Sorting process of mud-containing high-power semi-oxide collophanite

By combining pre-desliming and two-stage grinding with cyclone classification and shaking table separation, the problems of poor grinding and beneficiation effect and high reagent cost of sludge-containing high-particulate phosphate rock were solved, achieving efficient and low-cost beneficiation and wastewater reuse, and meeting the quality requirements of wet phosphoric acid process.

CN118950240APending Publication Date: 2024-11-15GUIZHOU CHANHEN CHEM CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411302106.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing technologies for processing phosphate rock containing high levels of mud and semi-oxides suffer from problems such as poor grinding and flotation effects, high reagent costs, and difficulty in wastewater reuse. They are unable to effectively reduce the impact of impurities on the concentrate, and the beneficiation process is complex.

Method used

The process employs pre-desliming, two-stage grinding combined with cyclone classification and shaking table separation. Through water washing and desliming and cyclone classification, the ore is precisely separated. Combined with reverse flotation for magnesium removal, special dispersants and collectors are used to achieve efficient separation.

Benefits of technology

It effectively reduces the content of sesquioxides and MgO in collophane, meets the requirements of subsequent wet phosphoric acid processing, improves beneficiation efficiency, reduces beneficiation costs, simplifies the process, and facilitates wastewater reuse.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950240A_ABST
    Figure CN118950240A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of mineral separation, and particularly relates to a separation process of mud-containing high-magnification semi-oxide collophanite, which comprises the following steps: carrying out coarse crushing and washing desliming on mud-containing high-magnification semi-oxide collophanite raw ore to respectively obtain deslimed mineral aggregate and mud; the deslimed mineral aggregate is subjected to first-stage ore grinding and rotational flow classification, and coarse-fraction mineral aggregate, middle-fraction mineral aggregate and fine-fraction mineral aggregate are obtained; carrying out second-stage ore grinding and rotational flow classification on the coarse-grained mineral aggregate, and respectively returning a coarse material and a fine material obtained by rotational flow classification to the second-stage ore grinding and the first-stage ore grinding; the middle fraction mineral aggregate is subjected to table separation, and low sesquioxide phosphate concentrate and table tailings are obtained respectively; and the fine-fraction mineral aggregate, the mud and the table tailings are subjected to reverse flotation magnesium removal, products in a flotation machine groove are high-power semi-oxide phosphate concentrate, and flotation froth is magnesium-removed tailings. The separation process provided by the invention has the characteristics that the adaptability is high, the separation cost is low, the process flow is simple, beneficiation wastewater is easy to reuse, and the production flow is easy to control and adjust.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of ore dressing, and in particular relates to a separation process of mud-containing high-sesquioxide collophanite. Background Art

[0002] Human activities are highly dependent on phosphorus. Phosphorus usually exists in nature in the form of orthophosphate, and the phosphorus chemical industry mainly uses apatite, phosphorite and collophanite. With the rapid development of the phosphorus chemical industry, it has gradually upgraded from a traditional extensive phosphorus chemical industry to an industrial cluster of green, efficient and sustainable development of phosphorus resources. With the high degree of integration of industries related to new energy materials such as "phosphorus, fluorine and lithium" and "sulfur, phosphorus and titanium", the demand for phosphorus resources is increasing, and the beneficiation technology of low-grade and difficult-to-select phosphate ore has also become a focus of attention.

[0004] Among the phosphate deposits with large reserves, some are calcium-magnesium carbonate phosphate ores. The use of fatty acid reverse flotation collectors for this part of phosphate ores has good application value and is currently widely used in phosphorus chemical enterprises. Since this type of phosphate ore is rich in quartz, feldspar, clayey substances and organic matter, the gangue minerals containing sesquioxides are adjacent to the collophanites with extremely fine embedded particles, and the gangue intergrowth is extremely difficult to dissociate, resulting in high grinding and flotation reagent costs, poor flotation effects, and low phosphorus recovery rates; in particular, the pH difference of the wastewater generated by direct-reverse flotation is extremely large, and the difficulty in reusing the beneficiation wastewater is the reason for restricting the large-scale application of mud-containing high-sesquioxide collophanites.

[0005] Under the current situation, the beneficiation of mud-containing high-sesquioxide collophanite becomes particularly important. A large number of ore layers in this part of collophanite belong to mud-containing high-sesquioxide phosphate ore. At present, a few phosphate mining companies treat high-alumina siliceous collophanite by positive flotation. Under alkaline conditions, water glass, sodium hexametaphosphate, sodium fluorosilicate, etc. are used as gangue inhibitors, and fatty acid collectors are added to float the phosphate ore; the separation cost is high and the process is complicated. Summary of the invention

[0006] In view of this, the purpose of the present invention is to provide a sorting process for high-sesquioxide collophanite containing mud, which can not only effectively reduce the contents of sesquioxide and MgO in the collophanite, but also fundamentally reduce the influence of impurities on the concentrate, meet the dosage and quality requirements of the subsequent wet phosphoric acid process, and fully realize the efficient and comprehensive utilization of difficult-to-select phosphate ore resources; the sorting process has the characteristics of strong adaptability, low sorting cost, simple process flow, easy reuse of mineral processing wastewater, and easy control and adjustment of the production process.

[0007] The present invention provides a separation process of high-sesquioxide collophanite containing mud, comprising the following steps:

[0008] The raw collophanite containing mud and high sesquioxide is coarsely crushed to obtain coarsely crushed ore;

[0009] The coarsely crushed ore is washed and deslimed to obtain deslimed ore and mud respectively;

[0010] The deslimed ore is subjected to a first-stage grinding to obtain a first-stage grinding product;

[0011] The first-stage grinding product is subjected to cyclone classification according to particle size, wherein the particle size > 0.1 mm is classified as coarse-grained ore, the particle size of 0.045-0.1 mm is classified as medium-grained ore, and the particle size < 0.045 mm is classified as fine-grained ore;

[0012] The coarse-grained ore is subjected to two-stage grinding, and the products of the second-stage grinding are subjected to cyclone classification according to particle size, and the ore with a particle size of >0.125 mm obtained by cyclone classification is returned to the second-stage grinding, and the ore with a particle size of ≤0.125 mm obtained by cyclone classification is returned to the first-stage grinding;

[0013] The intermediate-sized ore is subjected to shaking table separation to obtain low-sesquioxide phosphate concentrate and shaking table tailings respectively;

[0014] The fine-grained ore, mud and shaking table tailings are subjected to reverse flotation to remove magnesium, the product in the flotation machine tank is high-sesquioxide phosphate concentrate, and the flotation foam is the magnesium-removed tailings;

[0015] In the reverse flotation demagnesization process, the dispersant added to the slurry includes one or more of polymerized polyols, sodium pyrophosphate and triethylhexyl phosphate, and the mass ratio of dry basis ore volume, liquid in the slurry and dispersant is 1000:(1500-2500):(0.02-0.1).

[0016] Preferably, the P2O5 content of the mud-containing high-sesquioxide collophanite ore is 20-25wt%, the MgO content is 2.5-5wt%, and the sesquioxide content is 3-7wt%.

[0017] Preferably, the particle size of the coarsely crushed ore is 15 to 25 mm.

[0018] Preferably, the coarsely crushed ore is washed and desludified in a vibrating screen; the particle size of the mud is less than 0.038 mm, and the solid content of the mud is 15-35%.

[0019] Preferably, the equipment for the first stage grinding is a rod mill; the mass ratio of the ore to water when the rod mill is in operation is 1:(0.25-0.65).

[0020] Preferably, the cyclone classification of the first-stage grinding product is carried out in a cyclone group; the working pressure of the cyclone group is 45-100 kPa.

[0021] Preferably, the second-stage grinding is carried out in a ball mill; the cyclone classification of the second-stage grinding product is carried out in a hydrocyclone; and the working pressure of the hydrocyclone is 80-110 kPa.

[0022] Preferably, the intermediate-sized ore is mixed with water before being sorted on a shaking table, and the mass ratio of the ore to water is 1:(1.5-3); the equipment for the shaking table sorting is a fine sand shaking table, the bed inclination angle is 0.5-2°, the shaking table stroke is 11-18 mm, and the stroke frequency is 280-320 times / min.

[0023] Preferably, in the reverse flotation demagnesizing process, the flotation regulator added to the slurry includes sulfuric acid and / or phosphoric acid, and the demagnesizing collector added to the slurry is oxidized paraffin soap.

[0024] Preferably, the P2O5 content of the low-sesquioxide phosphate concentrate is ≥30wt%, the MgO content is ≤1wt%, and the sesquioxide content is ≤2wt%; the P2O5 content of the high-sesquioxide phosphate concentrate is ≥28wt%, the MgO content is ≤1.2wt%, and the sesquioxide content is 4-5wt%; the P2O5 content of the demagnesized tailings is ≤7wt%.

[0025] Compared with the prior art, the present invention provides a separation process of high-half-oxide collophanite containing mud, comprising the following steps: coarsely crushing the raw ore of high-half-oxide collophanite containing mud to obtain coarsely crushed ore; washing the coarsely crushed ore to remove mud, respectively obtaining deslimed ore and mud; subjecting the deslimed ore to one-stage grinding to obtain a first-stage grinding product; subjecting the first-stage grinding product to cyclone classification according to particle size, wherein particles with a particle size greater than 0.1 mm are classified as coarse-grained ore, particles with a particle size of 0.045 to 0.1 mm are classified as intermediate-grained ore, and particles with a particle size less than 0.045 mm are classified as fine-grained ore; subjecting the coarse-grained ore to two-stage grinding, subjecting the second-stage grinding product to cyclone classification according to particle size, and the particles obtained by the cyclone classification are further classified into the following steps: The ore with a particle size of more than 0.125 mm is returned to the second-stage grinding, and the ore with a particle size of ≤0.125 mm obtained by cyclone classification is returned to the first-stage grinding; the intermediate-sized ore is subjected to shaking table sorting to obtain low-sesquioxide phosphate concentrate and shaking table tailings respectively; the fine-sized ore, mud and shaking table tailings are subjected to reverse flotation de-magnesiumization, the product in the flotation machine tank is high-sesquioxide phosphate concentrate, and the flotation foam is de-magnesiumized tailings; in the process of reverse flotation de-magnesiumization, the dispersant added to the slurry includes one or more of polymerized polyols, sodium pyrophosphate and triethylhexyl phosphate, and the mass ratio of dry basis ore content, liquid in the slurry and dispersant is 1000:(1500-2500):(0.02-0.1). The separation process provided by the present invention can not only effectively reduce the content of sesquioxide and MgO in collophanite, but also fundamentally reduce the influence of impurities on the concentrate, meet the subsequent wet phosphoric acid process dosage and quality requirements, and fully realize the efficient and comprehensive utilization of difficult-to-select phosphate resources; the separation process has the characteristics of strong adaptability, low separation cost, simple process flow, easy reuse of mineral processing wastewater, and easy control and adjustment of the production process. More specifically, the present invention has the following advantages:

[0026] (1) For high-sesquioxide collophosphate containing mud, the first thing to solve is the influence of mud on the grinding product. Whether it is primary or secondary mud, the physical and chemical properties of the mineral surface will be affected after the ore surface is wrapped, which is one of the fundamental reasons for poor separation effect, large dosage of reagents and low recovery rate. The present invention first solves the problem of ore mudification. By washing and desludging the ore before classification, the sorting of the ore is significantly improved.

[0027] (2) Two-stage grinding is used for combined separation, and a cyclone is used to accurately and timely classify the raw ore. According to the "particle size segregation" phenomenon in the ore, the high- and low-sesquioxide collophosphates are separated in time, which minimizes the occurrence of over-grinding and ensures that the target mineral and the gangue ore reach a suitable dissociation particle size. In addition, the two-stage grinding has a large processing capacity and can adjust the process parameters in time according to the fluctuation of the ore properties, so as to obtain the best mineral processing indicators.

[0028] (3) Currently, both the forward-reverse and reverse-forward flotation processes cannot avoid the two-level differentiation of pH value. The cost of flotation reagents is high, and a large amount of pH adjuster residue enters the flotation water body, making it difficult to recycle the flotation water. Therefore, the present invention adopts a combined mineral processing process of water washing desludging-cyclone classification-gravity / flotation, and only adopts a reverse flotation demagnesization process to obtain a qualified phosphate concentrate product; on the one hand, the gravity separation process is simple, the process conditions are easy to control, and the dehydration and drying process of the gravity separation product is simple; on the other hand, the cost of a single reverse flotation reagent is low, and the difficulty of reusing flotation wastewater is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0030] Figure 1 It is a sorting process flow chart provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The present invention provides a separation process of high-sesquioxide collophanite containing mud, comprising the following steps:

[0033] The raw collophanite containing mud and high sesquioxide is coarsely crushed to obtain coarsely crushed ore;

[0034] The coarsely crushed ore is washed and deslimed to obtain deslimed ore and mud respectively;

[0035] The deslimed ore is subjected to a first-stage grinding to obtain a first-stage grinding product;

[0036] The first-stage grinding product is subjected to cyclone classification according to particle size, wherein the particle size > 0.1 mm is classified as coarse-grained ore, the particle size of 0.045-0.1 mm is classified as medium-grained ore, and the particle size < 0.045 mm is classified as fine-grained ore;

[0037] The coarse-grained ore is subjected to two-stage grinding, and the products of the second-stage grinding are subjected to cyclone classification according to particle size, and the ore with a particle size of >0.125 mm obtained by cyclone classification is returned to the second-stage grinding, and the ore with a particle size of ≤0.125 mm obtained by cyclone classification is returned to the first-stage grinding;

[0038] The intermediate-sized ore is subjected to shaking table separation to obtain low-sesquioxide phosphate concentrate and shaking table tailings respectively;

[0039] The fine-grained ore, mud and shaking table tailings are subjected to reverse flotation to remove magnesium, the product in the flotation machine tank is high-sesquioxide phosphate concentrate, and the flotation foam is the magnesium-removed tailings.

[0040] In the separation process provided by the present invention, the P2O5 content of the mud-containing high-sesquioxide collophanite ore is preferably 20-25wt%, specifically 20wt%, 20.5wt%, 21wt%, 21.5wt%, 22wt%, 22.5wt%, 23wt%, 23.5wt%, 24wt%, 24.5wt%, 24.7wt% or 25wt%; the MgO content of the mud-containing high-sesquioxide collophanite ore is preferably 2.5-5wt%. t%, specifically 2.5wt%, 3wt%, 3.1wt%, 3.5wt%, 4wt%, 4.3wt%, 4.5wt% or 5wt%, the sesquioxide (R2O3) content of the mud-containing high-sesquioxide collophanite ore is 3-7wt%, specifically 3wt%, 3.5wt%, 4wt%, 4.3wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 6.8wt% or 7wt%.

[0041] In the sorting process provided by the present invention, the specific process of the coarse crushing preferably includes: first using a jaw crusher for primary crushing, then screening, and using a high-pressure roller crusher, a cone crusher or other fine crushing equipment to perform secondary crushing on the screened material, and finally controlling the particle size of the ore after crushing to meet the requirements.

[0042] In the sorting process provided by the present invention, the particle size of the coarsely crushed ore is preferably 15-25 mm, specifically 15 mm, 16 mm, 17 mm, 18 mm, 19 mm, 20 mm, 21 mm, 22 mm, 23 mm, 24 mm or 25 mm.

[0043] In the sorting process provided by the present invention, the coarsely crushed ore is preferably washed and deslimed in a vibrating screen; the frequency of the vibrating screen is preferably 40-70 Hz, specifically 40 Hz, 45 Hz, 50 Hz, 55 Hz, 60 Hz, 65 Hz or 70 Hz; the amplitude of the vibrating screen is preferably 2-6 mm, specifically 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, 4.5 mm, 5 mm, 5.5 mm or 6 mm; the vibration intensity of the vibrating screen is preferably 6-10 g, specifically 6 g, 6.5 g, 7 g, 7.5 g, 8 g, 8.5 g, 9 g, 9.5 g or 10 g.

[0044] In the sorting process provided by the present invention, the particle size of the mud is preferably less than 0.038 mm; the solid content of the mud is preferably 15-35%, specifically 15%, 17%, 20%, 23%, 25%, 27%, 30%, 32% or 35%.

[0045] In the sorting process provided by the present invention, the equipment for the first stage of grinding is preferably a rod mill; the mass ratio of ore to water when the rod mill is running is preferably 1:(0.25-0.65), specifically 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6 or 1:0.65.

[0046] In the separation process provided by the present invention, before the first-stage grinding product is subjected to cyclone classification, a certain amount of water is preferably added. After the water is added, the mass ratio of the ore to water in the slurry is preferably 1:(1.5-3), specifically 1:1.5, 1:1.7, 1:2, 1:2.3, 1:2.5, 1:2.7 or 1:3.

[0047] In the sorting process provided by the present invention, the cyclone classification of the first-stage grinding product is preferably carried out in a cyclone group; the working pressure of the cyclone group is preferably 45-100 kPa, specifically 45 kPa, 50 kPa, 55 kPa, 60 kPa, 65 kPa, 70 kPa, 75 kPa, 80 kPa, 85 kPa, 90 kPa, 95 kPa or 100 kPa.

[0048] In the separation process provided by the present invention, the second-stage grinding is preferably carried out in a ball mill.

[0049] In the sorting process provided by the present invention, the cyclone classification of the second-stage grinding product is preferably carried out in a hydrocyclone; the working pressure of the hydrocyclone is preferably 80-110 kPa, specifically 80 kPa, 85 kPa, 90 kPa, 95 kPa, 100 kPa, 105 kPa or 110 kPa.

[0050] In the sorting process provided by the present invention, the intermediate particle size mineral material is preferably mixed with water before being sorted on a shaking table, and the mass ratio of the mineral material to water is preferably 1:(1.5-3), specifically 1:1.5, 1:1.7, 1:2, 1:2.3, 1:2.5, 1:2.7 or 1:3.

[0051] In the sorting process provided by the present invention, the equipment for the shaking table sorting is preferably a fine sand shaking table; the inclination angle of the shaking table sorting is preferably 0.5-2°, specifically 0.5°, 0.7°, 1°, 1.2°, 1.5°, 1.7° or 2°; the shaking table stroke of the shaking table sorting is preferably 11-18mm, specifically 11mm, 12mm, 13mm, 14mm, 15mm, 16mm, 17mm or 18mm; the stroke frequency of the shaking table sorting is preferably 280-320 times / min, specifically 280 times / min, 285 times / min, 290 times / min, 295 times / min, 300 times / min, 305 times / min, 310 times / min, 315 times / min or 320 times / min.

[0052] In the separation process provided by the present invention, after separation by the shaking table, the obtained products are distributed in a fan-shaped manner on the bed surface, wherein the products in the heavy product area are low-sesquioxide phosphate concentrates, and the light product area is mainly tailings composed of some mud-containing fine particles and calcium-magnesium gangue minerals, which enter the reverse flotation demagnesization operation stage.

[0053] In the separation process provided by the present invention, during the reverse flotation demagnesium process, the dispersant added to the slurry includes one or more of polymerized polyols, sodium pyrophosphate and triethylhexyl phosphate; wherein the polymerized polyol is preferably prepared by reacting raw materials including oxalic acid, triethanolamine (TEA) and glycerol, and the content of oxalic acid in the polymerized polyol raw material is preferably 40-50wt%, specifically 40wt%, 42wt%, 45wt%, 47wt% or 50wt%; the content of triethanolamine in the polymerized polyol raw material is preferably 25-30wt%, specifically 25wt%, 26wt%, 27wt%, 28wt%, 29wt% or 30wt%; the content of glycerol in the polymerized polyol raw material is preferably 20-35wt%, specifically 20wt%, 23wt%, 25wt%, 27wt%, 30wt%, 32wt% t% or 35wt%; the content of the polymeric polyol in the dispersant is preferably 30-40wt%, specifically 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt% or 40wt%; the content of the sodium pyrophosphate in the dispersant is preferably 10-15wt%, specifically 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%; the content of the triethylhexyl phosphate in the dispersant is preferably 45-60wt%, specifically 45wt%, 46wt%, 47wt%, 48wt%, 49wt%, 50wt%, 51wt%, 52wt%, 53wt%, 54wt%, 55wt%, 56wt%, 57wt%, 58wt%, 59wt% or 60wt%.

[0054] In the separation process provided by the present invention, in the process of reverse flotation demagnesiumization, the mass ratio of dry basis ore, liquid in slurry and dispersant is preferably 1000:(1500-2500):(0.02-0.1); wherein, the mass ratio of dry basis ore and liquid in slurry can be specifically 1000:1500, 1000:1600, 1000:1700, 1000:1800, 1000:1900, 1000:2000, 1000:2100, 1000:2200, 1000:2300, 1000:2400, 1000:2500, 1000:2600, 1000:2700, 1000:2800, 1000:2900, 1000:2900, 1000:2100, 1000:2200, 1000:29 ... 00:2300, 1000:2400 or 1000:2500; the mass ratio of dry basis ore to dispersant can be 1000:0.02, 1000:0.025, 1000:0.03, 1000:0.035, 1000:0.036, 1000:0.04, 1000:0.045, 1000:0.05, 1000:0.06, 1000:0.07, 1000:0.08, 1000:0.09 or 1000:0.1.

[0055] In the separation process provided by the present invention, during the reverse flotation demagnesiuming process, the flotation adjusting agent added to the ore pulp preferably includes sulfuric acid and / or phosphoric acid; the sulfuric acid is preferably a concentrated sulfuric acid solution, and its concentration is preferably 95-98wt%; the phosphoric acid is preferably a phosphoric acid solution, and its concentration is preferably 35-40wt%, more preferably 38wt%; the amount of sulfuric acid added is preferably 3-5kg / t ore, specifically 3kg / t ore, 3.25kg / t ore, 3.5kg / t ore, 4kg / t ore, 4.5kg / t ore or 5kg / t ore; the amount of phosphoric acid added is preferably 1.5-4kg / t ore, specifically 1.5kg / t ore, 2kg / t ore, 2.5kg / t ore, 3kg / t ore, 3.5kg / t ore or 4kg / t ore.

[0056] In the separation process provided by the present invention, in the process of reverse flotation demagnesiuming, the demagnesiuming collector added to the slurry is preferably oxidized paraffin soap; the addition amount of the demagnesiuming collector is preferably 300-800 g / t ore, specifically 300 g / t ore, 350 g / t ore, 400 g / t ore, 450 g / t ore, 500 g / t ore, 550 g / t ore, 600 g / t ore, 650 g / t ore, 700 g / t ore, 750 g / t ore or 800 g / t ore.

[0057] In the separation process provided by the present invention, the reverse flotation demagnesium preferably adopts an open-circuit process of "one roughing and one scavenging", and the mass ratio of the reagent dosage of the roughing and scavenging is preferably (6-9):(4-1), more preferably 7:3, and the middling product and the concentrate product are combined to obtain a mixed concentrate product.

[0058] In the separation process provided by the present invention, the P2O5 content of the low-sesquioxide phosphate concentrate is preferably ≥30wt%, the MgO content is preferably ≤1wt%, and the sesquioxide content is preferably ≤2wt%; the P2O5 content of the high-sesquioxide phosphate concentrate is preferably ≥28wt%, the MgO content is preferably ≤1.2wt%, and the sesquioxide content is preferably 4-5wt%; the P2O5 content of the demagnesized tailings is preferably ≤6wt%.

[0059] The separation process provided by the present invention can not only effectively reduce the content of sesquioxide and MgO in collophanite, but also fundamentally reduce the influence of impurities on the concentrate, meet the subsequent wet phosphoric acid process dosage and quality requirements, and fully realize the efficient and comprehensive utilization of difficult-to-select phosphate ore resources; the separation process has the characteristics of strong adaptability, low separation cost, simple process flow, easy reuse of mineral processing wastewater, and easy control and adjustment of the production process. More specifically, the beneficial effects of the present invention are:

[0060] (1) Pre-de-sludging, two-stage grinding combined with cyclone classification and shaking table separation are used to accurately separate the phosphate ore, reduce the energy consumption of the grinding operation, alleviate the "over-grinding phenomenon", reduce the impact of fine particles on the grinding and classification process, and achieve high beneficiation efficiency.

[0061] (2) Improve the utilization efficiency of mud-containing high-sesquioxide phosphate ore, effectively reduce the dolomite impurities and sesquioxide content in collophanite, and separate the high-sesquioxide raw ore into low-magnesium-low-sesquiphosphate concentrate and low-magnesium-high-sesquiphosphate concentrate through the grinding, grading, gravity-flotation combined separation process, so as to reasonably and efficiently utilize this part of the difficult-to-separate phosphate resources.

[0062] (3) The main impurities are introduced into the fine-grained product through precise grinding and classification technology, and reverse flotation and magnesium removal are carried out by adding special dispersants; the special dispersants have stable chemical properties, low dosage and low cost, and are highly targeted. They have a good polymerization-dispersion effect on this part of fine ore mud, effectively improving the selectivity of reverse flotation agents and improving sorting efficiency.

[0063] (4) The present invention has strong adaptability to different properties of collophanites. The water-washing-sludge-cyclone classification-gravity / flotation combined beneficiation process can obtain qualified phosphate concentrate products by only using the reverse flotation demagnesium process; on the one hand, the gravity separation process is simple, the process conditions are easy to control, and the gravity separation product dehydration and drying process is simple; on the other hand, the cost of a single reverse flotation agent is low, the pH change of flotation wastewater is small, and the degree of production water reuse is high; at the same time, it provides convenience for subsequent phosphorus chemical production processes. The combined separation process has the characteristics of low separation cost, simple process flow, easy reuse of beneficiation wastewater, and easy control and adjustment of the production process.

[0064] For the purpose of greater clarity, the present invention is described in detail with reference to the following examples and comparative examples.

[0065] Example 1

[0066] A separation process of high-semioxide collophanite containing mud, the process flow is as follows Figure 1 As shown, the details are as follows:

[0067] (1) Pre-demuding stage:

[0068] The raw colloidal phosphate ore (P2O5: 23.47wt%, MgO: 4.26wt%, R2O3: 4.31wt%) from Guizhou Province was crushed in two stages of closed circuit using a jaw crusher and a high-pressure roller crusher to obtain particles with a particle size of 15 to 25mm; the crushed material was pre-washed and desludged on a multi-stage high-frequency vibrating screen with a frequency of 55Hz, an amplitude of 4.0mm, and a vibration intensity of 8.0g to obtain desludged raw ore and desludged sieve mud (particle size <0.038mm, solid content of 25.0%), and the desludged sieve mud entered a fine-grained dense collection tank.

[0069] (2) Two-stage, one-closed-circuit, combined classification stage:

[0070] The desludging ore obtained in the pre-sludging stage is subjected to a first-stage grinding by a rod mill, and water is added to the water added before the rod mill according to the ratio of ore: water = 1:0.5 (mass ratio); the discharge product of the rod mill is supplemented with water according to the ratio of ore: water = 1:2 (mass ratio), and then enters the combined cyclone for classification operation, and the working pressure of the combined cyclone is 65Kpa; the sand settling product of the combined cyclone is a coarse-grained ore (>0.1mm), which enters the second-stage ball milling operation, and the discharge product of the ball mill is classified by a hydrocyclone, and the working pressure of the hydrocyclone is 90Kpa, wherein the ore with a bottom flow of the cyclone>0.125mm is returned to the feeding end of the second-stage ball mill, and the ore with a top flow of the cyclone≤0.125mm is returned to the feeding section of the first-stage grinding rod mill to re-enter the grinding system; the fine-grained ore (<0.045mm) obtained by the combined cyclone and the desludging screened mud obtained in the pre-sludging stage are entered into the fine-grained dense collection tank together.

[0071] (3) Gravity-floatation combined separation process:

[0072] The intermediate-sized ore (particle size range 0.045-0.1mm) obtained by combined hydrocyclone classification was added with water according to the ratio of ore: water = 1:2.5 (mass ratio) and then sorted on a shaking table. The sorting equipment was a fine sand shaking table with a bed surface inclination of 1.50°, a shaking table stroke of 15.0mm, and a stroke frequency of 290 times / min. The products obtained after the shaking table sorting were distributed in a fan-shaped manner on the bed surface. The products in the heavy product area were dehydrated by a plate and frame filter press, and the water content was controlled to be less than 10%. The product concentrate 1 was a low-sesquioxide phosphate concentrate product. The light product area was mainly composed of tailings composed of some mud-containing fine particles and calcium-magnesium gangue minerals. This part entered the reverse flotation demagnesium operation stage.

[0073] The tailings of the shaking table sorting, the fine-grained ore (<0.045mm) obtained by the combined cyclone, and the desludging screen mud (<0.038mm) obtained in the pre-sludging stage together constitute the reverse flotation demagnesized ore pulp, and the reverse flotation demagnesized operation is performed by adding a special dispersant, a flotation adjuster and a demagnesized collector; wherein the amount of the above-mentioned special dispersant is based on the dry basis ore volume: liquid in the slurry: special dispersant = 1000:1800:0.025 (mass ratio), and the composition of the special dispersant is 35wt% of polymer polyol, 15wt% of sodium pyrophosphate, and 50wt% of triethylhexyl phosphate, and the polymer polyol is prepared by a mixed reaction of oxalic acid, triethanolamine and glycerol The dosage of oxalic acid is 40wt%, the dosage of triethanolamine is 30wt%, and the dosage of glycerol is 30wt%; the flotation adjusters for reverse flotation demagnesiumization operation include concentrated sulfuric acid (H2SO4: 98wt%) and phosphoric acid solution (H3PO4: 38wt%), the dosage of concentrated sulfuric acid is 4.50kg / t ore, and the dosage of phosphoric acid solution is 3.0kg / t ore; the demagnesiumization collector for reverse flotation demagnesiumization operation is an oxidized paraffin soap collector, and the dosage is 650g / t ore; the reverse flotation demagnesiumization operation adopts an open-circuit process of "one roughing and one sweeping", and the dosage ratio of each reagent is roughing: sweeping = 7:3 (mass ratio), and the middling product and the concentrate product are combined to obtain a mixed concentrate product. The obtained flotation machine tank product and the middling product are dehydrated by a plate and frame filter press to control the moisture content to less than 13% to obtain a high-half-oxide phosphate concentrate product (concentrate 2). The flotation foam product is dehydrated by a plate and frame filter press to control the moisture content to less than 15% to obtain magnesium-free tailings.

[0074] Comparative Example 1-1

[0075] The implementation scheme of Example 1 is followed, except that no dispersant is added during the flotation operation.

[0076] Comparative Example 1-2

[0077] According to the implementation scheme of Example 1, the difference is that the dispersant added in the flotation operation stage is water glass (SiO2 / Na2O molar ratio = 2.50) and sodium hexametaphosphate (industrial grade) in a mass ratio of 1:1, and the amount of dispersant is based on the dry basis ore amount: liquid in the ore pulp: dispersant = 1000:1200:1.5 (mass ratio).

[0078] The products obtained in Example 1, Comparative Example 1-1 and Comparative Example 1-2 were dried (80-110°C) to remove free moisture, and chemical index analysis was performed using the standard method for phosphate rock analysis. The test results are shown in Table 1 (R2O3 represents the sesquioxide content, which is the total mass fraction of Fe2O3 and Al2O3).

[0079] Table 1 Test results of Example 1, Comparative Example 1-1, and Comparative Example 1-2 (unit: %)

[0080]

[0081] It can be seen from the test analysis results in Table 1 that by adopting the "pretreatment gravity-flotation combined separation process" of the present invention, controlling the process conditions, reagent ratio and dosage range, and obtaining the preferred test results through conditional tests, a high-quality low-sesquioxide phosphorus concentrate 1 can be obtained through a two-stage grinding-combined classification-shaking table separation process. Example 1 The high-sesquioxide collophanite containing mud is separated to obtain high-quality low-sesquioxide collophanite and high-sesquioxide collophanite with qualified MgO content. The total P2O5 recovery rate of high and low-sesquioxide concentrates is 94.09%, and the phosphorus loss is small.

[0082] The experimental analysis results of Comparative Examples 1-1 and 1-2 show that if the special dispersant described in the present invention is not used in the flotation demagnesiumization part of the fine-grained slurry, or if a conventional dispersant for flotation operation is used, it is impossible to obtain a high-sesquioxide phosphate concentrate 2 with a qualified MgO content, and it will also affect the content of sesquioxides in the concentrate 2; it will also lead to an increase in the P2O5 content in the flotation tail, resulting in a decrease in the recovery rate of the phosphate concentrate, affecting the overall economic value.

[0083] The improvement effect of adding conventional dispersant in Comparative Example 1-2 is weak compared with that of not adding dispersant in Comparative Example 1-1, because conventional dispersants can better electrostatically adsorb and selectively chemically adsorb muddy slurries with a wide range of particle sizes. For the fine-grained slurry with a narrow particle size content range composed of pre-de-sliming, combined classification fine-grained slurry and shaking table sorting tailings described in this method, and the slurry is rich in a large number of inevitable ions ionized from fine particles of aluminum silicate and calcium-magnesium gangue, resulting in a complex chemical composition of the slurry solution, it is difficult for conventional dispersants to obtain a good selective adsorption effect, resulting in failure of the dispersion ability.

[0084] Example 2

[0085] According to the implementation scheme of Example 1, the process conditions of the pre-de-sliming stage, the two-stage one-closed circuit, and the combined classification stage remain unchanged. The difference is that the test ore is the Sichuan collophanite ore (P2O5: 24.68wt%, MgO: 3.13wt%, R2O3: 6.84wt%); the conditions of the gravity-flotation combined separation process are: the dosage of the special dispersant is based on the dry basis ore volume: liquid in the ore pulp: special dispersant = 1000:1600:0.036 (mass ratio); the dosage of concentrated sulfuric acid in the reverse flotation de-magnesium operation is 3.25kg / t ore, the dosage of phosphoric acid solution is 2.0kg / t ore, and the dosage of the de-magnesium collector is 500g / t ore.

[0086] Comparative Example 2-1

[0087] According to the implementation scheme of Example 2, the process conditions of the pre-de-sludge stage, the two-stage one closed circuit, and the combined classification stage remain unchanged. The difference is that the amount of special dispersant is based on the dry basis ore volume: liquid in the ore slurry: special dispersant = 1000:1600:0.012 (mass ratio).

[0088] Comparative Example 2-2

[0089] According to the implementation scheme of Example 2, the process conditions of the pre-de-sludge stage, the two-stage one closed circuit, and the combined classification stage remain unchanged. The difference is that the amount of special dispersant is based on the dry basis ore volume: liquid in the ore slurry: special dispersant = 1000:1600:0.2 (mass ratio).

[0090] The products obtained in Example 2, Comparative Example 2-1 and Comparative Example 2-2 were dried (80-110° C.) to remove free moisture, and chemical index analysis was performed using the standard method for phosphate rock analysis. The test results are shown in Table 2.

[0091] Table 2 Test results of Example 2, Comparative Example 2-1, and Comparative Example 2-2 (unit: %)

[0092]

[0093]

[0094] It can be seen from the test analysis results in Table 2 that by adopting the "pretreatment gravity-floatation combined separation process" of the present invention, controlling the process conditions, reagent ratio and dosage range, and obtaining the preferred test results through conditional tests, a high-quality low-sesquioxide phosphorus concentrate 1 can be obtained through a two-stage grinding-combined classification-shaking table separation process. Example 2 The high-sesquioxide collophanite containing mud is separated to obtain high-quality low-sesquioxide collophanite and high-sesquioxide collophanite with qualified MgO content. The total P2O5 recovery rate of high-sesquioxide and low-sesquioxide concentrates is 94.12%, and the phosphorus loss is small.

[0095] The experimental analysis results of Comparative Examples 2-1 and 2-2 show that the special dispersant described in the present invention is used in the flotation demagnesization of fine-grained slurry, but the added amount is outside the preferred range. If the amount is too high or too low, the flotation operation cannot obtain a high-sesquioxide phosphate concentrate 2 with a qualified MgO content, and will also affect the content of sesquioxides in the concentrate 2; it will also lead to an increase in the P2O5 content in the flotation tail, resulting in a decrease in the recovery rate of the phosphate concentrate, affecting the overall economic value.

[0096] The addition amount of comparative example 2-1 is lower than the preferred range described in the present invention, resulting in poor dispersion effect of fine particle flotation pulp. A large number of inevitable ions generated during the crushing and grinding process cause different mineral particles to carry different charged ions on their surfaces, which causes positive and negative charge adsorption and agglomeration during the flotation machine stirring process, affecting the selective adsorption effect of the flotation collector, resulting in poor flotation index. The comparative example 2-2 is higher than the preferred range described in the present invention. The higher addition amount seriously affects the charge composition in the pulp solution, deteriorates the flotation environment, and causes a decrease in the selectivity of the flotation reagent; not only does it have a negative impact on the demagnesiation effect of fine particles, but a large amount of dispersant contains a large amount of organic matter, which will lead to poor pulp fluidity, failure of reagent selectivity, and difficulty in flotation water reuse.

[0097] In summary, it can be seen from the embodiments and comparative examples that the present invention can effectively reduce the impact of primary and secondary fine-particle products in the ore crushing and grinding process on the classification and flotation effects, the present invention has high sorting efficiency, can effectively separate sesquioxide impurities in phosphate ore, has the advantages of simple mineral processing flow, convenient process adjustment, and low mineral processing cost.

[0098] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A separation process for high-sesquioxide collophanite containing mud, characterized in that: The following steps are involved: The raw collophanite containing mud and high sesquioxide is coarsely crushed to obtain coarsely crushed ore; The coarsely crushed ore is washed and deslimed to obtain deslimed ore and mud respectively; The deslimed ore is subjected to a first-stage grinding to obtain a first-stage grinding product; The first-stage grinding product is subjected to cyclone classification according to particle size, wherein the particle size > 0.1 mm is classified as coarse-grained ore, the particle size of 0.045-0.1 mm is classified as medium-grained ore, and the particle size < 0.045 mm is classified as fine-grained ore; The coarse-grained ore is subjected to two-stage grinding, and the products of the second-stage grinding are subjected to cyclone classification according to particle size, and the ore with a particle size of >0.125 mm obtained by cyclone classification is returned to the second-stage grinding, and the ore with a particle size of ≤0.125 mm obtained by cyclone classification is returned to the first-stage grinding; The intermediate-sized ore is subjected to shaking table separation to obtain low-sesquioxide phosphate concentrate and shaking table tailings respectively; The fine-grained ore, mud and shaking table tailings are subjected to reverse flotation to remove magnesium, the product in the flotation machine tank is high-sesquioxide phosphate concentrate, and the flotation foam is the magnesium-removed tailings; In the reverse flotation demagnesization process, the dispersant added to the slurry includes one or more of polymerized polyols, sodium pyrophosphate and triethylhexyl phosphate, and the mass ratio of dry basis ore volume, liquid in the slurry and dispersant is 1000:(1500-2500):(0.02-0.1).

2. The separation process according to claim 1, characterized in that: The P2O5 content of the mud-containing high-sesquioxide collophanite ore is 20-25wt%, the MgO content is 2.5-5wt%, and the sesquioxide content is 3-7wt%.

3. The separation process according to claim 1, characterized in that: The particle size of the coarsely crushed ore is 15 to 25 mm.

4. The separation process according to claim 1, characterized in that: The coarsely crushed ore is washed with water to remove mud in a vibrating screen; the particle size of the mud is less than 0.038 mm, and the solid content of the mud is 15-35%.

5. The separation process according to claim 1, characterized in that: The equipment for the first stage grinding is a rod mill; the mass ratio of the ore material to water when the rod mill is in operation is 1:(0.25-0.65).

6. The separation process according to claim 1, characterized in that: The cyclone classification of the first-stage grinding product is carried out in a cyclone group; the working pressure of the cyclone group is 45-100 kPa.

7. The separation process according to claim 1, characterized in that: The second-stage grinding is carried out in a ball mill; the cyclone classification of the second-stage grinding product is carried out in a hydrocyclone; and the working pressure of the hydrocyclone is 80-110 kPa.

8. The separation process according to claim 1, characterized in that: The intermediate-sized ore is mixed with water before being sorted on a shaking table, and the mass ratio of the ore to water is 1:(1.5-3); the equipment for the shaking table sorting is a fine sand shaking table, the bed surface inclination is 0.5-2°, the shaking table stroke is 11-18 mm, and the stroke frequency is 280-320 times / min.

9. The separation process according to claim 1, characterized in that: In the reverse flotation demagnesizing process, the flotation regulator added to the ore pulp includes sulfuric acid and / or phosphoric acid, and the demagnesizing collector added to the ore pulp is oxidized paraffin soap.

10. The separation process according to claim 1, characterized in that: The low-sesquioxide phosphate concentrate has a P2O5 content of ≥30wt%, a MgO content of ≤1wt%, and a sesquioxide content of ≤2wt%; the high-sesquioxide phosphate concentrate has a P2O5 content of ≥28wt%, a MgO content of ≤1.2wt%, and a sesquioxide content of 4-5wt%; the demagnesized tailings has a P2O5 content of ≤7wt%.