Preparation method of super-wetting film based on stainless steel mesh modification

By using dopamine hydrochloride and polyethylene glycol for modification on stainless steel network, a highly hydrophilic and wear-resistant superwetting film was prepared, which solved the problems of complex and poor stability of the existing oil-water separation film preparation process and achieved the Efficient and economical oil-containing wastewater treatment.

CN118949703APending Publication Date: 2024-11-15CHONGQING TECH & BUSINESS UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411156209.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing oil-water separation membrane preparation process is cumbersome, the conditions are harsh, the chemical stability is poor, the long-term operation stability is poor, the flux is not high, and it is easy to contaminate, and large-scale production is not suitable.

Method used

Using stainless steel mesh as the base film, dopamine hydrochloride and polyethylene glycol as crosslinking agent and modifier, ultra-wetting film is prepared by ultrasonic cleaning, impregnation and oven drying steps to form a high hydrophilicity and friction resistance. Super wetting film.

Benefits of technology

It realizes simple and low energy consumption film preparation, has high separation efficiency and flow rate, can operate for a long time and wear-resistant, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a super-wetting film based on stainless steel mesh modification. The preparation method of the super-wetting film comprises the following steps: cleaning a stainless steel mesh, polymerizing a layer of polydopamine on the stainless steel mesh by an impregnation method, cleaning with deionized water, and drying to obtain a polydopamine stainless steel mesh; then carrying out hydrophilic modification on the polydopamine stainless steel mesh by using polyethylene glycol, dipping the polydopamine stainless steel mesh into a polyethylene glycol solution, then taking out the polydopamine stainless steel mesh, cleaning, and drying to obtain the super-wetting membrane. The obtained super-wetting film shows good hydrophilicity to water, various oil-water mixtures can be separated through gravity, the separation efficiency is still 95.0% or above after 50 times of friction, acid-base environment soaking and oil-water separation circulation, and it is indicated that the prepared stainless steel net film has good super-hydrophilicity, friction resistance, acid-base resistance and durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil-water separation, and in particular to a method for preparing a superwetting membrane based on stainless steel mesh modification. Background Art

[0002] With the rapid development of social economy, oil spill accidents occur frequently and a large amount of industrial wastewater is discharged, causing serious water pollution. On the one hand, oily wastewater not only seriously affects the ecological environment, but also endangers human health. On the other hand, water resources are closely related to human daily life and industrial development. Water shortage restricts social development, and oily wastewater also causes waste of water resources. Therefore, the treatment of oily wastewater is urgent. The oil in wastewater usually exists in four forms: floating oil, dispersed oil, emulsion and dissolved oil. Traditional methods for separating oily wastewater include centrifugation, coagulation, flotation, biological method, etc. These methods have the disadvantages of large footprint, secondary pollution, and high energy consumption.

[0003] Membrane separation technology is one of the most promising separation technologies. It has the advantages of high efficiency, energy saving, and no secondary pollution, and is widely used in various fields. Industrial oil-water separation membranes have high requirements for separation performance, membrane flux and stability. However, most oil-water separation membranes currently face problems such as complicated preparation process, harsh conditions, poor chemical stability, poor long-term operation stability, low flux and membrane pollution.

[0004] Chinese patent application number CN202410353172.0, the invention name is "A method for preparing a PS / PMMA bionic super-hydrophobic membrane for oil-water separation", the invention discloses a method for preparing a PS / PMMA bionic super-hydrophobic membrane for oil-water separation, the specific steps of preparing the PS / PMMA bionic super-hydrophobic membrane are as follows: using PI membrane as a substrate material, imprinting a bionic porous membrane on the PI membrane to form a bionic PI / PANI composite membrane, and attaching PMMA-b-PDMS-b-PS super-hydrophobic compound on the surface of the bionic PI / PANI composite membrane to obtain a PS / PMMA bionic super-hydrophobic membrane for oil-water separation, and using a poor solvent for phase separation to make the molecular chains of PS and PMMA curled to form random coils, and finally forming a rough structure of small coils adhering to large coils, the bionic structure gives the PS / PMMA membrane excellent hydrophobic properties, the invention uses PI membrane as a substrate material, can strengthen the mechanical strength of the membrane material while combining with the bionic porous membrane to improve the oil-water separation efficiency. However, the invention has complicated processes and is not suitable for large-scale production.

[0005] Chinese patent application number CN202111285960.3, the invention name is "A method for preparing a super-hydrophilic / underwater super-oleophobic separation membrane", which discloses a method for preparing a super-hydrophilic / underwater super-oleophobic separation membrane. The preparation method is to first deposit a layer of rough titanium dioxide on the base film, then use a surfactant to introduce reactive functional groups on its surface, and finally use a solution polymerization method to graft a hydrophilic polymer on the surface of the base film to obtain a super-hydrophilic / underwater super-oleophobic separation membrane. The super-hydrophilic / underwater super-oleophobic separation membrane of the invention has the properties of super-hydrophilicity in the air and super-oleophobicity underwater. After being wetted by water, oil can be trapped on it, and water quickly passes through the mesh, with large flux and high efficiency. However, it is difficult for the titanium dioxide and the substrate of the invention to be truly bonded together through chemical bonding, and the bonding force is weak. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a superwetting membrane based on modified stainless steel mesh.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A method for preparing a superwetting membrane based on stainless steel mesh modification, wherein the stainless steel mesh is used as a base membrane, dopamine hydrochloride is used as a crosslinking agent, and polyethylene glycol is used as a modifier; the stainless steel mesh is ultrasonically cleaned with clean water, ethanol, and deionized water in sequence; dopamine hydrochloride is added to 40-60 ml of a Tris-Hcl solution with a pH of 8-9, and the concentration of dopamine hydrochloride after addition is 0.5-2 mg / ml; then the cleaned stainless steel mesh is placed in the solution and immersed in the dark at room temperature for 18-24 hours, and then taken out and used The excess dopamine hydrochloride on the surface was washed off with deionized water, and then dried in an oven at 50-70°C for 0.5-1.5 hours to obtain a polydopamine stainless steel mesh; 4-6 mg / ml polyethylene glycol was dissolved in 40-60 ml deionized water and stirred evenly, and then the polydopamine stainless steel mesh obtained in step 2) was immersed in the polyethylene glycol solution for 0.5-1.5 hours, taken out and washed off the excess polyethylene glycol on the surface, and then placed in an oven at 50-70°C for reaction for 1-2 hours to finally obtain a superwet stainless steel mesh membrane.

[0008] The specific steps include: (1) Ultrasonic clean the stainless steel mesh with clean water, ethanol, and deionized water in sequence.

[0009] (2) Add dopamine hydrochloride to 40-60 ml of Tris-HCl solution with a pH of 8-9. The concentration of dopamine hydrochloride is 0.5-2 mg / ml. Then, place the cleaned stainless steel mesh in the solution and immerse it in the dark at room temperature for 18-24 hours. Then, take it out and wash off the excess dopamine hydrochloride on the surface with deionized water. Then, dry it in an oven at 50-70°C for 0.5-1.5 hours to obtain a polydopamine stainless steel mesh.

[0010] (3) Dissolve 4-6 mg / ml polyethylene glycol in 40-60 ml deionized water and stir evenly. Then, immerse the polydopamine stainless steel mesh obtained in step 2) in the polyethylene glycol solution for 0.5-1.5 h, remove it and wash off the excess polyethylene glycol on the surface, then place it in an oven at 50-70 ° C for 1-2 h to obtain a super-wet stainless steel mesh membrane.

[0011] Wherein: the pH of the Tris-HCl solution in step (2) is 8-9. When an appropriate amount of alkaline solution is added to the dopamine hydrochloride solution, self-polymerization can occur, and the speed of self-polymerization is greatly affected by pH. Under acidic conditions, dopamine molecules are in an acidic form and are easy to self-polymerize to form macromolecules; while under alkaline conditions, the hydroxyl bonds and amino bonds of dopamine can react with other electrophilic functional groups, so they are easy to polymerize, and the amino groups can also increase the interaction between the polymer and the metal ions to form a more stable complex.

[0012] In step (2), the concentration of dopamine hydrochloride is 0.5-2 mg / ml, and the immersion time is 18-24 h. The thickness of the polydopamine film formed can be determined by the length of the reaction time and the concentration of dopamine hydrochloride. If the concentration of dopamine hydrochloride is low or the immersion time is short, dopamine hydrochloride cannot be uniformly polymerized on the surface of the stainless steel mesh, resulting in uneven pore sizes of the membrane; if the concentration of dopamine hydrochloride is high or the immersion time is long, the thickness of the membrane will increase, the pore size of the membrane will become smaller, and the water flux of the membrane will be reduced.

[0013] In step (2), the drying temperature of the polydopamine stainless steel mesh is 50-70°C and the drying time is 0.5-1.5h. The temperature of dopamine polymerization will also affect its polymerization degree and polymer quality. Higher temperature can accelerate the polymerization rate of dopamine, but too high temperature will also cause over-polymerization, causing the polymer to lose its properties. When the temperature is too high, the structure of the polymer will be unstable, and the polymer will be easily peeled off and detached.

[0014] In step (3), the concentration of polyethylene glycol is 4-6 mg / ml, and the time is 0.5-1.5 h. The concentration of polyethylene glycol is an important factor affecting the grafting reaction. The higher the concentration, the higher the grafting reaction rate on the membrane surface. In a short period of time, more polyethylene glycol containing hydrophilic functional groups such as hydroxyl groups and amino groups is grafted to the modified membrane surface, which increases the hydrophilicity of the membrane surface and thus reduces the contact angle of the membrane surface. When the concentration of polyethylene glycol is too high, its concentration is no longer the main factor affecting the grafting reaction rate on the membrane surface, so the contact angle change is no longer obvious.

[0015] The reaction temperature of the stainless steel mesh after polyethylene glycol impregnation in step (3) is 50-70°C for 1-2 hours. As the reaction temperature increases, the polyethylene glycol functional groups are activated, which is conducive to the grafting reaction with dopamine. More polyethylene glycol is grafted to the surface of the dopamine modified membrane, which improves the hydrophilicity and reduces the contact angle. When the temperature is too high, the contact angle increases again and the hydrophilicity decreases.

[0016] Compared with the prior art, the present invention has the following beneficial effects: The superwetting membrane preparation method based on stainless steel mesh modification prepared by the present invention is simple and has low energy consumption and high economic feasibility; it has the characteristics of high hydrophilicity, long-term operation, good friction resistance, etc., and can ensure that the superwetting membrane has high separation efficiency and flow rate in treating oily wastewater. DETAILED DESCRIPTION

[0017] The present invention is further described in detail below with reference to specific embodiments. Unless otherwise specified in the embodiments, the raw materials used are common commercially available products. Example 1

[0018] (1) Ultrasonic clean the stainless steel mesh with clean water, ethanol, and deionized water in sequence.

[0019] (2) Add dopamine hydrochloride to 40 ml of Tris-HCl solution with a pH of 8. The concentration of dopamine hydrochloride is 0.5 mg / ml. Then, place the cleaned stainless steel mesh in the solution and immerse it in the dark at room temperature for 18 h. Then, take it out and wash off the excess dopamine hydrochloride on the surface with deionized water. Then, dry it in an oven at 50°C for 0.5 h to obtain a polydopamine stainless steel mesh.

[0020] (3) Dissolve 4 mg / ml polyethylene glycol in 40 ml of deionized water and stir evenly. Then, immerse the polydopamine stainless steel mesh obtained in step 2) in the polyethylene glycol solution for 0.5 h, take it out and wash off the excess polyethylene glycol on the surface, then put it in an oven at 50°C for 1 h to react, and finally obtain a super-wet stainless steel mesh membrane. Example 2

[0021] (1) Ultrasonic clean the stainless steel mesh with clean water, ethanol, and deionized water in sequence.

[0022] (2) Add dopamine hydrochloride to 50 ml of Tris-HCl solution with a pH of 8.5, so that the concentration of dopamine hydrochloride is 1 mg / ml. Then, place the cleaned stainless steel mesh in the solution and immerse it in the dark at room temperature for 20 h. Then, take it out and wash off the excess dopamine hydrochloride on the surface with deionized water. Then, dry it in an oven at 60°C for 1 h to obtain a polydopamine stainless steel mesh.

[0023] (3) Dissolve 5 mg / ml polyethylene glycol in 50 ml of deionized water and stir evenly. Then, immerse the polydopamine stainless steel mesh obtained in step 2) in the polyethylene glycol solution for 1 hour, take it out and wash off the excess polyethylene glycol on the surface, then place it in an oven at 60°C for 1.5 hours to react, and finally obtain a super-wet stainless steel mesh membrane. Example 3

[0024] (1) Ultrasonic clean the stainless steel mesh with clean water, ethanol, and deionized water in sequence.

[0025] (2) Add dopamine hydrochloride to 60 ml of Tris-HCl solution with a pH of 9 to obtain a dopamine hydrochloride concentration of 2 mg / ml. Then, place the cleaned stainless steel mesh in the solution and immerse it in the dark at room temperature for 24 h. Then, take it out and wash off the excess dopamine hydrochloride on the surface with deionized water. Then, dry it in an oven at 70°C for 1.5 h to obtain a polydopamine stainless steel mesh.

[0026] (3) Dissolve 6 mg / ml polyethylene glycol in 60 ml of deionized water and stir evenly. Then, immerse the polydopamine stainless steel mesh obtained in step 2) in the polyethylene glycol solution for 1.5 h, take it out and wash off the excess polyethylene glycol on the surface, then place it in an oven at 70°C for 2 h to react, and finally obtain a super-wet stainless steel mesh membrane. Example 4

[0027] (1) Ultrasonic clean the stainless steel mesh with clean water, ethanol, and deionized water in sequence.

[0028] (2) Add dopamine hydrochloride to 40 ml of Tris-HCl solution with a pH of 8 to obtain a dopamine hydrochloride concentration of 1 mg / ml. Then, place the cleaned stainless steel mesh in the solution and immerse it in the dark at room temperature for 22 h. Then, take it out and wash off the excess dopamine hydrochloride on the surface with deionized water. Then, dry it in an oven at 60°C for 1 h to obtain a polydopamine stainless steel mesh.

[0029] (3) Dissolve 5 mg / ml polyethylene glycol in 50 ml of deionized water and stir evenly. Then, immerse the polydopamine stainless steel mesh obtained in step 2) in the polyethylene glycol solution for 1 hour, take it out and wash off the excess polyethylene glycol on the surface, then place it in an oven at 70°C for 1 hour to react, and finally obtain a super-wet stainless steel mesh membrane. Example 5

[0030] (1) Ultrasonic clean the stainless steel mesh with clean water, ethanol, and deionized water in sequence.

[0031] (2) Add dopamine hydrochloride to 50 ml of Tris-HCl solution with a pH of 8.5, so that the concentration of dopamine hydrochloride is 2 mg / ml. Then, place the cleaned stainless steel mesh in the solution and immerse it in the dark at room temperature for 20 h. Then, take it out and wash off the excess dopamine hydrochloride on the surface with deionized water. Then, dry it in an oven at 70°C for 1.5 h to obtain a polydopamine stainless steel mesh.

[0032] (3) Dissolve 4 mg / ml polyethylene glycol in 60 ml of deionized water and stir evenly. Then, immerse the polydopamine stainless steel mesh obtained in step 2) in the polyethylene glycol solution for 1 hour, take it out and wash off the excess polyethylene glycol on the surface, then put it in an oven at 60°C for 1 hour to react, and finally obtain a super-wet stainless steel mesh membrane. Example 6

[0033] (1) Ultrasonic clean the stainless steel mesh with clean water, ethanol, and deionized water in sequence.

[0034] (2) Add dopamine hydrochloride to 40 ml of Tris-HCl solution with a pH of 9 to obtain a dopamine hydrochloride concentration of 2 mg / ml. Then, place the cleaned stainless steel mesh in the solution and immerse it in the dark at room temperature for 22 h. Then, take it out and wash off the excess dopamine hydrochloride on the surface with deionized water. Then, dry it in an oven at 60°C for 1 h to obtain a polydopamine stainless steel mesh.

[0035] (3) Dissolve 5 mg / ml polyethylene glycol in 60 ml of deionized water and stir evenly. Then, immerse the polydopamine stainless steel mesh obtained in step 2) in the polyethylene glycol solution for 1 hour, take it out and wash off the excess polyethylene glycol on the surface, then put it in an oven at 70°C for 1.5 hours to finally obtain a super-wet stainless steel mesh membrane.

[0036] The rejection rate and water flux of the superwet membranes prepared in Examples 1 to 6 for oily wastewater were measured respectively, and the data are shown in Table 1.

[0037] Table 1 Rejection rate and water flux of stainless steel mesh modified superwet membrane for oily wastewater Product Performance Retention rate (%) <![CDATA[Water flux (L / m 2 ·h)]]> Example 1 95.53 3202.83 Example 2 95.98 3389.34 Example 3 96.48 3191.70 Example 4 96.02 3288.79 Example 5 97.53 3085.87 Example 6 96.52 3194.62 It can be seen from Table 1 above that the present invention is about a method for preparing a superwetting membrane based on stainless steel mesh modification. The superwetting membrane has high rejection rate and water flux, can effectively treat oily wastewater, and the preparation method is simple. The superwetting membrane has good superhydrophilicity and durability.

[0038] Finally, it should be noted that the above embodiments of the present invention are only examples for illustrating the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes and modifications can be made based on the above description. It is impossible to list all implementation methods here. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.

Claims

1. A method for preparing a superwetting membrane based on modified stainless steel mesh, characterized in that: The method is as follows, comprising the following steps: (1) Cleaning the stainless steel mesh: ultrasonically clean the stainless steel mesh with clean water, ethanol, and deionized water in sequence; (2) Preparation of polydopamine stainless steel mesh: dissolve dopamine hydrochloride in 40-60 ml of Tris-HCl solution with a pH of 8-9, and the concentration of dopamine hydrochloride after addition is 0.5-2 mg / ml. Then, immerse the stainless steel mesh cleaned in step (1) in the solution for 18-24 h. Finally, dry the obtained polydopamine stainless steel mesh in an oven at 50-70 °C for 0.5-1.5 h. (3) Preparation of superwet stainless steel mesh: Add polyethylene glycol to 40-60 ml of deionized water, then immerse the polydopamine stainless steel mesh obtained in step (2) in the polyethylene glycol solution, take out, wash and dry to obtain a superwet stainless steel mesh, wherein the polyethylene glycol concentration is 4-6 mg / ml, the immersion time is 0.5-1.5 h, the drying temperature is 50-70 °C, and the drying time is 1-2 h.