Preparation method of folium artemisiae argyi volatile oil nano-silver mixture

By optimizing the distillation process and chemical reduction method to prepare a mixture of nano-silver from Artemisia argyi volatile oil, the problems of nano-silver stability and extract consistency were solved, achieving efficient and environmentally friendly mixture preparation with broad application prospects.

CN118948917AInactive Publication Date: 2024-11-15HUBEI UNIV OF CHINESE MEDICINE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958880.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing technology, the preparation process of the mixture of Artemisia argyi volatile oil and nano silver has problems such as poor stability of nano silver particles, inconsistency caused by differences in extract components, and loss of bioactivity.

Method used

Artemisia argyi volatile oil was extracted by precisely controlling the distillation temperature and time. Nano-silver was prepared using appropriate reducing agents and stabilizers. Artemisia argyi volatile oil and nano-silver were mixed under specific conditions, and surfactants were added to improve stability and bioactivity.

Benefits of technology

It significantly improves the extraction efficiency of Artemisia argyi volatile oil and the stability of nano-silver, ensuring the uniformity and bioactivity of the mixture, and the method is environmentally friendly and economical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118948917A_ABST
    Figure CN118948917A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of preparation of Chinese mugwort nano-silver compounds, and discloses a preparation method for preparing a nano-silver Chinese mugwort mixture from Chinese mugwort leaf volatile oil and application of the nano-silver Chinese mugwort mixture. According to the silver nitrate preparation method, a modified SSZ-13 chabazite molecular sieve chelating adsorbent is adopted for adsorption and filtration, the SSZ13 chabazite molecular sieve chelating adsorbent has very high adsorption capacity on chlorides, sulfides and metal ions contained in an industrial-grade silver nitrate solution, impurities in the industrial-grade silver nitrate solution can be effectively removed, and the purity of silver nitrate is greatly improved; therefore, the quality of the Chinese mugwort nano-silver compound is improved; meanwhile, high-quality absolute ethyl alcohol is prepared through an absolute ethyl alcohol preparation method, so that the quality of the Chinese mugwort nano-silver compound is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of mugwort leaf volatile oil nano-silver complexes, and in particular relates to a new method for preparing a mugwort leaf volatile oil nano-silver mixture. Background Art

[0002] Some problems exist in the traditional preparation process of the mixture of wormwood volatile oil and nano-silver. They mainly include how to improve the extraction efficiency of wormwood volatile oil, ensure the dispersibility and stability of nano-silver, and how to control various conditions in the mixing process of wormwood volatile oil and nano-silver to obtain a mixture of wormwood volatile oil and nano-silver with excellent biological activity and stability.

[0003] In the prior art, plant extracts are used to synthesize silver nanoparticles, and the bioactive properties of plant extracts are utilized in the process. This method is generally regarded as an environmentally friendly, low-cost and effective method for synthesizing nanomaterials.

[0004] Prior art: using a specific plant extract (such as tea extract, chamomile extract, etc.) to reduce silver ions to synthesize nanosilver. This method generally includes mixing a silver ion solution with a plant extract and reacting under specific conditions (such as a specific temperature and pH value) to form nanosilver particles.

[0005] Technical problems existing in the existing technology:

[0006] 1. Stability issue: When using plant extracts to synthesize nanosilver, the stability of nanosilver particles is a problem. Due to the complex chemical composition of plant extracts, nanosilver particles are prone to aggregation, affecting their long-term stability and uniformity.

[0007] 2. Standardization of extracts: Differences in composition between different plant extracts result in differences in the size, shape, and biological activity of synthesized nanosilver particles. Therefore, it is difficult to standardize the production process, affecting the consistency and predictability of the final product.

[0008] 3. Retention of biological activity: During the synthesis of nanosilver, the bioactive components of plant extracts are affected by heat or chemical reactions, thereby reducing their effectiveness. Summary of the invention

[0009] In view of the problems existing in the prior art, the present invention provides a preparation method and application of a nano-silver wormwood mixture by using wormwood volatile oil.

[0010] The present invention is achieved by a method for preparing a mixture of wormwood volatile oil and nano-silver. The following are the complete steps of the method for preparing the mixture of wormwood volatile oil and nano-silver:

[0011] 1. Extraction of volatile oil from Artemisia argyi:

[0012] 1.1. Select suitable distillation equipment, such as a fractionating tower or rotary evaporator.

[0013] 1.2. Place the mugwort leaves into the distillation equipment and add an appropriate amount of water or organic solvent (such as alcohol or ether).

[0014] 1.3. Precisely control the distillation temperature and time to ensure that distillation is carried out under optimal conditions. The time and temperature of this process need to be adjusted according to laboratory conditions and the equipment used.

[0015] 1.4. Collect the distillate, i.e. volatile oil from mugwort leaves.

[0016] 2. Preparation of Nanosilver:

[0017] 2.1. Dissolve a silver salt (such as silver nitrate) in an appropriate solution.

[0018] 2.2. Add an appropriate amount of reducing agent (such as sodium hydroxide or sodium borohydride) to the solution to reduce the silver ions to nanosilver.

[0019] 2.3. Add an appropriate amount of stabilizer, such as polyvinyl pyrrolidone (PVP) or citric acid, during the process to prevent the aggregation of nanosilver and ensure its dispersion and stability.

[0020] 3. Mixture of wormwood essential oil and nano silver:

[0021] 3.1. Mix the wormwood volatile oil and nano-silver under precisely controlled conditions, such as temperature, pH value and the ratio of wormwood volatile oil to nano-silver.

[0022] 3.2. During the mixing process, some surfactants, such as sodium dodecyl sulfate (SDS) or polysorbate 80, are added to increase the stability of the mixture and improve its biological activity.

[0023] 4. Post-processing:

[0024] 4.1. Cool the mixture to room temperature and then remove unreacted materials and large particles by centrifugation or filtration.

[0025] 4.2. Collect and dry the mixture to obtain the Artemisia argyi volatile oil and nanosilver mixture.

[0026] The above are the complete steps for preparing the mixture of wormwood essential oil and nanosilver. In each step, appropriate adjustments need to be made according to the experimental conditions and results to optimize the extraction and preparation process and improve the quality and stability of the product.

[0027] Further, including:

[0028] 1.2. Place the mugwort leaves in a distillation device and add an appropriate amount of water or organic solvent (such as alcohol or ether):

[0029] It is necessary to use about 500 grams of fresh wormwood leaves and use anhydrous ethanol as an organic solvent. The volume of anhydrous ethanol should be about 10 times the mass of the wormwood leaves, that is, about 5 liters.

[0030] This protocol aims to clarify the specific operating steps and precautions for extracting volatile oil from Artemisia argyi using anhydrous ethanol as a solvent.

[0031] 2. Materials and Equipment

[0032] 1. Materials: 500 grams of fresh mugwort leaves, anhydrous ethanol (purity is selected according to actual needs, such as 99.9%, 95% or 70%).

[0033] 2. Equipment: volatile oil extraction device or distillation equipment (including heating device, condenser, collecting bottle, etc.), crusher, electronic balance, weighing paper, beaker, glass rod, etc.

[0034] 3. Operation steps

[0035] 1. Preparation of mugwort leaves: Use a grinder to crush the fresh mugwort leaves into pieces of appropriate size so that they can better contact with the solvent and improve the extraction efficiency.

[0036] 2. Weighing: Use an electronic balance to accurately weigh 500 grams of crushed mugwort leaves.

[0037] 3. Solvent preparation: Prepare an appropriate amount of anhydrous ethanol according to the mass of the wormwood leaves. Generally speaking, the volume of anhydrous ethanol should be about 10 times the mass of the wormwood leaves, that is, about 5 liters.

[0038] 4. Extraction:

[0039] The crushed mugwort leaves are placed into a volatile oil extraction device or a distillation device.

[0040] Add the prepared anhydrous ethanol.

[0041] Turn on the heating device to allow the anhydrous ethanol and moxa leaves to fully contact and heat for reflux extraction. The extraction time can be adjusted according to the actual situation. It is generally recommended to extract 2-3 times, each time for about 2 hours.

[0042] During the extraction process, the volatilized oil gas is condensed into liquid through a condenser and flows into a collection bottle.

[0043] 5. Collection and storage: Collect the extracted volatile oil and store it in a sealed container to avoid volatilization and oxidation.

[0044] IV. Precautions

[0045] 1. Pay attention to safety during operation to avoid splashing or contact of anhydrous ethanol with sensitive parts such as skin and eyes.

[0046] 2. During the extraction process, the heating temperature and time must be controlled to avoid excessively high temperatures that may cause destruction of volatile oil components or burning of solvents.

[0047] 3. After the extraction is completed, turn off the heating device and clean the equipment in time for next use.

[0048] V. Suggestions for follow-up work

[0049] 1. Perform quality testing and analysis on the extracted volatile oil to determine its composition and purity.

[0050] 2. Based on actual demand and market research, consider further processing of volatile oils or application to develop new products.

[0051] 3. Properly handle the waste generated during the extraction process to avoid pollution to the environment.

[0052] The above scheme can systematically complete the extraction of volatile oil from Artemisia argyi and ensure that the extraction effect and quality meet the expected requirements.

[0053] 1.3. Precisely control the distillation temperature and time to ensure distillation under optimal conditions:

[0054] For the distillation of volatile oil from mugwort leaves, it needs to be carried out at a temperature of 80 degrees Celsius and last for about 3 hours. This process needs to be carried out according to the operating manual of the equipment or the manufacturer's recommendations to ensure optimal efficiency and yield.

[0055] 3.1. Mixing wormwood essential oil and nanosilver under precisely controlled conditions, such as temperature, pH value and the ratio of wormwood essential oil to nanosilver:

[0056] In order to prepare the mixture of wormwood essential oil and nano-silver, it is necessary to proceed at room temperature to prevent excessive temperature from affecting the stability of the mixture. The pH value should be in the range of 7-8 to ensure that both the wormwood essential oil and the nano-silver are in a stable state.

[0057] When adding wormwood essential oil and nanosilver, it is necessary to follow a 1:1 volume ratio. This ratio can be adjusted based on experimental results to optimize the properties of the mixture.

[0058] This protocol aims to clarify how to mix Artemisia argyi essential oil with nanosilver in a 1:1 volume ratio to ensure the uniformity and stability of the mixture.

[0059] 2. Materials and Equipment

[0060] 1. Materials: volatile oil of mugwort leaves, nano-silver powder, organic solvents (such as ethanol, methanol or isopropanol, etc.).

[0061] 2. Equipment: stirrer, ultrasonic generator, measuring cylinder, beaker, glass rod, etc.

[0062] 3. Operation steps

[0063] 1. Prepare nanosilver solution:

[0064] Select an appropriate organic solvent, such as ethanol.

[0065] Add an appropriate amount of organic solvent into the beaker.

[0066] According to the required volume ratio, a corresponding amount of nano silver powder is weighed and slowly added into the organic solvent.

[0067] Use a stirrer or ultrasonic generator to ensure that the nanosilver is evenly dispersed in the solvent to form a stable nanosilver solution or suspension.

[0068] 2. Mixing nanosilver solution and wormwood essential oil:

[0069] Use a measuring cylinder to accurately measure an equal volume of wormwood volatile oil to the nanosilver solution.

[0070] Slowly add the measured wormwood volatile oil into the nanosilver solution.

[0071] Stir gently with a blender or use an ultrasonicator to mix to ensure both are evenly mixed.

[0072] 3. Storage and use:

[0073] Store the mixed wormwood essential oil and nanosilver solution in a sealed container to avoid volatilization and oxidation.

[0074] When using, take an appropriate amount of the mixture as needed.

[0075] IV. Precautions

[0076] 1. Pay attention to safety during operation to avoid organic solvents splashing or contacting sensitive parts such as skin and eyes.

[0077] 2. Gently stir or use ultrasound during the mixing process to avoid destroying the uniform dispersion of nanosilver particles.

[0078] 3. During storage, ensure that the container is well sealed to prevent the mixture from volatilizing or being contaminated.

[0079] V. Suggestions for follow-up work

[0080] 1. Perform quality inspection and analysis on the mixed wormwood essential oil and nanosilver solution to determine its uniformity and stability.

[0081] 2. Consider further application development or experimental research on the mixture based on actual needs.

[0082] Through the above scheme, you can systematically complete the mixing of wormwood volatile oil and nanosilver and ensure the uniformity and stability of the mixture. Please note that this scheme is for reference only and needs to be adjusted and optimized according to actual conditions during specific operations. Further, including:

[0083] 1. Extraction of volatile oil from Artemisia argyi:

[0084] 1.1. The suitable distillation temperature and time are: 80 degrees Celsius, distillation time is 3 hours. These parameters need to be adjusted according to the type and quantity of wormwood leaves.

[0085] 1.2. As an organic solvent, anhydrous ethanol can be used, for example, the ratio is 1:10 (mugwort leaf: anhydrous ethanol).

[0086] 2. Preparation of Nanosilver:

[0087] 2.1. The concentration of silver nitrate is 0.01M and the concentration of reducing agent sodium hydroxide is 0.1M.

[0088] 2.2. The amount of the stabilizer PVP is 10% by weight of the silver nitrate.

[0089] Steps:

[0090] 1. Solution preparation:

[0091] Prepare 0.01 M silver nitrate solution and 0.1 M sodium hydroxide solution using deionized water.

[0092] According to the mass of silver nitrate, the required mass of PVP (10% of the mass of silver nitrate) was calculated and dissolved in deionized water.

[0093] 2. Preparation of Nanosilver:

[0094] Option 1 (equal volume mixing):

[0095] a. Add a certain volume of 0.01 M silver nitrate solution into the beaker under magnetic stirring.

[0096] b. Slowly add an equal volume of 0.1 M sodium hydroxide solution while maintaining magnetic stirring to ensure uniform reaction.

[0097] c. During the addition process, observe the color change of the solution and the formation of precipitation.

[0098] Option 2 (mixing by volume ratio of 10:1):

[0099] a. Add 10 volumes of 0.01 M silver nitrate solution to the beaker under magnetic stirring.

[0100] b. Slowly add 1 volume of 0.1 M sodium hydroxide solution dropwise while maintaining magnetic stirring.

[0101] c. Observe and record the phenomena during the reaction process.

[0102] 3. Stabilizer addition:

[0103] After the silver nanoparticles were generated, the pre-prepared PVP solution was immediately added to the reaction solution.

[0104] Continue stirring for a while to ensure that the stabilizer fully wraps the nanosilver particles.

[0105] 4. Post-processing:

[0106] Stop stirring and let the solution stand for a while to allow the unreacted ions and nanosilver particles to separate.

[0107] The silver nanoparticles are collected by centrifugation or filtration.

[0108] The nanosilver particles were washed with deionized water to remove excess ions and stabilizers.

[0109] Disperse the washed nanosilver particles in an appropriate amount of deionized water to form a nanosilver suspension. 3. Mixing of wormwood volatile oil and nanosilver:

[0110] 3.1. The mixing conditions are at room temperature, pH value is 7, and the ratio of wormwood volatile oil to nanosilver is 1:1 (volume ratio).

[0111] 3.2. The amount of surfactant SDS is 1% of the total volume of the mixture.

[0112] 4. Post-processing:

[0113] 4.1. Centrifuge at a speed of 10,000 rpm for 10 minutes.

[0114] Another object of the present invention is to provide a method for extracting wormwood volatile oil and preparing nanosilver, comprising the following steps: first, selecting suitable distillation equipment and extracting wormwood volatile oil, the process including precisely controlling the distillation temperature and time, and adding an appropriate amount of water or organic solvent, such as anhydrous ethanol, to maximize the extraction efficiency; second, preparing nanosilver by chemical reduction, the process including dissolving silver salt in an appropriate solution, adding a reducing agent such as sodium hydroxide, and introducing polyvinyl pyrrolidone (PVP) or citric acid as a stabilizer to prevent aggregation of nanosilver and ensure its dispersibility and stability.

[0115] Another object of the present invention is to provide a method for preparing a mixture of wormwood volatile oil and nanosilver, comprising the following steps: under precisely controlled conditions, such as specific temperature and pH value, mixing the extracted wormwood volatile oil with the prepared nanosilver in a predetermined ratio, wherein the ratio can be adjusted according to demand; during the mixing process, adding an appropriate amount of surfactant, such as sodium dodecyl sulfate (SDS), to enhance the stability of the mixture and improve its biological activity, thereby obtaining a mixture of wormwood volatile oil and nanosilver suitable for various applications.

[0116] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:

[0117] First, the preparation method of the wormwood volatile oil nano-silver mixture of the present invention has achieved significant technical progress:

[0118] 1. Improved extraction efficiency: By optimizing the distillation equipment and process, and using appropriate solvents, the present invention significantly improves the extraction efficiency of wormwood volatile oil, which not only increases the output of the product, but also reduces the production cost.

[0119] 2. Achieved efficient preparation and stability of nanosilver: By using appropriate reducing agents and stabilizers, the present invention successfully achieved efficient preparation and stability of nanosilver. This ensures uniform distribution and long-term stability of nanosilver, thereby improving the quality and durability of the product.

[0120] 3. Optimized mixing process: By precisely controlling the mixing conditions and adding appropriate surfactants, the present invention significantly optimizes the mixing process of wormwood volatile oil and nanosilver, which not only ensures the stability of the mixture but also improves its biological activity.

[0121] 4. Environmental protection and economy: The preparation method of the present invention does not need to use high energy consumption or harmful chemical reagents, which is both environmentally friendly and economical. In addition, since both wormwood and silver are abundant resources, the preparation method of the present invention has good economy and feasibility.

[0122] The method for preparing the wormwood volatile oil nano-silver mixture of the present invention has achieved remarkable technical progress in extraction efficiency, preparation stability, mixing optimization, environmental protection and economy, and has broad application prospects and commercial value.

[0123] Second, the method for preparing the mixture of wormwood volatile oil and nano-silver proposed in the present invention solves the problem of the stability of nano-silver particles in the prior art by optimizing the extraction process of wormwood volatile oil and improving the nano-silver preparation steps. In addition, it also includes using a surfactant to enhance the stability and biological activity of the final mixture, which provides a new solution for improving the prior art.

[0124] The invention solves some problems existing in the traditional preparation process of the mixture of wormwood leaf volatile oil and nano-silver, mainly including how to improve the extraction efficiency of wormwood leaf volatile oil, ensure the dispersibility and stability of nano-silver, and how to control various conditions in the mixing process of wormwood leaf volatile oil and nano-silver to obtain the mixture of wormwood leaf volatile oil and nano-silver with excellent biological activity and stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0125] Figure 1 It is a flow chart of a method for preparing a nano-silver wormwood mixture from wormwood volatile oil provided in an embodiment of the present invention;

[0126] Figure 2 It is a flow chart of the extraction method of wormwood volatile oil provided by an embodiment of the present invention;

[0127] Figure 3 is a flow chart of a method for preparing nanosilver provided in an embodiment of the present invention;

[0128] Figure 4 It is a flow chart of a method for mixing wormwood volatile oil and nano silver provided in an embodiment of the present invention;

[0129] Figure 5 It is a post-processing flow chart provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0130] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0131] The present invention mainly improves the following problems and defects of the prior art and achieves significant technical progress:

[0132] Extraction of volatile oil from mugwort leaves: By precisely controlling the mass ratio of mugwort leaves to anhydrous ethanol and distillation conditions (such as temperature and time), the extraction efficiency and purity of volatile oil can be effectively improved. This method overcomes the problem of low efficiency of traditional extraction technology.

[0133] Preparation of nanosilver: Using a specific ratio of silver nitrate, sodium hydroxide and PVP, effective reduction and stabilization of nanosilver is achieved. This solves the technical problem of excessive aggregation and poor stability of nanosilver.

[0134] Mixture of volatile oil from Artemisia argyi and nanosilver: By precisely controlling the pH value, volume ratio and adding an appropriate amount of surfactant (such as SDS), the stability and biological activity of the mixture were improved, and the adverse interactions and precipitation between the components were reduced.

[0135] Example 1: Preparation of Artemisia argyi volatile oil nanosilver mixture

[0136] Prepare 500 grams of fresh mugwort leaves and 5 liters of anhydrous ethanol.

[0137] Put mugwort leaves and anhydrous ethanol into a distiller, control the temperature to 80 degrees Celsius, and distill for 3 hours to extract mugwort volatile oil.

[0138] In another container, 0.01 M silver nitrate solution and 0.1 M sodium hydroxide solution were mixed, and polyvinyl pyrrolidone (PVP) was added as a stabilizer in an amount equal to 10% by weight of the silver nitrate to prepare nanosilver.

[0139] The extracted volatile oil from leaves of Artemisia argyi and the prepared nanosilver were mixed in a volume ratio of 1:1, and sodium dodecyl sulfate (SDS) was added as a surfactant in an amount equal to 1% of the volume of the mixture.

[0140] After the mixture was cooled to room temperature, unreacted substances and large particles were removed by centrifugation at 10,000 rpm for 10 minutes.

[0141] The mixture is collected and dried to obtain a mixture of Artemisia argyi volatile oil and nano-silver.

[0142] Example 2: Preparation of Artemisia argyi volatile oil nanosilver mixture and biological activity test

[0143] The Artemisia argyi volatile oil nano-silver mixture was prepared according to the steps of Example 1.

[0144] The prepared mixture is then tested for antimicrobial activity. Specifically, the mixture can be added to cultured bacteria, such as Escherichia coli or Staphylococcus aureus, and their growth observed.

[0145] The control group can be a culture medium to which only wormwood essential oil or nanosilver is added.

[0146] The antibacterial activity of the Artemisia argyi volatile oil-nanosilver mixture can be evaluated by comparing the bacterial growth between the experimental group and the control group.

[0147] like Figure 1As shown, the complete steps of the preparation method of the wormwood volatile oil nano-silver mixture provided by the present invention are:

[0148] Step S101, as Figure 2 As shown, extraction of volatile oil from Artemisia argyi:

[0149] 1.1. Select suitable distillation equipment, such as a fractionating tower or rotary evaporator.

[0150] 1.2. Place the mugwort leaves into the distillation equipment and add an appropriate amount of water or organic solvent (such as alcohol or ether).

[0151] 1.3. Precisely control the distillation temperature and time to ensure that distillation is carried out under optimal conditions. The time and temperature of this process need to be adjusted according to laboratory conditions and the equipment used.

[0152] 1.4. Collect the distillate, i.e. volatile oil from mugwort leaves.

[0153] Step S102, as Figure 3 As shown, the preparation of nanosilver:

[0154] 2.1. Dissolve a silver salt (such as silver nitrate) in an appropriate solution.

[0155] 2.2. Add an appropriate amount of reducing agent (such as sodium hydroxide or sodium borohydride) to the solution to reduce the silver ions to nanosilver.

[0156] 2.3. Add an appropriate amount of stabilizer, such as polyvinyl pyrrolidone (PVP) or citric acid, during the process to prevent the aggregation of nanosilver and ensure its dispersion and stability.

[0157] Step S103, as Figure 4 As shown, the mixture of mugwort essential oil and nanosilver:

[0158] 3.1. Mix the wormwood volatile oil and nano-silver under precisely controlled conditions, such as temperature, pH value and the ratio of wormwood volatile oil to nano-silver.

[0159] 3.2. During the mixing process, some surfactants, such as sodium dodecyl sulfate (SDS) or polysorbate 80, are added to increase the stability of the mixture and improve its biological activity.

[0160] In addition, if Figure 5 As shown, post-processing is also included:

[0161] 4.1. Cool the mixture to room temperature and then remove unreacted materials and large particles by centrifugation or filtration.

[0162] 4.2. Collect and dry the mixture to obtain the Artemisia argyi volatile oil and nanosilver mixture.

[0163] The above are the complete steps for preparing the mixture of wormwood essential oil and nanosilver. In each step, appropriate adjustments need to be made according to the experimental conditions and results to optimize the extraction and preparation process and improve the quality and stability of the product.

[0164] The present invention proposes a new method for preparing a mixture of wormwood essential oil and nano-silver. First, an optimized distillation process is used to extract wormwood essential oil, which includes selecting suitable distillation equipment and accurately controlling the distillation temperature and time to maximize the efficiency of extracting wormwood essential oil. This process also includes solution processing, such as adding an appropriate amount of water or organic solvent to improve distillation efficiency.

[0165] Next, an improved chemical reduction method is used to prepare nanosilver. In this process, an appropriate amount of stabilizer, such as polyvinyl pyrrolidone (PVP) or citric acid, is added to effectively prevent the aggregation of nanosilver and ensure the dispersibility and stability of nanosilver. Finally, under precisely controlled conditions, such as temperature, pH value and the ratio of wormwood volatile oil to nanosilver, wormwood volatile oil and nanosilver are mixed to obtain a wormwood volatile oil nanosilver mixture. In this process, some surfactants are also added to increase the stability of the mixture and improve its biological activity.

[0166] The present invention adopts a new method for preparing the mixture of wormwood essential oil and nanosilver. First, the wormwood essential oil is extracted through an optimized distillation process, which includes selecting suitable distillation equipment, accurately controlling the distillation temperature and time, and processing the solution, such as adding an appropriate amount of water or organic solvent, to maximize the extraction efficiency.

[0167] Secondly, an improved chemical reduction method is used to prepare nanosilver. In this process, an appropriate amount of stabilizer, such as polyvinyl pyrrolidone (PVP) or citric acid, is added to effectively prevent the aggregation of nanosilver and ensure its dispersibility and stability.

[0168] Finally, the present invention mixes the wormwood volatile oil and nano-silver under precisely controlled conditions, such as temperature, pH value and the ratio of wormwood volatile oil to nano-silver, to obtain a wormwood volatile oil nano-silver mixture. In this process, some surfactants are also added to increase the stability of the mixture and improve its biological activity.

[0169] The method for preparing the wormwood leaf volatile oil nano-silver mixture of the present invention can effectively improve the extraction efficiency of the wormwood leaf volatile oil, ensure the dispersibility and stability of the nano-silver, and obtain the wormwood leaf volatile oil nano-silver mixture with excellent biological activity and stability. In addition, the method is simple to operate, easy to implement, and has high practical value.

[0170] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a mixture of wormwood volatile oil and nano-silver, characterized in that: The following steps are involved: Select suitable distillation equipment; mix fresh mugwort leaves and anhydrous ethanol at a mass ratio of about 1:10, wherein the total amount of mugwort leaves is 500 grams; perform distillation under controlled conditions, specifically distillation at 80 degrees Celsius for 3 hours to maximize the extraction efficiency of mugwort leaf volatile oil; collect the liquid after distillation, which is the obtained mugwort leaf volatile oil; The method for extracting wormwood volatile oil includes the following steps: the amount of anhydrous ethanol used is exactly 10 times the mass of wormwood, and the anhydrous ethanol is anhydrous or low in water content, so as to improve the extraction purity and quality of wormwood volatile oil; The preparation method of the nano silver includes the following steps: dissolving 0.01 M silver nitrate in an aqueous solution as a source of silver ions; adding 0.1 M sodium hydroxide as a reducing agent to the solution to achieve effective reduction of the silver ions into nano silver; during the preparation process, adding polyvinyl pyrrolidone (PVP) equivalent to 10% of the weight of the silver nitrate as a stabilizer to prevent excessive aggregation of the nano silver and ensure its good dispersibility and stability in the solution.

2. The method for preparing the wormwood volatile oil nano-silver mixture as claimed in claim 1, characterized in that: The aqueous solution should be maintained at a neutral or slightly acidic pH to optimize the formation and stability of nanosilver.

3. The method for preparing the wormwood volatile oil nano-silver mixture as claimed in claim 1, characterized in that: The invention relates to a mixing method of wormwood essential oil and nano silver, The method comprises the following steps: at room temperature, mixing wormwood volatile oil and nanosilver in a volume ratio of 1:1, wherein the pH value is adjusted to 7-8 to maintain the stability of the mixture; during the mixing process, adding 1% of the total volume of sodium dodecyl sulfate (SDS) as a surfactant to improve the biological activity and stability of the mixture and reduce the interaction and precipitation between the components.

4. The method for preparing the wormwood volatile oil nano-silver mixture according to claim 3, characterized in that: By adding SDS surfactant, the applicability of the mixture in biological applications and pharmaceutical preparations is increased, and its stability and biological activity in vivo are improved.

5. The method for preparing the wormwood volatile oil nano-silver mixture according to claim 1, characterized in that: The post-processing method of the wormwood volatile oil nano-silver mixture is included. The method comprises the following steps: cooling the mixture to room temperature, and then purifying it by centrifugation or filtration, wherein the centrifugal speed is set to 10,000 rpm for 10 minutes to remove unreacted substances and large particles; collecting the purified mixture and drying it at low temperature to obtain the final wormwood volatile oil nanosilver mixture, which is suitable for industries such as medicine and cosmetics.

6. A method for extracting volatile oil from Artemisia argyi and preparing nanosilver, characterized in that: The method comprises the following steps: first, selecting suitable distillation equipment and extracting volatile oil from mugwort leaves, the process comprising precisely controlling the distillation temperature and time, and adding an appropriate amount of water or an organic solvent; second, preparing nanosilver by a chemical reduction method, the process comprising dissolving a silver salt in an appropriate solution, adding a reducing agent such as sodium hydroxide, and introducing polyvinyl pyrrolidone (PVP) or citric acid as a stabilizer to prevent the aggregation of nanosilver and ensure its dispersibility and stability.

7. The method for extracting wormwood volatile oil and preparing nano silver as claimed in claim 6, characterized in that: The preparation method of the wormwood volatile oil and nanosilver mixture comprises the following steps: under precisely controlled conditions, the extracted wormwood volatile oil and the prepared nanosilver are mixed in a predetermined ratio, wherein the ratio can be adjusted according to demand; during the mixing process, an appropriate amount of surfactant is added to enhance the stability of the mixture and improve its biological activity, thereby obtaining the wormwood volatile oil and nanosilver mixture suitable for various applications.