Hot and cold rolling coordinated regulation and control method for reducing same-plate difference of non-oriented silicon steel

By adopting thin slab continuous casting continuous rolling method and multi-frame continuous rolling process in the production of non-oriented silicon steel, combined with roll type and tension adjustment, the problem of large difference between the plate of non-oriented silicon steel is solved, and the optimization of cold-rolled finished products is achieved. The quality has been improved, meeting the needs of high-end products.

CN118950712AActive Publication Date: 2024-11-15BAOTOU IRON & STEEL (GROUP) CO LTD

Patent Information

Application Number
CN202410894272.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-15
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

The difference between the same plate of the finished products of non-oriented silicon steel is large, which affects the quality of the cold-rolled finished products. The hot rolling and cold rolling process are complicated, and the existing technology is difficult to effectively control the difference between the same plate, resulting in a low cold rolling yield.

Method used

The continuous casting and rolling method of thin slabs is used to control the heating temperature and temperature difference of the slabs, and the continuous rolling process and roller type adjustment are used. The cold rolling six-roller and five-strade continuous rolling mill set and roller type matching are used to adjust the tension and the roll volume to reduce the difference between the same plate.

Benefits of technology

By coordinating the hot rolling and cold rolling processes, the horizontal homogeneous plate difference of cold-rolled finished products of non-oriented silicon steel is significantly reduced, the quality and yield of cold-rolled strip steel are improved, and the demand for high-end products is met.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a hot and cold rolling coordinated regulation and control method for reducing the same-plate difference of non-oriented silicon steel, and belongs to the technical field of rolling of non-oriented silicon steel. According to the method, the matching of the hot rolling plate shape and the cold rolling mode is cooperatively controlled, so that the plate shape of the non-oriented silicon steel cold-rolled finished product is optimized and improved. Through the implementation of the method, the transverse same-plate difference of the cold-rolled strip steel is reduced to 4-8 microns, and compared with the same-plate difference of hot-rolled strip steel in the prior art which is 10-15 microns, the requirement for producing high-end non-oriented silicon steel products is met, the quality of the cold-rolled strip steel is improved, and the yield of the cold-rolled strip steel is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of non-oriented silicon steel rolling, and in particular relates to a hot and cold rolling coordinated control method for reducing the same-plate difference of non-oriented silicon steel. Background Art

[0002] At present, with the continuous development of non-oriented silicon steel production technology, users have higher and higher expectations for the plate quality of non-oriented silicon steel products. Good plate difference can significantly improve the added value of high non-oriented silicon steel products. However, the production process of non-oriented silicon steel is complex and the process flow is long. Among them, the hot rolling and cold rolling processes have the most serious impact on the plate difference of the product. The poor control performance of the plate difference of hot-rolled products will directly affect the plate difference quality of the finished products in downstream processes such as cold rolling. The plate difference of domestic hot-rolled strip is between 0.025 and 0.04 mm. Reducing the transverse plate difference of hot-rolled strip is the key to improving the quality of cold-rolled strip. Hot-rolled strip with large plate difference will lead to low cold rolling yield in the subsequent production process. Therefore, the optimization and improvement of the plate shape of non-oriented silicon steel cold-rolled finished products can be achieved by collaboratively controlling the matching of hot-rolled plate shape and cold-rolled rolling mode. Summary of the invention

[0003] In order to solve the problem of poor same-plate difference of non-oriented silicon steel finished products, the purpose of the present invention is to provide a hot and cold rolling coordinated control method for reducing the same-plate difference of non-oriented silicon steel, so as to optimize and improve the plate shape of non-oriented silicon steel cold-rolled finished products.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The present invention provides a hot and cold rolling coordinated control method for reducing the same plate difference of non-oriented silicon steel, comprising:

[0006] The hot rolling production process of non-oriented silicon steel adopts the thin slab continuous casting and rolling method. Before hot rolling, the slab is heated to the hot rolling start temperature of 1040-1080℃ in a tunnel furnace. The furnace pressure in the heating furnace is set to 20-23Pa, and the maximum temperature difference in the thickness and width directions of the slab is kept within ±20℃.

[0007] The hot rolling adopts a seven-stand continuous rolling process. The hot rolling roll type selects a roll with a small roll crown. The working roll crown of the hot rolling roll is 50-100μm. According to different rolling stages, the variable crown of the hot rolling CVC roll is adjusted, and the variable crown is -80-100μm.

[0008] Different tension adjustments are made for hot-rolled products of different thicknesses; when the thickness of the hot-rolled product is greater than 2.8mm, the strip tension increases by 1.2%-1.5%; when the thickness of the hot-rolled product is greater than 2.75mm and less than 2.8mm, the strip tension increases by 5%-8%; when the thickness of the hot-rolled product is greater than 2.65mm and less than 2.75mm, the strip tension increases by 12%-16%; when the thickness of the hot-rolled product is greater than 2.5mm and less than 2.65mm, the strip tension increases by 17%-20%; when the thickness of the hot-rolled product is less than 2.5mm, the strip tension increases by 21%-25%;

[0009] The cold rolling adopts a six-roller five-stand continuous rolling unit, and the cold rolling mode matching is carried out based on the hot rolling small crown plate rolling results;

[0010] Selection of roller type: In order to improve the ability of the rolling mill to control edge drop during the cold rolling of silicon steel, the first two stands F1 and F2 are adjusted to tapered rollers with a cubic curve on the roller surface;

[0011] Roll shifting amount for cold rolling: 60-80mm for F1 intermediate roll; 50-60mm for F2 intermediate roll;

[0012] Bending force of cold rolling working rolls: Bending force of working rolls of each stand F1: 310-320KN; F2: 320-330KN; F1-F5: 350-700KN;

[0013] Cold rolling tension: F1-F2: 150-170MPa; F2-F3: 180-200MPa; F3-F4: 220-240MPa; F4-F5: 210-230MPa.

[0014] Furthermore, the difference between hot-rolled finished plates is controlled within 15-30 μm.

[0015] Furthermore, the transverse difference of cold-rolled strip is reduced to 4-8μm.

[0016] Furthermore, the hot rolling production process of non-oriented silicon steel adopts the thin slab continuous casting and rolling method. Before hot rolling, the slab is heated to the hot rolling start temperature of 1050°C in a tunnel furnace, the furnace pressure in the heating furnace is set to 20Pa, and the maximum temperature difference in the thickness direction and the width direction of the slab is ensured to be kept within ±20°C;

[0017] The hot rolling adopts a seven-stand continuous rolling process. The hot rolling roll type selects a roll with a small roll crown, and the working roll crown of the hot rolling roll is 60μm. According to different rolling stages, the variable crown of the hot rolling CVC roll is adjusted, and the variable crown is 20μm.

[0018] Different tension adjustments are made for hot-rolled products of different thicknesses; for hot-rolled products with a thickness of 2.85 mm, the strip tension is increased by 1.5%;

[0019] The cold rolling adopts a six-roller five-stand continuous rolling unit, and the cold rolling mode matching is carried out based on the hot rolling small crown plate rolling results;

[0020] Selection of roller type: In order to improve the ability of the rolling mill to control edge drop during the cold rolling of silicon steel, the first two stands F1 and F2 are adjusted to tapered rollers with a cubic curve on the roller surface;

[0021] Roll shifting of cold rolling: 75mm for the middle roll of F1 and 55mm for the middle roll of F2.

[0022] Bending force of cold rolling working rolls: Bending force of working rolls of each stand F1: 315KN; F2: 325KN; F1-F5: 350-700KN;

[0023] Cold rolling tension: F1-F2: 156MPa; F2-F3: 186MPa; F3-F4: 230MPa; F4-F5: 213MPa.

[0024] Furthermore, the hot rolling production process of non-oriented silicon steel adopts thin slab continuous casting and rolling method. Before hot rolling, the slab is heated to the hot rolling start temperature of 1056°C in a tunnel furnace, the furnace pressure in the heating furnace is set to 22Pa, and the maximum temperature difference in the thickness direction and the width direction of the slab is ensured to be kept within ±20°C;

[0025] The hot rolling adopts a seven-stand continuous rolling process. The hot rolling roll type selects a roll with a small roll crown. The working roll crown of the hot rolling roll is 70μm. According to different rolling stages, the variable crown of the hot rolling CVC roll is adjusted, and the variable crown is 30μm.

[0026] Different tension adjustments are made for hot-rolled products of different thicknesses; for hot-rolled products with a thickness of 2.67mm, the strip tension increases by 14%;

[0027] The cold rolling adopts a six-roller five-stand continuous rolling unit, and the cold rolling mode matching is carried out based on the hot rolling small crown plate rolling results;

[0028] Selection of roller type: In order to improve the ability of the rolling mill to control edge drop during the cold rolling of silicon steel, the first two stands F1 and F2 are adjusted to tapered rollers with a cubic curve on the roller surface;

[0029] Roll shifting of cold rolling: 60mm for F1 intermediate roll and 53mm for F2 intermediate roll.

[0030] Bending force of cold rolling working rolls: Bending force of working rolls of each stand F1: 313KN; F2: 325KN; F1-F5: 350-700KN;

[0031] Cold rolling tension: F1-F2: 153MPa; F2-F3: 186MPa; F3-F4: 223MPa; F4-F5: 216MPa.

[0032] Furthermore, the hot rolling production process of non-oriented silicon steel adopts thin slab continuous casting and rolling method. Before hot rolling, the slab is heated to the hot rolling start temperature of 1045°C in a tunnel furnace, the furnace pressure in the heating furnace is set to 22Pa, and the maximum temperature difference in the thickness direction and the width direction of the slab is ensured to be kept within ±20°C;

[0033] The hot rolling adopts a seven-stand continuous rolling process. The hot rolling roll type selects a roll with a small roll crown, and the working roll crown of the hot rolling roll is 80μm. According to different rolling stages, the variable crown of the hot rolling CVC roll is adjusted, and the variable crown is 10μm.

[0034] Different tension adjustments are made for hot-rolled products of different thicknesses; for hot-rolled products with a thickness of 2.55, the strip tension increases by 18%;

[0035] The cold rolling adopts a six-roller five-stand continuous rolling unit, and the cold rolling mode matching is carried out based on the hot rolling small crown plate rolling results;

[0036] Selection of roller type: In order to improve the ability of the rolling mill to control edge drop during the cold rolling of silicon steel, the first two stands F1 and F2 are adjusted to tapered rollers with a cubic curve on the roller surface;

[0037] Roll shifting of cold rolling: 73mm for F1 intermediate roll and 53mm for F2 intermediate roll.

[0038] Bending force of cold rolling working rolls: Bending force of working rolls of each stand F1: 318KN; F2: 326KN; F1-F5: 350-700KN;

[0039] Cold rolling tension: F1-F2: 163MPa; F2-F3: 192MPa; F3-F4: 236MPa; F4-F5: 226MPa.

[0040] Compared with the prior art, the beneficial technical effects of the present invention are:

[0041] Through the implementation of this method, the transverse plate difference of cold-rolled strip is reduced to 4-8μm, compared with the hot-rolled strip difference of 10-15μm in the prior art, which meets the demand for producing high-end non-oriented silicon steel products and improves the quality and yield rate of cold-rolled strip.

[0042] The present invention optimizes and improves the plate shape of the non-oriented silicon steel cold-rolled finished product by collaboratively controlling the matching of the hot-rolled plate shape and the cold-rolled rolling mode. DETAILED DESCRIPTION

[0043] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0044] Example 1

[0045] The hot rolling production process of non-oriented silicon steel adopts thin slab continuous casting and rolling method. Before hot rolling, the slab is heated to the hot rolling start temperature of 1050℃ in a tunnel furnace. The furnace pressure in the heating furnace is set to 20Pa, and the maximum temperature difference in the thickness and width directions of the slab is kept within ±20℃.

[0046] The hot rolling adopts a seven-stand continuous rolling process. The hot rolling roll type selects rolls with small roll crown, and the working roll crown of the hot rolling roll is 60μm. According to different rolling stages, the variable crown of the hot rolling CVC roll is adjusted, and the variable crown is 20μm.

[0047] Different tension adjustments are made for hot-rolled products of different thicknesses; for hot-rolled products with a thickness of 2.85 mm, the strip tension is increased by 1.5%

[0048] The difference between hot rolled finished plates is controlled within 25μm.

[0049] The cold rolling adopts a six-roller five-stand continuous rolling mill, and the cold rolling mode is matched based on the hot rolling results of small crown plate.

[0050] Selection of roller type: In order to improve the ability of the rolling mill to control edge drop during the cold rolling of silicon steel, the first two stands F1 and F2 are adjusted to tapered rollers with a cubic curve on the roller surface;

[0051] Roll shifting of cold rolling: 75mm for the middle roll of F1 and 55mm for the middle roll of F2.

[0052] Bending force of cold rolling work rolls: Bending force of each stand work roll F1: 315KN; F2: 325KN; F1-F5: 350-700KN

[0053] Cold rolling tension: F1-F2: 156MPa; F2-F3: 186MPa; F3-F4: 230MPa; F4-F5: 213MPa.

[0054] Through the implementation of this method, the transverse plate difference of cold-rolled strip is reduced to 7μm, which meets the demand for producing high-end non-oriented silicon steel products and improves the quality and yield rate of cold-rolled strip.

[0055] Example 2

[0056] The hot rolling production process of non-oriented silicon steel adopts thin slab continuous casting and rolling method. Before hot rolling, the slab is heated to the hot rolling start temperature of 1056℃ in a tunnel furnace. The furnace pressure in the heating furnace is set to 22Pa, and the maximum temperature difference in the thickness and width directions of the slab is kept within ±20℃.

[0057] The hot rolling adopts a seven-stand continuous rolling process. The hot rolling roll type selects rolls with small roll crown, and the working roll crown of the hot rolling roll is 70μm. According to different rolling stages, the variable crown of the hot rolling CVC roll is adjusted, and the variable crown is 30μm.

[0058] Different tension adjustments are made for hot-rolled products of different thicknesses; when the thickness of the hot-rolled product is 2.67 mm, the strip tension increases by 14%

[0059] The difference between hot rolled finished plates is controlled within 20μm.

[0060] The cold rolling adopts a six-roller five-stand continuous rolling mill, and the cold rolling mode is matched based on the hot rolling results of small crown plate.

[0061] Selection of roller type: In order to improve the ability of the rolling mill to control edge drop during the cold rolling of silicon steel, the first two stands F1 and F2 are adjusted to tapered rollers with a cubic curve on the roller surface;

[0062] Roll shifting of cold rolling: 60mm for F1 intermediate roll and 53mm for F2 intermediate roll.

[0063] Bending force of cold rolling work rolls: Bending force of each stand work roll F1: 313KN; F2: 325KN; F1-F5: 350-700KN

[0064] Cold rolling tension: F1-F2: 153MPa; F2-F3: 186MPa; F3-F4: 223MPa; F4-F5: 216MPa.

[0065] Through the implementation of the method, the transverse plate difference of the cold-rolled strip is reduced to 5μm, which meets the demand for producing high-end non-oriented silicon steel products and improves the quality and yield rate of the cold-rolled strip.

[0066] Example 3

[0067] The hot rolling production process of non-oriented silicon steel adopts thin slab continuous casting and rolling method. Before hot rolling, the slab is heated to the hot rolling start temperature of 1045℃ in a tunnel furnace. The furnace pressure in the heating furnace is set to 22Pa, and the maximum temperature difference in the thickness and width directions of the slab is kept within ±20℃.

[0068] The hot rolling adopts a seven-stand continuous rolling process. The hot rolling roll type selects rolls with small roll crown, and the working roll crown of the hot rolling roll is 80μm. According to different rolling stages, the variable crown of the hot rolling CVC roll is adjusted, and the variable crown is 10μm.

[0069] Different tension adjustments are made for hot-rolled products of different thicknesses; when the thickness of the hot-rolled product is 2.55, the strip tension is increased by 18%.

[0070] The difference between hot rolled finished plates is controlled within 22μm.

[0071] The cold rolling adopts a six-roller five-stand continuous rolling mill, and the cold rolling mode is matched based on the hot rolling results of small crown plate.

[0072] Selection of roller type: In order to improve the ability of the rolling mill to control edge drop during the cold rolling of silicon steel, the first two stands F1 and F2 are adjusted to tapered rollers with a cubic curve on the roller surface;

[0073] Roll shifting of cold rolling: 73mm for F1 intermediate roll and 53mm for F2 intermediate roll.

[0074] Bending force of cold rolling work rolls: Bending force of each stand work roll F1: 318KN; F2: 326KN; F1-F5: 350-700KN

[0075] Cold rolling tension: F1-F2: 163MPa; F2-F3: 192MPa; F3-F4: 236MPa; F4-F5: 226MPa.

[0076] Through the implementation of this method, the transverse plate difference of cold-rolled strip is reduced to 6μm, which meets the demand for producing high-end non-oriented silicon steel products and improves the quality and yield rate of cold-rolled strip.

[0077] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for coordinated hot and cold rolling control to reduce the difference between non-oriented silicon steel sheets, characterized in that: include: The hot rolling production process of non-oriented silicon steel adopts the thin slab continuous casting and rolling method. Before hot rolling, the slab is heated to the hot rolling start temperature of 1040-1080℃ in a tunnel furnace. The furnace pressure in the heating furnace is set to 20-23Pa, and the maximum temperature difference in the thickness and width directions of the slab is kept within ±20℃. The hot rolling adopts a seven-stand continuous rolling process. The hot rolling roll type selects a roll with a small roll crown, and the working roll crown of the hot rolling roll is 50-100μm; According to different rolling stages, the variable crown of the hot rolling CVC roll is adjusted, and the variable crown is -80-100μm; Different tension adjustments are made for hot-rolled products of different thicknesses; when the thickness of the hot-rolled product is greater than 2.8mm, the strip tension increases by 1.2%-1.5%; when the thickness of the hot-rolled product is greater than 2.75mm and less than 2.8mm, the strip tension increases by 5%-8%; when the thickness of the hot-rolled product is greater than 2.65mm and less than 2.75mm, the strip tension increases by 12%-16%; when the thickness of the hot-rolled product is greater than 2.5mm and less than 2.65mm, the strip tension increases by 17%-20%; when the thickness of the hot-rolled product is less than 2.5mm, the strip tension increases by 21%-25%; The cold rolling adopts a six-roller five-stand continuous rolling unit, and the cold rolling mode matching is carried out based on the hot rolling small crown plate rolling results; Selection of roller type: In order to improve the ability of the rolling mill to control edge drop during the cold rolling of silicon steel, the first two stands F1 and F2 are adjusted to tapered rollers with a cubic curve on the roller surface; Roll shifting amount for cold rolling: F1 intermediate roll shifting amount 60-80mm; F2 intermediate roller shifting amount 50-60mm; Bending force of cold rolling work roll: Bending force of each stand work roll F1: 310-320KN; F2: 320-330KN; F1-F5: 350-700KN; Cold rolling tension: F1-F2: 150-170MPa; F2-F3: 180-200MPa; F3-F4: 220-240MPa; F4-F5: 210-230MPa.

2. The method for coordinated hot and cold rolling control of reducing the same sheet difference of non-oriented silicon steel according to claim 1, characterized in that: The difference between hot-rolled finished plates is controlled within 15-30μm.

3. The method for coordinated hot and cold rolling control of reducing the same sheet difference of non-oriented silicon steel according to claim 1, characterized in that: The transverse difference of cold-rolled strip is reduced to 4-8μm.

4. The method for coordinated hot and cold rolling control of reducing the same sheet difference of non-oriented silicon steel according to claim 1, characterized in that: The hot rolling production process of non-oriented silicon steel adopts thin slab continuous casting and rolling method. Before hot rolling, the slab is heated to the hot rolling start temperature of 1050℃ in a tunnel furnace. The furnace pressure in the heating furnace is set to 20Pa, and the maximum temperature difference in the thickness and width directions of the slab is kept within ±20℃. The hot rolling adopts a seven-stand continuous rolling process. The hot rolling roll type selects a roll with a small roll crown, and the working roll crown of the hot rolling roll is 60μm. According to different rolling stages, the variable crown of the hot rolling CVC roll is adjusted, and the variable crown is 20μm. Different tension adjustments are made for hot-rolled products of different thicknesses; The thickness of the hot-rolled finished product is 2.85 mm, and the strip tension increases by 1.5%; The cold rolling adopts a six-roller five-stand continuous rolling unit, and the cold rolling mode matching is carried out based on the hot rolling small crown plate rolling results; Selection of roller type: In order to improve the ability of the rolling mill to control edge drop during the cold rolling of silicon steel, the first two stands F1 and F2 are adjusted to tapered rollers with a cubic curve on the roller surface; Roll shifting of cold rolling: 75mm for the middle roll of F1 and 55mm for the middle roll of F2. Bending force of cold rolling working rolls: Bending force of working rolls of each stand F1: 315KN; F2: 325KN; F1-F5: 350-700KN; Cold rolling tension: F1-F2: 156MPa; F2-F3: 186MPa; F3-F4: 230MPa; F4-F5: 213MPa.

5. The method for coordinated hot and cold rolling control of reducing the same sheet difference of non-oriented silicon steel according to claim 1, characterized in that: The hot rolling production process of non-oriented silicon steel adopts thin slab continuous casting and rolling method. Before hot rolling, the slab is heated to the hot rolling start temperature of 1056℃ in a tunnel furnace. The furnace pressure in the heating furnace is set to 22Pa, and the maximum temperature difference in the thickness and width directions of the slab is kept within ±20℃. The hot rolling adopts a seven-stand continuous rolling process. The hot rolling roll type selects a roll with a small roll crown. The working roll crown of the hot rolling roll is 70μm. According to different rolling stages, the variable crown of the hot rolling CVC roll is adjusted, and the variable crown is 30μm. Different tension adjustments are made for hot-rolled products of different thicknesses; The thickness of the hot-rolled finished product is 2.67 mm, and the strip tension is increased by 14%; The cold rolling adopts a six-roller five-stand continuous rolling unit, and the cold rolling mode matching is carried out based on the hot rolling small crown plate rolling results; Selection of roller type: In order to improve the ability of the rolling mill to control edge drop during the cold rolling of silicon steel, the first two stands F1 and F2 are adjusted to tapered rollers with a cubic curve on the roller surface; Roll shifting of cold rolling: 60mm for F1 intermediate roll and 53mm for F2 intermediate roll. Bending force of cold rolling working rolls: Bending force of working rolls of each stand F1: 313KN; F2: 325KN; F1-F5: 350-700KN; Cold rolling tension: F1-F2: 153MPa; F2-F3: 186MPa; F3-F4: 223MPa; F4-F5: 216MPa.

6. The method for coordinated control of hot and cold rolling to reduce the same sheet difference of non-oriented silicon steel according to claim 1, characterized in that: The hot rolling production process of non-oriented silicon steel adopts thin slab continuous casting and rolling method. Before hot rolling, the slab is heated to the hot rolling start temperature of 1045℃ in a tunnel furnace. The furnace pressure in the heating furnace is set to 22Pa, and the maximum temperature difference in the thickness and width directions of the slab is kept within ±20℃. The hot rolling adopts a seven-stand continuous rolling process. The hot rolling roll type selects a roll with a small roll crown, and the working roll crown of the hot rolling roll is 80μm. According to different rolling stages, the variable crown of the hot rolling CVC roll is adjusted, and the variable crown is 10μm. Different tension adjustments are made for hot-rolled products of different thicknesses; The thickness of the hot-rolled finished product is 2.55, and the strip tension increases by 18%; The cold rolling adopts a six-roller five-stand continuous rolling unit, and the cold rolling mode matching is carried out based on the hot rolling small crown plate rolling results; Selection of roller type: In order to improve the ability of the rolling mill to control edge drop during the cold rolling of silicon steel, the first two stands F1 and F2 are adjusted to tapered rollers with a cubic curve on the roller surface; Roll shifting of cold rolling: 73mm for F1 intermediate roll and 53mm for F2 intermediate roll. Bending force of cold rolling working rolls: Bending force of working rolls of each stand F1: 318KN; F2: 326KN; F1-F5: 350-700KN; Cold rolling tension: F1-F2: 163MPa; F2-F3: 192MPa; F3-F4: 236MPa; F4-F5: 226MPa.

Citation Information

Patent Citations

  • Method of producing high-grade non-oriented electrical steel by cold continuous rolling and product thereof

    CN109622619A

  • Pickling rolling production process for thin medium-high-grade non-oriented silicon steel

    CN113198866A

  • Cold rolling method for producing high-grade non-oriented silicon steel based on UCMW cold continuous rolling mill

    CN114833195A

  • Method for producing high-magnetic-induction oriented electrical steel through cold continuous rolling and product

    CN115318830A

  • Method for reducing transverse same-plate difference of hot-rolled strip steel

    CN116713316A

Cited By

  • Method for improving section shape of non-oriented silicon steel

    CN120605954A

  • Silicon steel same-plate difference plate shape control method in hot continuous rolling-cold continuous rolling whole process

    CN121222826A