellent performance of the aramid fiber itself is not further reflected. Summary of the invention
[0004] In view of this, the present application provides a method for preparing an aramid fiber product to solve the above technical problems.
[0005] The first aspect of the present application provides a method for preparing an aramid fiber product, comprising the following steps: washing the aramid fiber and drying it; adding a superacid to the washed and dried aramid fiber to fully dissolve it to obtain a mixed solution or a mixed colloid, wherein the superacid is at least one of trifluoromethanesulfonic acid or chlorosulfonic acid; controlling the viscosity of the mixed solution or the mixed colloid to obtain a mixed solution or a mixed colloid with good processing performance; and preparing the mixed solution or the mixed colloid as the aramid fiber product. The superacid in the present application refers to an acid with a stronger acidity than pure sulfuric acid.
[0006] Based on the first aspect, in one embodiment, the dissolution temperature is 25°C-120°C, and the dissolution time is 0.5h-72h.
[0007] Based on the first aspect, in one embodiment, based on the total volume of the aramid fiber and the super acid, the content of the aramid fiber is 1 mg / ml-100 mg / ml.
[0008] Based on the first aspect, in one embodiment, the aramid fiber is washed with a washing solution, and the washing solution is any one of ethanol, deionized water, acetone, a salt solution and isopropanol.
[0009] Based on the first aspect, in one embodiment, the aramid fiber product is a composite of a nanomaterial and the aramid fiber. Before the mixed liquid or mixed colloid is made into the aramid fiber product, the preparation method further includes: adding the nanomaterial to the washed and dried aramid fiber, and dispersing the mixed liquid or mixed colloid with an emulsifier, and the dispersion speed of the emulsifier is 7000rpm-24000rpm.
[0010] Based on the first aspect, in one implementation, the nanomaterial is at least one of hexagonal boron nitride, graphene, molybdenum disulfide, carbon nanotubes and halloysite nanotubes.
[0011] Based on the first aspect, in one embodiment, the aramid fiber product is an aramid nanofiber bundle, and preparing the mixed liquid or mixed colloid as the aramid nanofiber bundle includes the following steps: sealing the mixed liquid or mixed colloid in a spinning device; using deionized water as a coagulation bath, wet spinning the mixed liquid or mixed colloid through a spinning device to obtain formed hydrogel fibers; and drying the formed hydrogel fibers to obtain the aramid nanofiber bundle.
[0012] Based on the first aspect, in one implementation, the spinning rate of the wet spinning is 10 μl / min-500 μl / min; and the diameter of the aramid nanofiber bundle is 15 μm-500 μm.
[0013] Based on the first aspect, in one embodiment, in the wet spinning process, the common models of the spinning needle tubes used are 20G (inner diameter is 0.23mm) to 32G (inner diameter is 0.8mm).
[0014] Based on the first aspect, in one embodiment, the aramid fiber product is an aramid nanofiber membrane, and the mixed liquid or mixed colloid is made into the aramid nanofiber membrane, which includes the following steps: after adjusting the temperature viscosity of the mixed liquid or mixed colloid, the viscosity of the mixed liquid or mixed colloid is 350mPa / s-10500mPa / s; forming the mixed liquid or mixed colloid into a film; and transferring the film to a polar solvent for quenching and forming, and obtaining the aramid nanofiber membrane after drying.
[0015] Based on the first aspect, the viscosity test method is a rotational viscometer with a rotation speed of 6 rpm.
[0016] Based on the first aspect, in one embodiment, the viscosity adjustment step is specifically: heating the mixed liquid or mixed colloid to 40°C-100°C or placing the mixed liquid or mixed colloid into a magnetic stirrer for stirring, and the stirring speed is 50rpm-500rpm.
[0017] Based on the first aspect, in one implementation, in the step of forming the mixed liquid or mixed colloid into a thin film, a forming method such as spin coating, flow coating, and blade coating can be used.
[0018] The present application utilizes the cracking and dispersing ability of trifluoromethanesulfonic acid or chlorosulfonic acid on aramid fibers to prepare a stable mixed solution or mixed colloid, i.e., a dispersed colloid of aramid fibers. The mixed solution or mixed colloid can be processed into aramid fiber products with high elongation at break and high fracture toughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a transmission electron microscope image of the aramid nanofiber bundle prepared in Example 1.
[0020] Figure 2 This is a scanning electron microscope image of the aramid nanofiber bundle prepared in Example 1.
[0021] Figure 3 This is a scanning electron microscope image of the aramid nanofiber bundle prepared in Example 1 from another angle.
[0022] Figure 4 This is the X-ray diffraction pattern of the aramid nanofiber bundle prepared in Example 1.
[0023] Figure 5 This is a scanning electron microscope image of the aramid nanofiber membrane prepared in Example 2.
[0024] Figure 6 This is a scanning electron microscope image of the nanomaterial and aramid fiber composite prepared in Example 7. DETAILED DESCRIPTION
[0025] The embodiments of the present application are described in detail below. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application. The reagents and materials described in the following embodiments can all be obtained from commercial sources.
[0026] An embodiment of the present application provides a method for preparing an aramid fiber product, comprising the following steps:
[0027] Step 1, washing the aramid fiber and drying it;
[0028] In some embodiments, the washing solution used for washing the aramid fiber is any one of ethanol, deionized water, acetone, saline solution, and isopropanol. The washing solution is blended with the aramid fiber, and the washing is completed by filtering. This process is repeated twice to obtain a clean aramid fiber with no impurities on the surface.
[0029] In some embodiments, the aramid fiber is a commercially available high-crystalline aramid fiber or aramid fiber pulp and other forms of polymers obtained based on aramid products.
[0030] In some embodiments, the temperature of the drying process can be adjusted to 40° C.-200° C., and the time of the drying process is 1 hour-24 hours.
[0031] Step 2, adding a super acid to the washed and dried aramid fiber to fully dissolve it to obtain a mixed solution or a mixed colloid, wherein the super acid is at least one of trifluoromethanesulfonic acid and chlorosulfonic acid;
[0032] The purpose of adding trifluoromethanesulfonic acid or chlorosulfonic acid to the washed and dried aramid fiber is to utilize the cracking and dispersing ability of trifluoromethanesulfonic acid or chlorosulfonic acid on the aramid fiber to prepare a mixed liquid or mixed colloid.
[0033] In some embodiments, in the aramid fiber / the trifluoromethanesulfonic acid or chlorosulfonic acid, the aramid fiber content is 1 mg / ml-100 mg / ml.
[0034] In some embodiments, nanomaterials may be added to the washed and dried aramid fibers, and the nanomaterials may be any one of carbon nanotubes, hexagonal boron nitride, graphene, molybdenum disulfide, and halloysite nanotubes.
[0035] In some embodiments, the nanomaterial is added to the washed and dried aramid fiber. During the dissolution process, the mixed liquid or mixed colloid can be dispersed in an emulsifier. The dispersion speed of the emulsifier is 7000rpm-24000rpm. The purpose of adding the emulsifier is to effectively disperse and mix to obtain a uniform and stable mixed liquid or mixed colloid.
[0036] In some embodiments, the dissolution temperature is 25°C-120°C, and the dissolution time is 0.5h-72h.
[0037] Step 3: Prepare aramid fiber products from the mixed solution or mixed colloid. The aramid fiber products may have higher strength, elongation at break and fracture toughness.
[0038] The aramid fiber product may specifically be an aramid nanofiber bundle or an aramid nanofiber membrane.
[0039] Taking the aramid fiber product as an aramid nanofiber bundle as an example, an embodiment of the present application further provides a method for preparing the aramid nanofiber bundle, comprising the following steps:
[0040] Step 1, sealing the mixed liquid or mixed colloid in a spinning device;
[0041] In some embodiments, the spinning device is specifically a glass or tetrafluoroethylene needle tube.
[0042] Step 2, using deionized water as a coagulation bath, and wet spinning the mixed solution or mixed colloid through a spinning device to obtain formed hydrogel fibers;
[0043] In some embodiments, the spinning rate of wet spinning is 10 μl / min-500 μl / min, the purpose of which is to ensure that the fibers obtained by wet spinning can be well formed and continuously produced.
[0044] Step three, drying the formed hydrogel fibers to obtain the aramid nanofiber bundles.
[0045] In some embodiments, the diameter of the aramid nanofiber bundle is 15 μm-500 μm.
[0046] In some embodiments, the specific method of drying treatment is natural drying, stretch drying, drying and other common fiber processing and collection methods.
[0047] Taking the aramid fiber product as an aramid nanofiber membrane as an example, an embodiment of the present application further provides a method for preparing the aramid nanofiber membrane, comprising the following steps:
[0048] Step 1, adjusting the viscosity of the mixed liquid or mixed colloid, the viscosity is 350mPa / s-10500mPa / s, the above viscosity testing method is a rotational viscometer, the rotation speed is 6rpm; by adjusting the viscosity to achieve good molding of the mixed liquid or mixed colloid under different processing conditions, such as the rotation speed and time in the spin coating process; the scraper speed and height in the scraping process.
[0049] In some embodiments, the viscosity adjustment step is specifically as follows: heating the mixed liquid or mixed colloid to 40°C-100°C or placing the mixed liquid or mixed colloid into a magnetic stirrer for stirring, and the stirring speed is 50rpm-500rpm. The stirring speed is adjusted to within the range of 50rpm-500rpm, the purpose of which is to make the temperature inside the mixed liquid or mixed colloid uniform and not introduce bubbles due to stirring.
[0050] Step 2, forming the mixed liquid or mixed colloid into a film;
[0051] In some embodiments, the film is prepared in a dry fume hood or an inert gas glove box.
[0052] In some embodiments, in the step of molding the mixed liquid or mixed colloid into a thin film, spin coating, flow rock, scraper coating and other molding methods can be used. Among them, when the thin film is prepared by the spin coating molding method, the temperature of the spin coater is 40°C-100°C, the spin coating rate is 100rpm-20000rpm, and the spin coating time is 1s-300s. The spin coating substrate material is any one of silicon wafer, stainless steel or other flat surface corrosion-resistant plate. The above-mentioned spin coating rate is set within the range of 100rpm-20000rpm to control the thickness of the aramid nanofiber membrane and shake off excess mixed liquid or mixed colloid.
[0053] Step 3, transferring the film to a polar solvent for quenching and forming, and drying to obtain the aramid nanofiber membrane. The aramid nanofiber membrane prepared by the trifluoromethanesulfonic acid processing method has a better material peeling effect, so it appears as a transparent film on a macro scale, effectively expanding the performance space of new aramid products.
[0054] In some embodiments, the polar solvent is water or any other polar solution that meets the requirements.
[0055] The following is an explanation of the preparation method of the aramid fiber product of the present application through specific examples and comparative examples. Those skilled in the art should understand that the preparation method described in the present application is only an example, and any other suitable preparation method is within the scope of the present application.
[0056] Example 1
[0057] The preparation steps of aramid nanofiber bundles are as follows:
[0058] S1: Provide 500 mg aramid fiber, 10 ml trifluoromethanesulfonic acid, and ethanol;
[0059] S2: After washing the aramid fiber with ethanol, the aramid fiber is placed in an oven for drying at a temperature of 120° C. for 2 h;
[0060] S3: adding trifluoromethanesulfonic acid to the washed and dried aramid fiber to dissolve it at a dissolving temperature of 90° C. for 18 hours to obtain a yellow uniform and transparent mixed liquid or mixed colloid;
[0061] S4: Take 400 μl of the above mixed solution or mixed colloid and seal it in a 1 ml syringe;
[0062] S5: using deionized water as a coagulation bath, wet spinning the mixed solution or mixed colloid to obtain formed hydrogel fibers, wherein the spinning rate of the wet spinning is 100 μl / min, and the spinning needle model is 30G;
[0063] S6: using a wind tube with a diameter of 5 cm to collect and dry the formed hydrogel fibers to prepare aramid nanofiber bundles, wherein the diameter of the aramid nanofiber bundles is 30 μm.
[0064] The aramid nanofiber bundles prepared in Example 1 were tested by transmission electron microscopy and scanning electron microscopy. Figure 1 This is a transmission electron microscope image of aramid nanofiber bundles. Figure 2 and Figure 3 This is a scanning electron microscope image of aramid nanofiber bundles. Figure 1 As shown in the figure, it can be found that the aramid fibers are transformed into highly entangled aramid nanofiber bundles, which provide new processing characteristics and physicochemical properties. Figure 2 and Figure 3 As shown, the surface of the aramid fiber bundle obtained by wet spinning presents a wrinkled morphology different from that of traditional aramid, and the cross section has an obvious entangled network structure composed of aramid nanofibers and fiber bundles.
[0065] The aramid nanofiber bundles prepared in Example 1 were subjected to X-ray diffraction test. Figure 4 is the X-ray diffraction pattern of aramid nanofiber bundle. Figure 4 As shown, after superacid treatment, the aramid fibers are converted into aramid nanofiber bundles with lower crystallinity.
[0066] Example 2
[0067] The preparation steps of aramid nanofiber membrane are as follows:
[0068] S1-1: Provide 500 mg of aramid fiber, 10 ml of trifluoromethanesulfonic acid, and ethanol;
[0069] S1-2: After washing the aramid fiber with ethanol, the aramid fiber is placed in an oven for drying at a temperature of 120° C. for 2 h;
[0070] S1-3: adding trifluoromethanesulfonic acid to the washed and dried aramid fiber to dissolve it at a dissolving temperature of 90° C. for 18 hours to obtain a yellow uniform and transparent mixed liquid or mixed colloid;
[0071] S1-4: The mixed liquid or mixed colloid is heated to 90° C. to adjust the viscosity. The viscosity of the mixed liquid or mixed colloid is 2480 mPas. The viscosity is tested by a rotational viscometer at a rotation speed of 6 rpm.
[0072] S1-5: forming the mixed liquid or mixed colloid into a thin film by spin coating, specifically: heating the temperature of a spin coater placed in a glove box to 90° C., selecting an appropriate amount of the mixed liquid or mixed colloid after adjusting the viscosity and adding it to the silicon wafer, placing it in a spin coater with a spin coating speed of 500 rpm and pre-spin coating for 30 seconds to complete the uniform coating, and then adjusting the spin coating speed of the spin coater to 6000 rpm, rotating for 60 seconds to complete the film forming;
[0073] S1-6: transferring the film into water through a sealed box for quenching and forming to obtain a formed aramid nanofiber membrane;
[0074] S1-7: The formed aramid nanofiber membrane is suspended in a four-sided controlled manner and dried.
[0075] The aramid nanofiber membrane of Example 2 was tested by scanning electron microscopy. Figure 5 This is a scanning electron microscope image of the aramid nanofiber membrane. Figure 5 As shown, the aramid nanofiber membrane prepared by this method has obvious skin-core, and the aramid nanofiber membrane is an ultra-thin structure with a thickness of 500nm. Its microstructure shows that it is significantly different from the traditional alkaline lysis method.
[0076] Example 3
[0077] The difference between Example 3 and Example 1 and Example 2 is that 500 mg of aramid fiber in step S1 and step S1-1 is replaced by 300 mg of aramid fiber, and the other conditions / preparation methods are the same.
[0078] Example 4
[0079] The difference between Example 4 and Example 1 and Example 2 is that 500 mg of aramid fiber in step S1 and step S1-1 is replaced by 200 mg of aramid fiber, and the other conditions / preparation methods are the same.
[0080] Example 5
[0081] The difference between Example 5 and Example 1 and Example 2 is that 500 mg of aramid fiber in step S1 and step S1-1 is replaced by 1000 mg of aramid fiber, and the other conditions / preparation methods are the same.
[0082] Example 6
[0083] The difference between Example 6 and Example 1 and Example 2 is that 10 ml of trifluoromethanesulfonic acid in step S1 and step 1-1 is replaced by 10 ml of chlorosulfonic acid, and the other conditions / preparation methods are the same.
[0084] Example 7
[0085] The difference between Example 7 and Example 2 is that in step S1-3, the step of adding trifluoromethanesulfonic acid to the washed and dried aramid fibers for dissolution is replaced by adding trifluoromethanesulfonic acid and carbon nanotubes to the washed and dried aramid fibers for dissolution. An emulsifier is added to assist in dispersion during the dissolution process. The dispersion speed of the emulsifier is 7000 rpm. The nanomaterial aramid composite is prepared. The scanning electron microscope image of the carbon nanotube and aramid fiber composite is as follows: Figure 6 As shown, the rest of the conditions / preparation methods are the same.
[0086] The composite of the nanomaterial and aramid fiber of Example 7 was tested by scanning electron microscopy. Figure 6 This is a scanning electron microscope image of the aramid nanofiber membrane. Figure 6 As shown, in the composite film of aramid fiber and carbon nanotubes prepared by the doctor blade coating method, the carbon nanotubes and aramid are in close contact, and the carbon nanotubes are well dispersed and well oriented.
[0087] Comparative Example 1
[0088] The difference between Comparative Example 1 and Example 1 and Example 2 is that 500 mg of aramid fiber in step S1 and step S1-1 is replaced by 5 mg of aramid fiber, and the other conditions / preparation methods are the same.
[0089] Comparative Example 2
[0090] The difference between Comparative Example 2 and Example 1 and Example 2 is that 500 mg of aramid fiber in step S1 and step S1-1 is replaced by 2000 mg of aramid fiber, and the other conditions / preparation methods are the same.
[0091] Comparative Example 3
[0092] The difference between Comparative Example 3 and Example 1 and Example 2 is that the heat treatment temperature of 90°C in step S3 and step S1-3 is replaced by a heat treatment temperature of 0°C, and the heat treatment time of 18h is replaced by a heat treatment time of 0.3h, and the other conditions / preparation methods are the same.
[0093] Comparative Example 4
[0094] The difference between Comparative Example 4 and Example 1 and Example 2 is that the heat treatment temperature of 90°C in step S3 and step S1-3 is replaced by a heat treatment temperature of 140°C, and the heat treatment time of 18h is replaced by a heat treatment time of 108h, and the other conditions / preparation methods are the same.
[0095] Performance Testing
[0096] The mechanical properties of the aramid nanofiber bundles prepared in Example 1 were tested using a universal testing machine. Six aramid nanofiber bundle samples (sample numbers 1-6) were taken and the aramid nanofiber bundle samples No. 1-6 were tested respectively. The test results are shown in Table 1:
[0097] Table 1 Mechanical properties of 1-6 aramid nanofiber bundle samples prepared in Example 1
[0098] Sample No. Breaking strength(Mpa) Fracture strain (%) <![CDATA[Toughness (MJ / m 3 )]]> 1 443.53 218.42 620.35 2 438.56 226.37 612.92 3 450.74 236.86 632.12 4 432.81 231.33 629.42 5 445.19 226.85 624.49
[0099] As can be seen from Table 1, compared with the 2% elongation at break of the original aramid fiber, the aramid nanofiber bundles prepared by trifluoromethanesulfonic acid have high elongation at break and fracture toughness due to the entanglement of the aramid nanofiber bundles to form amorphous fibers, which greatly broadens the performance range of the aramid nanofiber bundles.
[0100] The mechanical properties of the aramid nanofiber membrane prepared in Example 2 were tested using a universal testing machine. Two aramid nanofiber membrane samples (sample numbers 1-2) were taken and the aramid nanofiber membrane samples 1-2 were tested respectively. The test results are shown in Table 2:
[0101] Table 2 Mechanical properties of aramid nanofiber membrane samples No. 1-2 of Example 2
[0102] Sample No. Breaking strength(Mpa) Fracture strain (%) <![CDATA[Toughness (MJ / m 3 )]]> 1 980.84 79.78 488.66 2 1177.66 42.02 326.70
[0103] The mechanical properties of the aramid nanofiber bundles prepared in Examples 3-6 and Comparative Examples 1-4 were tested using a universal testing machine. The test results are shown in Table 3:
[0104] Table 3 Mechanical properties of aramid nanofiber bundles of Examples 3-6 and Comparative Examples 1-4
[0105] Example / Comparative Example Breaking strength(Mpa) Fracture strain (%) <![CDATA[Toughness (MJ / m 3 )]]> Example 3 423.76 98.36 489.74 Example 4 225.83 146.66 344.81 Example 5 447.74 43.55 145.53 Example 6 367.13 46.89 126.86 Comparative Example 1 / / / Comparative Example 2 / / / Comparative Example 3 / / / Comparative Example 4 / / /
[0106] Note: “ / ” in Table 3 means there is no corresponding parameter.
[0107] In combination with Table 1 and Table 3, the aramid nanofiber bundles prepared by trifluoromethanesulfonic acid or chlorosulfonic acid in Example 1 and Example 3-6 greatly improve the elongation at break and fracture toughness of the aramid nanofiber bundles compared to the 2% elongation at break of the original aramid fiber.
[0108] Compared with Example 1 (aramid fiber / trifluoromethanesulfonic acid is 50 mg / ml), the amount of aramid fiber added in Comparative Example 1 (aramid fiber / trifluoromethanesulfonic acid is less than 1 mg / ml) is too little, which makes it difficult to shape the aramid fiber during subsequent processing. Compared with Example 1, the amount of aramid fiber added in Comparative Example 2 (aramid fiber / trifluoromethanesulfonic acid is greater than 100 mg / ml) is too much, which makes the viscosity of the prepared aramid nanofiber bundle too high, causing processing difficulties. Therefore, based on the total volume of the aramid fiber and the superacid, when the content of the aramid fiber meets the range of 1 mg / ml-100 mg / ml, the prepared aramid nanofiber bundle has high elongation at break and fracture toughness, and can be better processed later.
[0109] Compared with Example 1 (dissolution temperature of 90°C and heat treatment time of 19h), Comparative Example 3 (dissolution temperature of 0°C and time of 0.3h) lowered the dissolution temperature and time, and the aramid fiber could not be completely dissolved, resulting in the inability to prepare the formed aramid nanofiber bundles; Comparative Example 4 (dissolution temperature of 140°C and dissolution time of 108h) increased the heat treatment temperature and time compared with Example 1, and trifluoromethanesulfonic acid evaporated during the preparation process, thus failing to prepare the formed aramid nanofiber bundles. Therefore, when the dissolution temperature is 25°C-120°C and the dissolution time is 0.5h-72h, the prepared aramid nanofiber bundles have high elongation at break and fracture toughness, and can be better processed later.
[0110] The mechanical properties of the nanomaterial and aramid fiber composite prepared in Example 7 were tested using a universal testing machine. Two composite samples of nanomaterial and aramid fiber (sample numbers 1-2) were taken, and the composite samples of nanomaterial and aramid fiber No. 1-2 were tested respectively. The test results are shown in Table 4:
[0111] Table 4 Mechanical properties of the composite samples of nanomaterial No. 1-2 and aramid fiber in Example 7
[0112] Sample No. Breaking strength(Mpa) Fracture strain (%) <![CDATA[Toughness (MJ / m 3 )]]> 1 897.97 16.79 71.62 2 1177.75 22.53 121.66
[0113] The above implementation modes are only used to illustrate the technical solutions of the present application and are not intended to limit the present application. Although the present application is described in detail with reference to the above implementation modes, a person skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present application.
Claims
1. A method for preparing an aramid fiber product, characterized in that: The following steps are involved: Washing aramid fibers and drying; Adding a super acid to the washed and dried aramid fiber to dissolve it and obtain a mixed solution or a mixed colloid, wherein the super acid is at least one of trifluoromethanesulfonic acid and chlorosulfonic acid; The mixed liquid or the mixed colloid is made into the aramid fiber product; The dissolution temperature is 25° C.-120° C., and the dissolution time is 0.5 h-72 h. Based on the total volume of the aramid fiber and the superacid, the content of the aramid fiber is 1 mg / ml-100 mg / ml.
2. The method for preparing an aramid fiber product according to claim 1, characterized in that: The aramid fiber is washed with a washing solution, and the washing solution is any one of ethanol, deionized water, acetone, saline solution and isopropanol.
3. The method for preparing an aramid fiber product according to claim 1, characterized in that: The aramid fiber product is a composite of nanomaterials and the aramid fiber. Before the mixed liquid or the mixed colloid is made into the aramid fiber product, the preparation method further includes: adding the nanomaterial to the washed and dried aramid fiber, and dispersing the mixed liquid or the mixed colloid with an emulsifier, and the dispersing speed of the emulsifier is 7000rpm-24000rpm.
4. The method for preparing an aramid fiber product according to claim 3, characterized in that: The nano material is at least one of hexagonal boron nitride, graphene, molybdenum disulfide, carbon nanotubes and halloysite nanotubes.
5. The method for preparing an aramid fiber product according to claim 1, characterized in that: The aramid fiber product is an aramid nanofiber bundle, and preparing the mixed liquid or the mixed colloid into the aramid nanofiber bundle includes the following steps: Sealing the mixed liquid or the mixed colloid in a spinning device; Using deionized water as a coagulation bath, wet spinning the mixed solution or the mixed colloid through a spinning device to obtain formed hydrogel fibers; and The formed hydrogel fibers are dried to obtain the aramid nanofiber bundles.
6. The method for preparing an aramid fiber product according to claim 5, characterized in that: The spinning rate of the wet spinning is 10 μl / min-500 μl / min; the diameter of the aramid nanofiber bundle is 15 μm-500 μm.
7. The method for preparing an aramid fiber product according to claim 1, characterized in that: The aramid fiber product is an aramid nanofiber membrane, and preparing the mixed solution or the mixed colloid into the aramid nanofiber membrane comprises the following steps: Adjusting the viscosity of the mixed liquid or the mixed colloid to 350 mPa / s-10500 mPa / s; forming the mixed liquid or the mixed colloid into a film; and The film is transferred to a polar solvent for quenching and forming, and the aramid nanofiber membrane is obtained after drying.
8. The method for preparing an aramid fiber product according to claim 7, characterized in that: The viscosity adjustment step is specifically: heating the mixed liquid or the mixed colloid to 40°C-100°C.
9. The method for preparing an aramid fiber product according to claim 7, characterized in that: The method of forming the mixed liquid or the mixed colloid into a thin film is specifically any one of extrusion, blade coating and spin coating.
Citation Information
Cited By
Preparation method of ultrafine aramid nanofiber dispersion liquid
CN121736320A
Preparation method of superfine aramid nanofiber dispersion liquid
CN121736320B