Preparation method of porous alloy screw structure for additive manufacturing and porous alloy screw structure thereof

Through additive manufacturing technology and functional gradient porous structure design, combined with epoxy resin embedding protection and CNC lathe precision machining, the problem of porosity and strength balance in traditional porous alloy screw design is solved, and the overall strength of the screw is improved and Stability simplifies manufacturing processes and expands application potential.

CN118951023AActive Publication Date: 2024-11-15CENT SOUTH UNIV

Patent Information

Application Number
CN202411217195.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-15
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

Traditional porous alloy screw design is difficult to achieve the optimal balance between porosity and strength, the welding process is complex and the porous connectivity is poor, which affects the stability and reliability of the structure.

Method used

Using additive manufacturing technology, the cylinder axis radius R and the characteristic parameters of the lattice structure are field driven by nTopology, Grasshopper or Matlab software, and functional gradient porous structure is constructed, combined with epoxy resin embedding protection and CNC lathe precision machining, to achieve Continuous gradient variation from the axis to the periphery.

Benefits of technology

It realizes seamless transition design, optimizes force, heat and liquid conduction efficiency, enhances overall strength and stability, simplifies manufacturing processes, lowers technical thresholds, and broadens the application potential of porous alloy screws in multiple fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951023A_ABST
    Figure CN118951023A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a porous alloy screw structure for additive manufacturing and the porous alloy screw structure, and belongs to the technical field of alloys. Comprising the whole process of tool and functional gradient lattice structure design, 3D printing pretreatment, titanium alloy or tantalum alloy additive manufacturing, post-treatment powder removal, heat treatment strengthening, porous area resin embedding protection, precision machining, resin removal and final detection packaging, and finally the high-performance porous alloy screw is obtained. The continuous gradient porous design from the axis to the periphery is achieved by accurately controlling the R value and field driving of lattice structure characteristic parameters, a transition interface in traditional design is eliminated, physical quantity conduction is optimized, the strength and stability of the screw are enhanced, meanwhile, the porous area is protected through the resin embedding technology, the manufacturing process is simplified, and the manufacturing cost is reduced. And the technical difficulty is reduced, the lightweight target is achieved, the quality of the finished screw is guaranteed, and the application prospects of the porous alloy screw in multiple fields are widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of alloy technology, and in particular to a preparation method of an additively manufactured porous alloy screw structure and the porous alloy screw structure. Background Art

[0002] Porous alloy screw structures are usually prepared using additive manufacturing technology. In terms of material selection, high-performance alloys such as titanium alloys, aluminum alloys, and nickel-based alloys are commonly used materials due to their excellent mechanical properties and corrosion resistance.

[0003] However, the traditional porous alloy screw design is often limited to a single pore structure, and it is difficult to achieve the best balance between porosity and strength, thus limiting its performance optimization in specific application scenarios. To solve this problem, although some studies have proposed a solution of combining an internal solid alloy with an external welded porous alloy bracket, aiming to provide strength support through an internal solid structure, while the external porous structure achieves lightweight or other specific functions, this assembly method faces many challenges in practical applications, including complex welding processes, poor porous connectivity, and weak stress at welding points, which affect the stability and reliability of the overall structure. To this end, in response to this problem, the present invention proposes a preparation method for an additively manufactured porous alloy screw structure and a porous alloy screw structure thereof. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and to provide a method for preparing an additively manufactured porous alloy screw structure and a porous alloy screw structure thereof that can overcome the above problems or at least partially solve the above problems.

[0005] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is: a preparation method of a porous alloy screw structure manufactured by additive manufacturing, comprising the following steps: S1, using a cylinder as the basic shape for the design of the porous alloy screw structure; S2, using nTopology or Grasshopper or Matlab software to field drive the axial radius R of the cylinder and the characteristic parameters of the lattice structure, to construct a functional gradient porous structure with high porosity on the periphery and low porosity on the inner surface from the axis of the cylinder along the radial direction.

[0006] S3. Process the designed model structure before 3D printing; S4. Select alloy materials and manufacture porous alloy screw precursors by additive manufacturing technology; S5. Remove residual alloy powder adhering to the porous structure by sandblasting, air blowing and ultrasonic washing; S6. Heat treat the porous alloy screw precursor; S7. Embed the porous area of ​​the porous alloy screw precursor with epoxy resin for protection; S8. Use a CNC lathe to perform precision machining on the porous alloy screw precursor;

[0007] S9. Perform heat treatment to remove the embedded resin on the processed porous alloy screws; S10. Inspect, clean, disinfect and package.

[0008] Preferably, the characteristic parameters of the lattice structure driven by the field in step S2 include the t value of the spiral dodecahedron, the rod diameters of the cubic square hole, cubic round hole, and rhombic dodecahedron structure, and the cubic size of the lattice structure. By adjusting these parameters, the overall porosity is between 40% and 90%, the beam diameter is 100-500μm, the pore diameter is 200-800μm, and the porosity of the starting area near the axis of the cylinder is between 50% and 70%, while the porosity of the end area near the outer diameter of the cylinder is between 60% and 90%.

[0009] Preferably, the epoxy resin embedding protection in the step S7 includes: S71, preparing the epoxy resin to a suitable flowing colloid state by heating, stirring or adding a diluent; S72, preparing a soft silicone bracket with a shape and size matching the porous alloy screw precursor, placing the porous alloy screw precursor in the soft silicone bracket, and then immersing or spraying the porous alloy screw precursor in the epoxy resin flowing colloid.

[0010] Preferably, the embedding resin is removed by heat treatment in the step S9, including: S91, placing the porous alloy screw precursor in a temperature-controllable aerobic furnace, setting the temperature to 400°C-500°C, and performing a heating treatment for 0.5-1h to remove the embedded epoxy resin; S92, after the heating is completed, allowing the porous alloy screw precursor to naturally cool to room temperature in the aerobic furnace, and after taking it out, carefully checking to confirm that the epoxy resin has been completely removed.

[0011] Preferably, the alloy material in step S4 is Ti6Al4V titanium alloy or grade 4 pure titanium or tantalum alloy.

[0012] Preferably, in the step S4, the powder particle size of the alloy material is 5-53 μm.

[0013] The present invention also provides an additively manufactured porous alloy screw structure, which comprises a reinforcing part made of an alloy material, wherein the reinforcing part extends from the inner center of the cylinder to the outer cylinder edge to form a gradient porous structure with gradually increasing porosity, and the reinforcing part is composed of a plurality of basic units, each of which comprises a connecting node and a plurality of connecting arms, wherein the plurality of connecting arms are used to connect between two adjacent connecting nodes, and a plurality of channels are formed between the two adjacent connecting nodes and the plurality of connecting arms.

[0014] Preferably, the basic unit comprises a spiral dodecahedron, a rhombic dodecahedron, a cubic square hole or a cubic round hole.

[0015] Preferably, when the basic unit of the reinforcement portion is a spiral dodecahedron, it includes a connecting node and twelve spiral connecting arms, and the plurality of connecting arms are used to connect between two adjacent connecting nodes, and a plurality of continuous, spiral channels are formed between the two adjacent connecting nodes and the plurality of connecting arms. The "continuous" here means that the channel has no interruption or breakpoints in space, ensuring that the fluid or substance can flow smoothly in the channel without bypassing any obstacles. At the same time, the spiral-shaped structural channel can effectively disperse stress and load when subjected to external loads. Since the spiral connecting arms are arranged in a spiral manner in space, the force can be gradually dispersed to the entire structure along the spiral path instead of concentrating it in a local area. This stress dispersion effect helps to reduce the stress concentration phenomenon of the structure, thereby improving the overall strength and bearing capacity of the structure.

[0016] Preferably, when the basic unit of the reinforcement portion is a rhombus dodecahedron, it comprises a connecting node and twelve rhombus-shaped connecting arms, and the plurality of connecting arms are used to connect between two adjacent connecting nodes, and a plurality of rhombus-shaped channels with clear edges and corners are formed between the two adjacent connecting nodes and the plurality of connecting arms. The "clear edges and corners" here refer to the clear and sharp corners or fold lines formed at the intersection of two adjacent connecting nodes and the adjacent rhombus-shaped connecting arms. These corners or fold lines have clear boundaries visually, and are not smooth or fuzzy transitions, but present obvious changes in geometric shape.

[0017] Specifically, since the connecting arm is diamond-shaped, when the connecting arm intersects with the connecting node, two acute angles and two obtuse angles are generated at the intersection point. The clear division of these angles forms the so-called "clear edges and corners", which not only add a unique geometric beauty to the entire structure, but more importantly, they also play a role in dispersing stress and enhancing structural stability in mechanics.

[0018] Preferably, when the basic unit of the reinforcement portion is a cubic square hole, it includes a connecting node and four right-angle connecting arms, and the multiple connecting arms are used to connect between two adjacent connecting nodes, so that multiple channels with square cross-sections are formed between two adjacent connecting nodes and the multiple connecting arms.

[0019] Preferably, when the basic unit of the reinforcement portion is a cubic circular hole, it includes a connecting node and four arc-shaped connecting arms, and the multiple connecting arms are used to connect between two adjacent connecting nodes, so that multiple channels with circular cross-sections are formed between two adjacent connecting nodes and the multiple connecting arms.

[0020] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0021] 1. By precisely controlling the field drive of the R value and the characteristic parameters of the lattice structure, the present invention realizes a continuous gradient change from the axis to the periphery, eliminating the obvious transition interface that may exist in the traditional design. This seamless transition design not only optimizes the conduction efficiency of physical quantities such as force, heat, and liquid inside the screw, but also further enhances the overall strength and stability of the screw, so that it can maintain excellent performance under various complex working conditions. Compared with traditional welding methods or simple partitioned porous designs, the continuous gradient porous structure of the present invention not only simplifies the manufacturing process and lowers the technical threshold, but also achieves the goal of lightweight while maintaining the strength of the screw, thereby broadening the application potential of porous alloy screws in multiple fields.

[0022] 2. Before the porous screw precursor enters the machining stage, the present invention uses resin embedding technology to carefully protect the porous area, effectively avoiding contamination of the porous area and significantly reducing the risk of surface damage of the porous area during machining, thereby ensuring the quality and performance of the finished screw.

[0023] 3. The porous alloy screw structure manufactured in one piece of the present invention realizes a fine gradient change of the lattice structure from the axial region to the outer diameter of the axial surface by constructing a field drive based on the R value of the axial surface radius of the cylinder and the characteristic parameters of the lattice structure. In the axial region, a larger rod diameter and a higher t value are used to design low porosity. The larger rod diameter significantly enhances the strength of the supporting rods in the lattice structure and provides a more stable structural support. The higher t value means that the wall thickness or rod diameter of the rod is larger than the size of the pores around it, which further improves the compactness and stiffness of the structure. The two complement each other, so that the axial region can show excellent load-bearing capacity and stability when facing external loads, thereby ensuring the reliability and durability of the overall structure of the screw;

[0024] In sharp contrast to the axial area, the peripheral area adopts a smaller rod diameter and a lower t-value design to achieve a high porosity. This design effectively reduces the material density and significantly reduces the overall weight of the screw, achieving the goal of lightweighting. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A schematic diagram of a process flow of a method for preparing a porous alloy screw structure manufactured by additive manufacturing provided by the present invention;

[0026] Figure 2 A schematic diagram of a functional gradient model structure of a reinforcement portion of an additively manufactured porous alloy screw structure provided by the present invention;

[0027] Figure 3A schematic diagram of a reinforcement forming structure of an additively manufactured porous alloy screw structure provided by the present invention;

[0028] Figure 4 A schematic diagram of the overall forming structure of an additively manufactured porous alloy screw structure provided by the present invention;

[0029] Figure 5 A schematic diagram of the three-dimensional structure of the spiral dodecahedron pores of an additively manufactured porous alloy screw structure provided by the present invention;

[0030] Figure 6 A schematic diagram of the three-dimensional structure of rhombic dodecahedron pores of an additively manufactured porous alloy screw structure provided by the present invention;

[0031] Figure 7 A schematic diagram of the three-dimensional structure of a cube-shaped square hole of a porous alloy screw structure manufactured by additive manufacturing provided by the present invention;

[0032] Figure 8 A schematic diagram of the three-dimensional structure of a cubic circular hole of a porous alloy screw structure manufactured by additive manufacturing provided by the present invention;

[0033] Fig. 9 A schematic diagram of the forming structure of the spiral dodecahedron pores of an additively manufactured porous alloy screw structure provided by the present invention;

[0034] Fig.10 A schematic diagram of the forming structure of the rhombic dodecahedron pores of an additively manufactured porous alloy screw structure provided by the present invention;

[0035] Fig.11 A schematic diagram of the forming structure of a cubic square hole of a porous alloy screw structure manufactured by additive manufacturing provided by the present invention;

[0036] Fig.12 A schematic diagram of the forming structure of cubic circular holes of a porous alloy screw structure manufactured by additive manufacturing provided by the present invention.

[0037] In the figure: 1, reinforcement part; 2, basic unit; 21, connection node; 22, connection arm. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments so that those skilled in the art can implement the invention with reference to the description.

[0039] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0040] In the description of the present invention, the terms "lateral", "longitudinal", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc. to indicate directions or positional relationships are based on the directions or positional relationships shown in the accompanying drawings and are only for the convenience of describing the present invention and simplifying the description. They do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present invention.

[0041] Reference Figure 1-Figure 4 , a method for preparing a porous alloy screw structure manufactured by additive manufacturing, comprising the following steps:

[0042] S1. With reference to commonly used implants in clinical practice, the cylinder is used as the basic shape of the porous alloy screw structure design, and the overall tooling model of the porous alloy screw is designed using SolidWorks / UG modeling software;

[0043] S2. After the overall model of the tooling is successfully imported into nTopology, Grasshopper or Matlab software, the software is used to perform field drive on the axial radius R of the cylinder and the characteristic parameters of the lattice structure, and a functional gradient porous structure with high porosity on the periphery and low porosity on the inside is constructed from the axis of the cylinder along the radial direction to the outer surface. Specifically, during the design, the characteristic parameters of the lattice structure in the field drive are the t value of the spiral dodecahedron, the rod diameter of the cubic square hole, cubic round hole, and rhombus dodecahedron structure, and the cubic size of the lattice structure. The aperture range of the porous alloy screw is set to 200 μm to 100 μm. 800μm to meet different application requirements. At the same time, the types of crystal structure characteristics include rhombic dodecahedron, spiral dodecahedron, cubic square hole and cubic round hole. These structural types each have unique mechanical and biocompatibility characteristics and can be selected according to the use requirements. By adjusting the characteristic parameters of the lattice structure, the porosity of the area close to the starting point of the cylinder axis is between 50% and 70% to ensure sufficient structural strength and stability, while the porosity of the area close to the end point of the outer diameter of the cylinder is between 60% and 90% to achieve higher porosity and looser structure, which may enhance certain specific properties, such as bone tissue ingrowth ability;

[0044] S3. Import the designed model into Magics software for model processing before additive manufacturing, slice the porous alloy screws in layers, and use the self-supporting ability of the model to reduce the support design and place them vertically;

[0045] S4. A porous alloy screw structure precursor is manufactured by selective laser cladding additive manufacturing, wherein the laser cladding additive manufacturing material is Ti6Al4V titanium alloy or grade 4 pure titanium or tantalum alloy, the powder particle size of the titanium alloy material is 5-53μm, and the laser cladding additive manufacturing process conditions are: laser spot diameter is 50-200μm, speed is 200-1100m / s, laser power is 100-300W, powder thickness is 25-60μm, and for tantalum alloy material powder particle size is 5-53μm ... The process conditions of optical cladding additive manufacturing are: laser spot diameter of 50-200μm, speed of 300-1100m / s, laser power of 200-450W, and powder thickness of 30-60μm. When implementing the above process, reference can be made to the relevant technologies and experiences in "A method for manufacturing a porous tantalum bone implant prosthesis with a medical trabecular structure by laser additive manufacturing-high temperature vacuum sintering", especially the part about porous structure design and post-processing process, so as to further optimize the performance and structural characteristics of the porous alloy screw precursor;

[0046] S5. After printing is completed and the remaining powder is blown off, the porous alloy screw precursor is removed from the printed substrate by a wire cutting machine, and the porous alloy screw precursor is removed by air blowing, sandblasting, etc. to remove the titanium powder adhered to the surface and inside of the porous implant. The cleaned porous alloy screw is placed in an ultrasonic cleaning machine for ultrasonic vibration cleaning, and then dried;

[0047] S6. The cleaned and dried porous alloy screw structure precursor is sent to the heat treatment equipment for strict heat treatment according to ASTM Standard 2924-2014, including:

[0048] Titanium alloy screw precursor: a heat treatment process of heating and holding is carried out at a temperature of 855-955°C and a vacuum degree of 1x10-1 to 1x10-5Pa. The holding time will be set to 180±60 minutes, and then the temperature is slowly lowered to 425°C and maintained for 30 minutes before the power is turned off and the temperature is lowered to less than 50°C. Finally, the vacuum operation is stopped and the porous alloy screw precursor is taken out;

[0049] Tantalum alloy screw precursor: a three-stage heating and holding heat treatment process is carried out in an environment with a vacuum degree of 1x10-1 to 1x10-5Pa. The first stage: heating to 1500°C and holding for 0.5-2h; the second stage: heating to 1650°C and holding for 0.5-2h; the third stage: heating to 1800°C and holding for 0.5-4h, then power off and cool to less than 50°C. Finally, the vacuum operation is stopped and the porous alloy screw precursor is taken out.

[0050] S7, embedding the porous area of ​​the porous alloy screw precursor with epoxy resin for protection. During embedding, the epoxy resin is prepared to a suitable flowing colloid state by heating, stirring or adding a diluent, and a soft silicone stent of a shape and size matching the porous alloy screw precursor is prepared, and the porous alloy screw precursor is placed in the soft silicone stent, and then the porous alloy screw precursor is immersed in or sprayed with the epoxy resin flowing colloid;

[0051] S8. Use a CNC lathe to put the porous alloy screw precursor taken out in step S7 into the CNC lathe, stably clamp the porous alloy screw precursor through the clamping part, accurately process the external thread of the porous alloy screw precursor according to the CAD drawing designed in step S1 to ensure that it meets the design requirements, and perform corresponding processing on the bottom conical structure and the discharge groove. After completing the external thread and the bottom processing, cut off the connection area on the screw precursor to ensure the independence and dimensional accuracy of the screw, and put the cut porous alloy screw precursor into a protective cover to protect the thread and the base part from damage in subsequent processing. Then, put the screw precursor with the protective cover into the clamping groove to ensure stable clamping. After the clamping is stable, perform hexagonal or octagonal punching processing on the porous alloy screw base connection area to meet the installation and connection requirements. After completing the punching, perform internal thread processing and preparation of the porous alloy screw to ensure the accuracy and fit of the internal thread;

[0052] S9, heat-treat the processed porous alloy screw to remove the embedded resin. When removing, place the porous alloy screw precursor in a temperature-controlled aerobic furnace, set the temperature to 400°C-500°C, and perform heating treatment for 0.5-1h to remove the embedded epoxy resin. After heating, let the porous alloy screw precursor cool naturally to room temperature in the aerobic furnace. After taking it out, carefully check to confirm that the epoxy resin has been completely removed;

[0053] S10. Finally, the porous alloy screws that have been cleaned and epoxy resin removed are placed in an ultrasonic cleaning machine for multiple ultrasonic vibration cleanings. The cleaning sequence is acetone, anhydrous ethanol, and deionized pure water, each for 30 minutes, so as to thoroughly remove any remaining organic material residues, tiny particles, and impurities. After cleaning, they are ready for subsequent use.

[0054] The implicit equation of the spiral dodecahedron mentioned in step S2 above is:

[0055]

[0056] Among them, (x, y, z) are the coordinates in three-dimensional space, l is the unit length of the porous structure, which is used to determine the periodicity and size of the spiral dodecahedron structure, t is the offset parameter of the surface, which is used to adjust the position of the surface, and f is a constant, usually set to 0, to define the position of the spiral dodecahedron surface.

[0057] The concept of field driving mentioned in the above step S2 is to associate a specific value with each grid point in the three-dimensional space. At each point P = (x, y, z) in the three-dimensional space, the scalar field F provides a corresponding value F (x, y, z). In this embodiment, a field is defined by the cross-sectional distance from the axis of the cylinder (the distance on the x, y plane). The characteristic parameter values ​​of the lattice structure are controlled and driven by this field. Higher lattice structure characteristic parameter values ​​are obtained in the area close to the axis of the cylinder, such as a larger t value, a larger rod diameter, and a higher density (i.e., a lower porosity), and lower lattice structure characteristic parameter values ​​are obtained in the area far from the axis of the cylinder. This porous structure design method based on the field-driven concept is highly precise and flexible, and can prepare multi-layer and various porous structures with complex pore distribution.

[0058] The characteristic parameters of the lattice structure mentioned in the above step S2 are the t value of the spiral dodecahedron, the rod diameter of the cubic square hole, cubic round hole, and rhombic dodecahedron structure, and the cubic size of the lattice structure.

[0059] Compared with traditional casting, forging or machining methods, this porous screw prepared by combining additive manufacturing and machining technology has higher precision of threads and screw mouths and more complex pore structure in the porous area, which can better meet the diverse needs of clinical applications. In the medical field, this porous implant can be used in bone tissue engineering, dental implants and soft tissue repair. Its excellent pore connectivity and biocompatibility help cells to attach, proliferate and differentiate, thereby accelerating tissue regeneration and repair.

[0060] In the above step S2, the specific parameters to be regulated include the t value of the spiral dodecahedron, the rod diameter of the cubic square hole, cubic round hole, and rhombic dodecahedron structure, and the cubic size of the lattice structure. By regulating these parameters, the overall porosity is achieved between 40% and 90%. While controlling the porosity, the beam diameter should be between 100-500 μm. A wider beam diameter provides stronger mechanical support, while a narrower beam diameter is conducive to increasing porosity and bioactivity. In terms of pore size, it is recommended to select within the range of 200-800 μm to support cell growth, nutrient transport, and improve interaction with the surrounding environment. However, considering that an overly large pore size may reduce mechanical strength, it is necessary to find a balance between biocompatibility and mechanical properties to ensure good biocompatibility and interactivity while maintaining sufficient mechanical strength. Therefore, the porosity of the axis starting area is maintained between 50% and 70%, while the porosity of the end area of ​​the cylindrical outer circumference is maintained between 60% and 90%.

[0061] Specifically, since a lower porosity close to 40% generally means a denser material and higher mechanical strength, but may sacrifice a certain degree of biocompatibility, a higher porosity close to 90% provides a larger bioactive surface area, but may require optimizing the beam diameter and aperture to ensure adequate mechanical support. The axial starting area is located at the core of the screw and bears the main load. In this area, selecting a porosity of 50% to 70% allows a certain degree of bioactivity while maintaining a high mechanical strength. Such a design ensures that when the screw is subjected to external loads, the core area can stably withstand stress. The end area of ​​the outer circumference of the cylinder is adjacent to the surface of the screw and is in direct contact with the surrounding tissue. Therefore, selecting the end area of ​​the outer circumference of the cylinder between 60% and 90% is conducive to enhancing the interaction between the screw and the surrounding tissue, promoting bone tissue to grow into the pores of the screw, and achieving better biological fixation. At the same time, this design also helps to improve the heat exchange performance of the screw, which is particularly important in industrial applications that require efficient heat conduction.

[0062] The powder particle size of the alloy material is controlled within the range of 5-53μm, which complies with relevant industry standards. For example, the ASTM F2924 standard specifies the particle size distribution and physical properties of metal powders used for additive manufacturing. Powder particles within this range have appropriate sphericity and fluidity, which is conducive to the formation of a uniform molten pool and a dense printing layer during the additive manufacturing process, achieving higher material uniformity and density, and ensuring that the porous alloy screw structure has excellent physical and mechanical properties and excellent biocompatibility.

[0063] Reference Figure 2-Figure 4 The present invention also provides an additively manufactured porous alloy screw structure, which is made of titanium alloy or tantalum alloy material. The titanium alloy and tantalum alloy materials have excellent biocompatibility and mechanical properties. In terms of material selection, it can be selected from Ti6Al4V titanium alloy, grade 4 pure titanium, and tantalum alloy according to the needs of actual applications. These alloy materials not only ensure the strength and stability of the screw structure, but also ensure the biosafety and durability of the porous alloy screw structure in the use environment.

[0064] Reference Figure 2 and Figure 3 In order to further improve the service strength of the additively manufactured porous alloy screw structure, the reinforcement portion 1 is specially designed to form a continuous functional gradient porous design from the inside to the outside: it can be divided into a starting area close to the axis of the cylinder and an end area close to the outer diameter of the cylinder.

[0065] In the area near the starting point of the cylinder axis, the porosity of the porous structure is relatively small. This design provides higher material density and strength, significantly enhancing the core bearing capacity of the screw. When the screw is subjected to external loads, this structure can ensure that the core area bears greater stress, thereby improving the stability of the overall structure.

[0066] In the area near the end point of the outer diameter of the cylinder, the porosity of the porous structure is relatively large. This design helps to reduce the overall density of the material and achieve lightweight screws. At the same time, this large-pore structure can improve the interaction between the screw and bone tissue or heat exchange media while maintaining sufficient mechanical strength, thereby improving the adaptability of implantation or assembly. The design of the porous structure in both the inner and outer regions ensures the strength of the screw while achieving lightweight and enhancing the interaction between the screw and the environment. It is an effective way to improve the strength of the porous alloy screw structure.

[0067] And because the driving equation group of R value and lattice structure is constructed, the gradient change is a continuous transition, and there is no transition interface between the inner and outer areas in conventional design. The conduction of force, heat and liquid is more streamlined, further improving the overall strength of the screw.

[0068] It should be noted that this porous alloy screw structure, due to its material properties and structural design, is not only suitable for the field of medical implants, but is also widely used in industrial occasions that have strict requirements on mechanical strength and pursue lightweight and efficient heat exchange.

[0069] In the field of medical implants, this porous structure can promote integration with bone tissue. This is because the large pore size provides more space and surface for bone tissue growth, which helps bone tissue grow into the pores of the screws and achieve better biological fixation. At the same time, due to the good biocompatibility of titanium alloy materials, the immune response that may be caused by the implant is reduced, further improving the success rate of the implant surgery.

[0070] In industrial applications, for example in heat exchangers, the large pore structure of the screw can increase the contact area with the heat exchange medium, thereby improving the heat conduction efficiency. This design enables the screw to transfer heat more effectively and improve the performance of the heat exchanger. Similarly, in assembly structures such as high-performance artificial intelligence robotic arms and drones, the porous structure of the screw can also enhance the bonding force with the surrounding materials, provide stable mechanical support, and ensure the stable operation of the entire system. The screw provides an ideal choice for these applications due to its stable mechanical support and efficient thermal conductivity. Therefore, the porous alloy screw structure provided in this technical solution not only meets the special needs of medical implants, but also plays an indispensable and important role in multiple industrial fields.

[0071] In the field of aerospace, it can be used for assembly screws of drones. Since drones have strict requirements on the weight and strength of components, the porous alloy screw structure design of the present technical solution adopts a gradient design with low internal porosity and high external porosity. The interior of the screw can maintain high strength to meet the requirements of the drone for structural stability in complex flight environments, while the high porosity design on the outside helps to reduce the overall weight of the screw and improve the flight efficiency of the drone, which can meet the high requirements of the drone for component strength, weight, heat dissipation and environmental adaptability.

[0072] In the field of mechanical engineering, this gradient pore structure design can also be used to manufacture components that are subjected to high loads and impacts, such as robotic arms. The internal low-porosity area ensures the strength of the component, while the external high-porosity area can reduce weight, improve heat dissipation performance, and reduce noise and vibration.

[0073] In a preferred embodiment, referring to Figure 5-Figure 12 The reinforcement part 1 is composed of a plurality of basic units 2, each of which includes a connection node 21 and a plurality of connection arms 22, the plurality of connection arms 22 are used to connect between two adjacent connection nodes 21, and a plurality of channels are formed between two adjacent connection nodes 21 and the plurality of connection arms 22, and the basic unit 2 includes a spiral dodecahedron, a rhombic dodecahedron, a cubic square hole or a cubic round hole.

[0074] When selecting different basic units 2, comprehensive consideration can be made based on the application conditions in different fields to ensure that the selected basic unit can meet specific needs and achieve the best effect.

[0075] In the medical field, the basic units of porous structures can be carefully selected according to the different needs of surgical scenarios. For scenarios that promote cell attachment and proliferation, such as fracture repair, the spiral dodecahedron is an ideal choice with its unique spiral pore design, which is conducive to cell growth and nutrient transport. In scenarios that require a balance between mechanical support and biological performance, the rhombic dodecahedron provides sufficient support while promoting bone tissue ingrowth by optimizing porosity and mechanical properties. For large-scale production and standardized applications, cubic square holes / cubic round holes become efficient and reliable choices with their regular geometric shapes and easily controllable porosity. In addition, due to their strong resistance to compression, they provide sufficient support in application scenarios such as intervertebral fusion devices or joint gaskets. These carefully selected basic units are precisely controlled by additive manufacturing technology to ensure the best effect of medical implants during surgery and promote the rehabilitation and recovery of patients.

[0076] In the industrial field, choosing a suitable basic unit 2 is of great significance for achieving efficient production, ensuring product quality and extending equipment life. For example, in the design of a heat exchanger, a basic unit 2 of a rhombic dodecahedron or a cubic square hole can be selected. The sharp channels of the rhombic dodecahedron help to increase the contact area with the heat exchange medium and improve the heat exchange efficiency, while the cubic square hole basic unit 2 provides regular channels and a larger internal space as well as better compressive strength, which facilitates fluid flow and heat transfer.

[0077] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which are equivalent modifications and improvements made to the above embodiments based on the essential technology of the present invention, and all of them belong to the protection scope of the present invention.

Claims

1. A method for preparing a porous alloy screw structure by additive manufacturing, characterized in that: The following steps are involved: S1. The cylinder is used as the basic shape for the porous alloy screw structure design; S2. Field-driven the axial radius R of the cylinder and the characteristic parameters of the lattice structure by using nTopology, Grasshopper or Matlab software to construct a functional gradient porous structure with high porosity on the periphery and low porosity on the interior from the axis of the cylinder to the outer surface in the radial direction, so as to gradually increase the porosity; S3, processing the designed model structure before 3D printing; S4, selecting alloy materials, and manufacturing a porous alloy screw precursor by additive manufacturing technology; S5, removing the residual alloy powder adhering to the porous structure by sandblasting, air blowing and ultrasonic washing; S6. heat treating the porous alloy screw precursor; S7, embedding and protecting the porous area of ​​the porous alloy screw precursor with epoxy resin; S8. Use a CNC lathe to perform precision machining on the porous alloy screw precursor; S9, performing heat treatment to remove the embedded resin on the processed porous alloy screws; S10, testing, cleaning, disinfection and packaging.

2. The method for preparing a porous alloy screw structure by additive manufacturing according to claim 1, characterized in that: The characteristic parameters of the lattice structure driven by the field in step S2 include the t value of the spiral dodecahedron, the rod diameters of the cubic square hole, cubic round hole, and rhombic dodecahedron structure, and the cubic size of the lattice structure. By adjusting these parameters, the overall porosity is between 40% and 90%, the beam diameter is 100-500μm, the pore diameter is 200-800μm, and the porosity of the starting area near the axis of the cylinder is between 50% and 70%, while the porosity of the end area near the outer diameter of the cylinder is between 60% and 90%.

3. The method for preparing a porous alloy screw structure by additive manufacturing according to claim 1, characterized in that: The alloy material in step S4 is Ti6Al4V titanium alloy or grade 4 pure titanium or tantalum alloy.

4. The method for preparing a porous alloy screw structure by additive manufacturing according to claim 1, characterized in that: The powder particle size of the alloy material in step S4 is 5-53 μm.

5. The method for preparing a porous alloy screw structure by additive manufacturing according to claim 1, characterized in that: The epoxy resin embedding protection in step S7 includes: S71, preparing the epoxy resin into a suitable fluid colloid state by heating, stirring or adding a diluent; S72. Prepare a soft silicone stent of a shape and size matching the porous alloy screw precursor, place the porous alloy screw precursor in the soft silicone stent, and then immerse or spray the porous alloy screw precursor in epoxy resin flow colloid.

6. The method for preparing a porous alloy screw structure by additive manufacturing according to claim 1, characterized in that: The heat treatment and removal of the embedding resin in step S9 includes: S91, placing the porous alloy screw precursor in a temperature-controllable oxygen furnace, setting the temperature to 400° C.-500° C., and performing a heating treatment for 0.5-1 h to remove the embedded epoxy resin; S92. After heating is completed, the porous alloy screw precursor is allowed to cool naturally to room temperature in the aerobic furnace. After being taken out, a careful inspection is performed to confirm that the epoxy resin has been completely removed.

7. An additively manufactured porous alloy screw structure, characterized in that: Obtained by the preparation method according to claim 1, comprising: A reinforcement part made of an alloy material, wherein the reinforcement part extends from the inner center of the cylinder to the outer cylinder edge to form a gradient porous structure with gradually increasing porosity; The reinforcement part is composed of a plurality of basic units, each of which includes a connection node and a plurality of connection arms. The plurality of connection arms are used to connect between two adjacent connection nodes, and a plurality of channels are formed between two adjacent connection nodes and the plurality of connection arms.

8. The additively manufactured porous alloy screw structure according to claim 7, characterized in that: The basic units include a spiral dodecahedron, a rhombic dodecahedron, a cubic square hole or a cubic round hole.

9. The additively manufactured porous alloy screw structure according to claim 8, characterized in that: When the basic unit of the reinforcement portion is a spiral dodecahedron, it includes a connecting node and twelve spiral connecting arms, and multiple connecting arms are used to connect between two adjacent connecting nodes, and multiple continuous, spiral channels are formed between two adjacent connecting nodes and multiple connecting arms.

10. The additively manufactured porous alloy screw structure according to claim 7, characterized in that: When the basic unit of the reinforcing portion is a rhombic dodecahedron, it comprises a connecting node and twelve rhombic connecting arms, and a plurality of the connecting arms are used to connect between two adjacent connecting nodes, and a plurality of angular and rhombic channels are formed between the two adjacent connecting nodes and the plurality of the connecting arms.

11. The additively manufactured porous alloy screw structure according to claim 7, characterized in that: When the basic unit of the reinforcement part is a cubic square hole, it includes a connecting node and four right-angle connecting arms, and the multiple connecting arms are used to connect between two adjacent connecting nodes, and multiple channels with square cross-sections are formed between the two adjacent connecting nodes and the multiple connecting arms.

12. The additively manufactured porous alloy screw structure according to claim 7, characterized in that: When the basic unit of the reinforcement part is a cubic circular hole, it includes a connecting node and four arc-shaped connecting arms, and the multiple connecting arms are used to connect between two adjacent connecting nodes, and multiple channels with circular cross-sections are formed between the two adjacent connecting nodes and the multiple connecting arms.

Citation Information

Patent Citations

  • Design and additive manufacturing method of gradient porous structure heat dissipation device based on temperature distribution

    CN112191849A

  • Preparation device and method of sample for measuring appearance of cable sheath and test method

    CN113358453A

  • Radial gradient porous structure with complete lattice interface, preparation method and application

    CN117017577A

  • Tantalum-modified porous titanium alloy material with imitated bone trabecula structure and preparation method of tantalum-modified porous titanium alloy material

    CN117512541A

  • Variable density lattice metal having vibration damping characteristics and additive manufacturing method therefor

    WO2023066408A2

Cited By

  • Multi-scale hybrid lattice structure interface transition optimization method

    CN121859472A

  • A multi-scale hybrid lattice structure interface transition optimization method

    CN121859472B