3D printed laser gyroscope shell as well as preparation method and application thereof
Through SLM technology and heat treatment, the problem of difficulty in preparing complex and precise laser gyro shells in traditional processing methods is solved, and an efficient and low-cost manufacturing process is achieved, and the accuracy and performance requirements of laser gyro shells are met.
Patent Information
- Application Number
- CN202411064294.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional equal-material or reduced-material processing methods are difficult to quickly and efficiently prepare precision laser gyro shells with complex structures and lightweight, resulting in problems of long cycles, high process conditions and high cost.
Selective laser melting (SLM) technology is used to regulate the composition and physical and chemical properties of alloy powder, adjust the process parameters of the SLM process, and directly and quickly print the molded metal components, and perform subsequent heat treatment to remove residual stress and improve component performance.
It realizes high-precision manufacturing of laser gyroscope shells with complex structure and lightweight, meets the requirements of sealing properties and mechanical properties, reduces production costs and process conditions, and improves production efficiency.
Smart Images

Figure CN118951044A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal parts processing, and in particular to a 3D printed laser gyroscope housing and a preparation method and application thereof. Background Art
[0002] The gyro housing and gyro base are two key components of the gyro, each of which has different performance requirements and functions. The gyro base refers to the platform on which the gyro is installed and fixed. It needs to have higher mechanical strength and good heat dissipation performance. The laser gyro housing needs to have sufficient rigidity, stability and sealing. The high-precision manufacturing of the resonant structure needs to be considered. The geometric accuracy and internal stress of the housing have a direct impact on the performance of the gyroscope to ensure that its shape and size can be maintained under various environmental conditions, and the internal optical and electronic components are protected from the influence of the external environment. On the premise of meeting the performance requirements, the housing should be as light as possible to reduce the impact on the entire system. Therefore, the selection of housing materials and processing technology is crucial.
[0003] Due to the complex shape of the laser gyroscope shell and the high precision requirements, the traditional method is to use equal material or subtractive processing, but it has the characteristics of long cycle, high process conditions and cost, and is not suitable for the preparation of complex and lightweight precision alloy parts. Summary of the invention
[0004] In view of the above analysis, an embodiment of the present invention aims to provide a 3D printed laser gyroscope shell and a preparation method and application thereof, so as to solve at least one of the problems in the prior art of long preparation cycle, high process conditions and high cost of complex and lightweight precision laser gyroscope shells.
[0005] In a first aspect, the present invention provides a 3D printing method for a laser gyroscope housing, the method comprising:
[0006] (1) Preparing laser gyroscope shell alloy powder;
[0007] (2) importing the three-dimensional design drawing of the laser gyroscope shell into an SLM printing device, placing the alloy powder in a powder cylinder of the SLM printer, setting process parameters, and printing to obtain an alloy component;
[0008] (3) Heat treating the alloy component.
[0009] Furthermore, in terms of mass percentage, the composition of the alloy powder specifically includes: C: 0-0.05%, Mn: 0.2-0.6%, Si: 0-0.3%, P: 0-0.02%, S: 0-0.002%, Ni: 35-37%, and the rest is Fe.
[0010] Furthermore, the alloy powder has a particle size of 15-63 μm, a powder hollow ratio of ≤1%, and an oxygen content of ≤200 ppm.
[0011] Furthermore, in step (1), the alloy powder is prepared by smelting + supersonic inert gas vacuum atomization method.
[0012] Furthermore, the smelting conditions are: vacuum degree <10 -2 Pa, the refining temperature is 1550-1650℃, and the time is 10-20min; the conditions of the supersonic inert gas vacuum atomization are: the insulation temperature is 1680±25℃, the insulation time is 15min, the leakage bag temperature is 1250±20℃, the leakage nozzle aperture is 4mm, the annular gap is 0.9mm, and the atomization pressure is 3-4MPa.
[0013] Furthermore, in step (2), the process parameters include: scanning speed of 950-1150 mm / s, line spacing of 0.12-0.18 mm, layer thickness of 30 μm, and output power of 190-220 W.
[0014] Furthermore, in step (3), the post-treatment is heat treatment.
[0015] Furthermore, the heat treatment step comprises: heating the alloy component obtained in step (2) to 820-860°C, keeping the temperature for 1-2 hours, and water quenching; keeping the temperature at 305-325°C for 1-2 hours, and cooling.
[0016] In a second aspect, the present invention provides a laser gyroscope housing, which is manufactured by the method described in the first aspect.
[0017] Furthermore, the linear expansion coefficients of the component in the horizontal direction and the vertical direction at -60 to 100°C are ≤1×10 -6 / ℃,≤1×10 -6 / ℃.
[0018] Furthermore, the tensile strength of the component in the horizontal direction and the vertical direction are ≥450MPa and ≥410MPa respectively.
[0019] Furthermore, the yield strength of the component in the horizontal direction and the vertical direction are ≥290MPa and ≥270MPa respectively.
[0020] Furthermore, the elongation after fracture of the component in the horizontal direction and the vertical direction is ≥33% and ≥37% respectively.
[0021] In a third aspect, the present invention provides a laser gyroscope shell for use in aerospace, navigation, military fields, earth science research, industrial automation, and autonomous driving, wherein the laser gyroscope shell is manufactured by the method described in the first aspect.
[0022] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0023] 1. The present invention utilizes the selective laser melting (SLM) technology to directly and rapidly print the designed alloy powder into metal components, and further prepares a complex and lightweight alloy laser gyroscope shell, which meets the requirements for the sealing of the laser gyroscope shell in practical applications; the SLM metal components are post-processed to remove the residual stress inside the components, improve the performance of the components, reduce the deformation in practical applications, and meet the requirements for high geometric accuracy of the laser gyroscope shell. Figure 3 The invention discloses a three-axis laser gyroscope shell component with a complex structure.
[0024] 2. The present invention adjusts the process parameters of the SLM process by regulating the composition and physicochemical properties of the alloy powder, so that the laser gyroscope shell can be manufactured by a process completely different from the traditional process of equal material or subtractive processing, and the manufactured laser gyroscope shell has high precision and no deformation; the microstructure of the shell is highly uniform, without pores, cracks and slag inclusions; in addition, the overall component has good performance: low linear expansion coefficient (≤1×10 -6 / ℃), good mechanical properties (tensile strength ≥410MPa, yield strength ≥270MPa, elongation after fracture ≥33%), which can meet the requirements of rigidity and thermodynamic stability in practical applications of laser gyroscope shells.
[0025] 3. The present invention reduces the adverse effects of directional differences on performance and improves the performance and reliability of components by optimizing the preparation process parameters. The thermal and mechanical properties of the prepared laser gyroscope shell have small differences in the horizontal and vertical directions, and the performance in each direction can meet the actual application requirements of the laser gyroscope shell, avoiding deformation or cracking during use.
[0026] 4. The preparation method of the present invention has a simple process flow, is easy to operate, and has a short processing cycle. While ensuring the good performance of the laser gyroscope shell, it improves the production efficiency of the product, reduces the process conditions and production costs, and further expands the application of components in multiple fields such as automobiles, aerospace, energy, medical care, molds, nuclear industry, precision instruments, communications, and electronics.
[0027] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.
[0029] Figure 1 The morphology and particle size distribution diagram of alloy powder 1 (4J36) in Example 1;
[0030] Figure 2 is the XRD pattern of alloy powder 1 (4J36) in Example 1;
[0031] Figure 3 The three-axis laser gyroscope shell prepared in Example 1;
[0032] Figure 4 The microstructure diagram of the three-axis laser gyroscope shell prepared in Example 1;
[0033] Figure 5 This is an optical microscope image of the three-axis laser gyroscope housing prepared in Example 2;
[0034] Figure 6 This is an optical microscope image of the three-axis laser gyroscope shell prepared in comparative example 1. DETAILED DESCRIPTION
[0035] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0036] The laser gyro housing needs to have sufficient rigidity, stability and sealing to ensure that it can maintain its shape and size under various environmental conditions and protect the internal optical and electronic components from the external environment. While meeting performance requirements, the housing should be as light as possible to reduce the impact on the entire system.
[0037] Due to the complex shape of the laser gyroscope shell and the high precision requirements, the traditional equal material or subtractive processing methods have a long cycle, high process conditions and costs, and are not suitable for the preparation of complex and lightweight precision alloy parts.
[0038] Therefore, the present invention provides a 3D printing method for a laser gyroscope housing, the method comprising:
[0039] (1) Preparing laser gyroscope shell alloy powder;
[0040] (2) importing the three-dimensional design drawing of the laser gyroscope shell into an SLM printing device, placing the alloy powder in a powder cylinder of the SLM printer, setting process parameters, and printing to obtain an alloy component;
[0041] (3) Post-processing the alloy component.
[0042] The complexity of the shape and high precision of the laser gyroscope shell place higher demands on its materials and manufacturing process.
[0043] Selective laser melting (SLM) is the most widely used additive manufacturing technology. This technology uses a high-energy laser beam to selectively melt a pre-laid thin layer of metal powder, waits for it to solidify and form, and then produces high-density, high-precision three-dimensional metal parts after layer-by-layer stacking. The technical characteristics of layered scanning and stacking enable it to form various complex and special-shaped structures that are difficult to manufacture with traditional processing technologies, greatly improving the design freedom.
[0044] However, the study found that the materials of complex and lightweight precision components 3D printed using SLM have high thermal expansion coefficients and poor mechanical properties, and their application range is limited. They are not suitable for scenarios with large temperature changes and high precision requirements. In addition, when using SLM to 3D mold different materials, the requirements for SLM process parameters are different. If the process selection and adjustment are not appropriate, some defects may also occur during the SLM printing process, such as: spheroidization, pores, geometric deformation, cracks, etc. These defects will affect the quality and performance of the printed components.
[0045] The present invention utilizes the selective laser melting (SLM) technology to control the composition and physicochemical properties of alloy powders, adjust the process parameters of the SLM process, and directly and quickly print the designed alloy powder into metal components, thereby further preparing a laser gyroscope shell with a complex structure and light weight; combined with the subsequent heat treatment of the SLM metal components, the residual stress inside the components is removed, and the performance of the components is improved, so that the prepared laser gyroscope shell has high precision and no deformation; and the shell microstructure has high uniformity, no pores, cracks and slag inclusions, and has good performance, which can meet the requirements of practical applications. Figure 3 The invention discloses a three-axis laser gyroscope shell component with a complex structure.
[0046] The laser gyroscope shell has a complex shape and needs to have good impact resistance. It also needs to meet the requirements of geometric accuracy, internal stress, and lightweight. At the same time, it needs to meet the needs of SLM printing. Therefore, the material for preparing the laser gyroscope shell needs to be designed.
[0047] The composition of the alloy powder of the present invention specifically includes, by mass percentage, C: 0-0.05%, Mn: 0.2-0.6%, Si: 0-0.3%, P: 0-0.02%, S: 0-0.002%, Ni: 35-37%, and the rest is Fe. In the temperature range of -60 to 100°C, the alloy has a low thermal expansion coefficient and is suitable for use in environments with large temperature changes and high precision requirements.
[0048] Nickel is a key element in this alloy, which can significantly reduce the alloy's thermal expansion coefficient. The strong bonding force between nickel atoms allows the alloy to maintain good dimensional stability when the temperature changes. This is a key factor in achieving a low thermal expansion coefficient in the alloy within the temperature range of -60 to 100°C. The high nickel content in the alloy and the low content of harmful elements (carbon, phosphorus, and sulfur) work together to enable the 4J36 alloy to maintain a low thermal expansion coefficient in the temperature range of -60 to 100°C.
[0049] In order to improve the quality and performance of SLM printed components, the present invention not only limits the composition of the alloy powder used, but also needs to limit the physical and chemical properties of the alloy so as to better meet the process requirements of additive manufacturing.
[0050] Specifically, the alloy powder has a high sphericity, a particle size of 15-63 μm, a powder hollow ratio of ≤1%, and an oxygen content of ≤200 ppm.
[0051] The alloy powder of the present invention has a high sphericity, such as Figure 1 As shown, it is conducive to the flow of powder. The fluidity of powder determines the uniformity and consistency of the SLM powder spreading process. Good fluidity can ensure that each layer of powder can be evenly laid on the substrate without defects such as cracks and warping, thereby avoiding defects or errors in the printing process.
[0052] The particle size range of the alloy powder of the present invention is 15-63 μm. The powder particle size is small, the alloy powder has a high loose density, reduces the voids and defects in the powder bed, is conducive to achieving high-precision printing of components and smoother surface quality, and is conducive to improving the density of components. According to a preferred embodiment of the present invention, the particle size of the alloy powder is mainly concentrated in 20-30 μm. Figure 1 As shown, the size is concentrated, which is conducive to laser focusing to melt the powder and ensure uniform melting and solidification of the alloy powder.
[0053] The alloy powder of the present invention has a relatively low hollow ratio (≤1%), reduces pores and defects during the SLM process, and is beneficial to improving the density of components.
[0054] The alloy powder of the present invention has a low oxygen content of less than 200 ppm. On the one hand, it avoids the generation of metal oxides during the SLM process, which leads to a decrease in metal purity and affects the mechanical properties of the component; on the other hand, it is not easy to generate gas during the melting process of the metal powder, avoiding the formation of holes or other defects during the solidification process, thereby ensuring the density and integrity of the component.
[0055] The alloy powder used for SLM printing of the present invention is prepared by the process of "smelting + supersonic inert gas vacuum atomization powder making".
[0056] Specifically, the process steps of "melting + supersonic inert gas vacuum atomization powder making" include:
[0057] S1: Prepare the master alloy ingot according to the alloy ratio and through the "vacuum melting + electroslag remelting" process;
[0058] S2: Low alloy powder is produced by supersonic inert gas vacuum atomization powder making process.
[0059] Specifically, the alloy has the following composition by mass percentage: C: 0-0.05%, Mn: 0.2-0.6%, Si: 0-0.3%, P: 0-0.02%, S: 0-0.002%, Ni: 35-37%, and the rest is Fe.
[0060] The specific steps of step S1 are:
[0061] S1-1: According to the alloy composition ratio, smelting is carried out using a 200 kg vacuum induction furnace + electroslag remelting;
[0062] S1-2: Vacuum to 10 -2 Pa, start heating, add alloy elements in order from low melting point to high melting point, the refining temperature is 1550-1650℃, the refining time is 10-20min, and the alloy ingot is obtained;
[0063] S1-3: electroslag remelting the alloy ingot to further purify it to obtain a master alloy ingot.
[0064] In step S2, the specific process of supersonic inert gas vacuum atomization powder making is: placing the master alloy ingot obtained in step S1 under vacuum or protective atmosphere, keeping it at 1680±25°C for 15 minutes to melt it; the ladle temperature is 1250±20°C, the nozzle aperture is 4mm, the annular gap is 0.9mm, and the atomization pressure is 3-4MPa. By adjusting the nozzle aperture and / or the atomization pressure, a finer powder particle size and a more uniform particle size distribution can be obtained.
[0065] The present invention obtains the particle size of the alloy powder by screening or microscopy; obtains the hollow ratio of the alloy powder by scanning electron microscope observation or image processing-analysis software measurement; and obtains the oxygen content of the alloy powder by reduction-extraction method or pulse heating inert gas melting-coulometric titration method.
[0066] It should be noted that in order to ensure the quality and accuracy of SLM printing, process parameters such as laser power and scanning speed need to be strictly controlled.
[0067] Specifically, the present invention defines the process parameters in the above step (2) as follows: scanning speed is 950-1150 mm / s, line spacing is 0.12-0.18 mm, layer thickness is 30 μm, and output power is 190-220 W.
[0068] Laser power is one of the key factors in the SLM process, which directly affects the melting degree of alloy powder and the quality of the formed components. If the laser power is too low, the alloy powder will not be fully melted, which may easily lead to the presence of unmelted metal powder inside the component, resulting in defects such as holes and non-density inside the component, affecting the strength and density of the component. If the laser power is too high, the alloy powder will be over-melted, spheroidizing and splashing will occur, resulting in excessively large grains, under-fusion and porosity defects, and will also cause the next alloy powder layer to be uneven and uneven, affecting the tensile strength and fatigue resistance of the formed component.
[0069] Laser scanning speed is also one of the key parameters in the SLM process, which will affect the microstructure and mechanical properties of the component; if the scanning speed is too fast, the laser beam will stay on the metal powder bed for too short a time, which may lead to insufficient melting of the metal powder or reduce the fluidity of the melt, affecting the density and mechanical properties of the molded part; if the scanning speed is too slow, it will easily cause excessive sintering of the alloy powder and increase the risk of thermal cracks, leading to molding defects, and will also cause the processing time to be too long, reducing production efficiency.
[0070] The distance between adjacent scanning lines will also affect the molding quality and mechanical properties of the parts. If the line spacing is too large, the molten pools will not be able to fully combine, resulting in incompletely melted powder particles inside the component, thus affecting the strength and density of the component; if the line spacing is too small, the molten pools will overlap excessively, the material will be over-melted, and unnecessary heat accumulation will occur, which can easily lead to spheroidization and spattering, affecting the quality of the component; in addition, too small a line spacing will also reduce production efficiency.
[0071] During the SLM process, the thickness of each layer of alloy powder will directly affect the printing accuracy and surface quality. If the powder thickness is too thick, the laser beam will not be able to penetrate completely, and the alloy powder will not be fully melted, which will affect the density and mechanical properties of the component. If the powder thickness is too thin, it may cause overburning or insufficient bonding between layers, and will also increase costs.
[0072] In order to ensure that the SLM molded components meet the final application requirements, the alloy components obtained in step (2) of the present invention need to be post-processed to improve the performance, precision and surface quality of the components.
[0073] Specifically, the post-processing of the present invention includes the removal of residual powder on the product surface, heat treatment, removal of printing support structures, and surface treatment. First, the excess alloy powder on the surface of the rough product is removed to make the outline of the component cleaner and facilitate further subsequent processing. The excess alloy powder on the surface of the rough product can be removed by a soft brush or a vacuum cleaner; the chemical composition and organization on the surface or inside of the material are changed by means of heating, heat preservation and cooling to eliminate the residual stress inside the component and improve the mechanical properties and stability of the material; the printing support structure is used to ensure the stability of the component during the SLM process. These support structures need to be removed in the post-processing to facilitate subsequent surface processing. The printing support structure can be removed by mechanical methods or chemical dissolution; in order to improve the smoothness and fineness of the surface of the final product, the component is further surface treated by grinding, polishing or sandblasting.
[0074] Specifically, the heat treatment step of the present invention includes: heating the alloy component obtained in step (2) to 820-860°C, keeping the temperature for 1-2 hours, and water quenching; keeping the temperature at 305-325°C for 1-2 hours, and cooling. By adjusting the heat treatment process steps and parameters to change the microstructure of the SLM molded component, the residual stress inside the component is reduced, the directional difference is improved, and the thermal and mechanical properties of the alloy component are less affected.
[0075] It should be noted that in order to reduce the risk of component deformation and cracking during heat treatment and improve the yield of components; improve the overall performance of SLM molded components, meet the use requirements under complex working conditions, and extend the service life; and improve the heat treatment efficiency and reduce energy consumption, the present invention performs segmented heat treatment on the components at high and low temperatures respectively.
[0076] During the SLM molding process, due to the rapid melting and solidification of metal powder, large residual stress will be generated inside the component. High-temperature heat treatment can promote phase change and recrystallization inside the component, eliminating or reducing the residual stress generated during the SLM process; by controlling the temperature and time of the high-temperature heat treatment section, the residual stress can be refined and evenly distributed, which helps to improve the strength and toughness of the structure.
[0077] The low-temperature heat treatment stage helps to stabilize the constructed microstructure, prevent transitional changes or phase changes in the internal structure of the component after high-temperature heat treatment, and ensure the stability of component performance; low-temperature heat treatment further eliminates or reduces the stress concentration phenomenon generated in the high-temperature heat treatment stage, and reduces the risk of cracking of the component during use; the thermal stress of the material under low-temperature heat treatment is small and the structure is relatively stable, so low temperature helps to reduce component deformation caused by heat treatment.
[0078] The present invention can give full play to the effects of these two stages through reasonable heat treatment process design, thereby improving the performance and quality of SLM molded components.
[0079] The present invention adjusts the composition and physicochemical properties of the alloy powder and the process parameters of the SLM process, so that the prepared laser gyroscope shell has high precision and no deformation; the shell microstructure is highly uniform, without pores, cracks and slag inclusions; in addition, the overall component has good performance: low linear expansion coefficient (≤1×10 -6 / ℃), good mechanical properties (tensile strength ≥410MPa, yield strength ≥270MPa, elongation after fracture ≥33%), and can meet the requirements of practical applications.
[0080] Alloys with low expansion coefficients have complex crystal structures and special thermal expansion characteristics. When they are applied to additive manufacturing, the process window is relatively narrow, and the control during the printing process is more difficult to master. In addition, there are large differences in the directionality of the prepared alloy components, which seriously affect the mechanical properties, microstructure, fatigue life and durability, residual stress and other aspects of the complex and lightweight precision alloy parts, causing the components to easily deform or crack during use. When using SLM printing, it is necessary to further solve the problem caused by the large difference in directionality.
[0081] The present invention regulates the composition and physicochemical properties of alloy powder and adjusts the process parameters of the SLM process, so that the performance difference between the horizontal and vertical directions of the components 3D printed by the SLM technology is relatively small. After the components are subjected to segmented heat treatment, the difference in this direction becomes smaller, the internal microstructure is more uniform, the component performance tends to be isotropic, the adverse effect of directional difference on performance is reduced, the performance and reliability of the components are improved, the thermal properties and mechanical properties of the prepared laser gyroscope shell are relatively small in the horizontal and vertical directions, and the performance in each direction can meet the actual application requirements of the laser gyroscope shell, avoiding deformation or cracking during use.
[0082] Specifically, the linear expansion coefficients of the component in the horizontal direction and the vertical direction at (-60)-100°C are ≤1×10 -6 / ℃,≤1×10 -6 / ℃.
[0083] Specifically, the tensile strength of the component in the horizontal and vertical directions is ≥450MPa and ≥410MPa respectively, the yield strength of the component in the horizontal and vertical directions is ≥290MPa and ≥270MPa respectively, and the elongation after fracture of the component in the horizontal and vertical directions is ≥33% and ≥37% respectively.
[0084] It can be seen from the data in the specific embodiments of the present invention that the linear expansion coefficient, strength and elongation after fracture of the component before and after heat treatment change little, indicating that the heat treatment process of the present invention has little effect on the thermal and mechanical properties of the alloy component while removing the stress of the component.
[0085] The present invention utilizes a thermal expansion tester (such as an inductive expansion instrument, a telescope direct reading device or a laser scanning thermal expansion instrument, etc.) to measure the linear expansion coefficient of a component.
[0086] Example 1
[0087] Alloy powder 1 (4J36) is prepared, and component 1 three-axis laser gyroscope housing is 3D printed by SLM technology, the steps comprising:
[0088] (1) The mass fractions of the main alloying elements in the alloy powder 1 are C: 0.015%, Mn: 0.39%, Si: 0.14%, P: 0.003%, S: 0.001%, Ni: 36.30%, and the rest is Fe; according to the alloy composition ratio, a 200 kg vacuum induction furnace + electroslag remelting is used for smelting, and the vacuum is 10 -2 Pa, the refining temperature is 1620°C, the refining time is 20 min, and an alloy ingot is obtained; the alloy ingot is further purified by electroslag remelting to obtain a mother alloy ingot;
[0089] (2) Using supersonic inert gas vacuum atomization to prepare powder, keep it at 1690°C for 15 minutes to make it melt; the temperature of the ladle is 1260°C, the aperture of the nozzle is 4mm, the annular gap is 0.9mm, and the atomization pressure is 3MPa. The particle size range of the alloy powder 1 is 15-53μm, and it is set aside. Figure 1 As shown, the powder has a high sphericity, an average particle size of 29 μm, an oxygen content of 174 ppm, and a single-phase FCC (face-centered cubic) structure ( Figure 2 );
[0090] (3) The three-dimensional design drawing of the three-axis laser gyroscope shell was imported into the SLM printing equipment, and the alloy powder 1 was placed in the powder cylinder of the SLM printer. The process parameters were set as follows: the scanning speed was 1000 mm / s, the line spacing was 0.12 mm, the layer thickness was 30 μm, and the output power was 200 W. The alloy component 1 was printed. The linear expansion coefficients of the alloy component 1 in the horizontal and vertical directions at -60 to 100 °C were 0.49×10 -6 / ℃、0.62×10 -6 / ℃, the tensile strength of alloy component 1 in horizontal and vertical directions are 458MPa and 423MPa respectively, the yield strength is 379MPa and 345MPa respectively, and the elongation after fracture is 33.5% and 37.5% respectively;
[0091] (4) The alloy component 1 is subjected to heat treatment, specifically comprising: keeping the alloy component 1 at 840° C. for 1 hour, and quenching the alloy component 1 with water; keeping the alloy component 1 at 320° C. for 1 hour, and cooling the alloy component 1 with furnace cooling; Figure 3 The three-axis laser gyro shell shown in the figure; the alloy component 1 after heat treatment has a complex structure, is lightweight, has high precision, and has no cracking and deformation; the linear expansion coefficients of the alloy component 1 in the horizontal and vertical directions at -60 to 100°C are 0.86×10 -6 / ℃、0.98×10 -6 / ℃; after heat treatment, the tensile strength of alloy component 1 in horizontal and vertical directions are 452MPa and 415MPa respectively, the yield strength is 299MPa and 276MPa respectively, and the elongation after fracture is 33% and 39.5% respectively;
[0092] (5) The alloy component 1 after heat treatment was tested by scanning electron microscope with a magnification of 3000 times. The test results are as follows: Figure 4 As shown, from Figure 4 It can be seen that after heat treatment, the microstructure of alloy component 1 is highly uniform, without pores, cracks and slag inclusions.
[0093] Example 2
[0094] The same alloy powder 1 (4J36) as that in Example 1 is used to 3D print the alloy component 2 three-axis laser gyroscope housing by SLM technology, and the steps include:
[0095] (1) The three-dimensional design drawing of the three-axis laser gyroscope shell was imported into the SLM printing equipment, and the alloy powder 1 was placed in the powder cylinder of the SLM printer. The process parameters were set as follows: the scanning speed was 950 mm / s, the line spacing was 0.15 mm, the layer thickness was 30 μm, and the output power was 190 W. The alloy component 2 was printed. The linear expansion coefficients of the alloy component 2 in the horizontal and vertical directions at -60 to 100 °C were 0.53×10 -6 / ℃、0.67×10 -6 / ℃, the tensile strength of alloy component 2 in horizontal and vertical directions are 451MPa and 412MPa respectively, the yield strength is 367MPa and 336MPa respectively, and the elongation after fracture is 33.5% and 37% respectively;
[0096] (2) The alloy component 2 is heat treated, specifically including: keeping at 840°C for 1 hour, water quenching; keeping at 320°C for 1 hour, cooling with the furnace, and obtaining the heat-treated alloy component 2 three-axis laser gyroscope shell; the heat-treated alloy component 2 has a complex structure, light weight, high precision, no cracking and deformation; the linear expansion coefficients of the alloy component 2 in the horizontal direction and the vertical direction at -60 to 100°C are 0.88×10 -6 / ℃、1.0×10 -6 / ℃; after heat treatment, the tensile strength of alloy component 2 in horizontal and vertical directions are 450MPa and 411MPa respectively, the yield strength is 295MPa and 271MPa respectively, and the elongation after fracture is 33% and 38.5% respectively;
[0097] (3) The heat treated alloy component 2 was observed under a light microscope with a magnification of 500 times. The test results are as follows: Figure 5 As shown, from Figure 5 It can be seen that after heat treatment, the surface of the alloy component 2 is dense and has no fine pores and cracks.
[0098] Example 3
[0099] The same alloy powder 1 (4J36) as that in Example 1 is used to 3D print the alloy component 3 three-axis laser gyroscope housing by SLM technology, and the steps include:
[0100] (1) The three-dimensional design drawing of the three-axis laser gyroscope shell was imported into the SLM printing equipment, and the alloy powder 1 was placed in the powder cylinder of the SLM printer. The process parameters were set as follows: the scanning speed was 1100 mm / s, the line spacing was 0.18 mm, the layer thickness was 30 μm, and the output power was 220 W. The alloy component 3 was printed. The linear expansion coefficients of the alloy component 3 in the horizontal and vertical directions at -60 to 100 °C were 0.51×10 -6 / ℃、0.62×10 -6 / ℃, the tensile strength of alloy component 3 in horizontal and vertical directions are 453MPa and 414MPa respectively, the yield strength is 361MPa and 332MPa respectively, and the elongation after fracture is 34.5% and 37.5% respectively;
[0101] (2) The alloy component 3 is heat treated, specifically including: keeping at 840°C for 1 hour, water quenching; keeping at 320°C for 1 hour, cooling with the furnace, and obtaining the heat-treated alloy component 3 three-axis laser gyroscope shell; the heat-treated alloy component 3 has a complex structure, light weight, high precision, no cracking and deformation; the linear expansion coefficients of the alloy component 3 in the horizontal and vertical directions at -60 to 100°C are 0.85×10 -6 / ℃、0.99×10 -6 / ℃; after heat treatment, the tensile strengths of alloy component 3 in horizontal and vertical directions are 450MPa and 411MPa respectively, the yield strengths are 297MPa and 271MPa respectively, and the elongations after fracture are 33% and 37.5% respectively.
[0102] Comparative Example 1
[0103] The alloy component 4 three-axis laser gyroscope housing is prepared by using the same alloy powder 1 and method as in Example 1, except that:
[0104] In step (3), the scanning speed is set to 800 mm / s, and the laser power is set to 240 W, to obtain an alloy component 4, wherein the linear expansion coefficients of the alloy component 4 in the horizontal direction and the vertical direction at -60 to 100 ° C are 0.69×10 -6 / ℃、0.71×10 -6 / ℃, the tensile strength of alloy component 4 in horizontal and vertical directions are 437MPa and 403MPa respectively, the yield strength is 354MPa and 322MPa respectively, and the elongation after fracture is 32% and 36% respectively;
[0105] The linear expansion coefficients of the alloy component 4 obtained after heat treatment in the horizontal and vertical directions at -60 to 100 °C are 0.96×10 -6 / ℃、1.09×10 -6 / ℃; after heat treatment, the tensile strengths of the alloy component 4 in the horizontal and vertical directions were 425MPa and 393MPa, respectively, the yield strengths were 269MPa and 247MPa, respectively, and the elongations after fracture were 32% and 37%, respectively.
[0106] The heat treated alloy component 4 was observed under a light microscope with a magnification of 500 times. The test results are as follows: Figure 6 As shown, from Figure 6 It can be seen that there are small holes and micro cracks on the surface of alloy component 4.
[0107] Comparative Example 2
[0108] The alloy component 5 three-axis laser gyroscope housing is prepared by using the same alloy powder and method as in Example 1, except that:
[0109] In step (3), the scanning speed is set to 850 mm / s, and the laser power is set to 250 W, to obtain an alloy component 5, wherein the linear expansion coefficients of the alloy component 5 in the horizontal direction and the vertical direction at -60 to 100 ° C are 0.71×10 -6 / ℃、0.75×10 -6 / ℃, the tensile strength of alloy component 5 in horizontal and vertical directions are 428MPa and 397MPa respectively, the yield strength is 289MPa and 269MPa respectively, and the elongation after fracture is 32% and 36.5% respectively;
[0110] The linear expansion coefficients of the alloy component 5 obtained after heat treatment in the horizontal and vertical directions at -60 to 100 °C are 0.97×10 -6 / ℃、1.11×10 -6 / ℃; after heat treatment, the tensile strengths of alloy component 5 in horizontal and vertical directions are 421MPa and 389MPa respectively, the yield strengths are 268MPa and 236MPa respectively, and the elongations after fracture are 32.5% and 37% respectively.
[0111] Comparative Example 3
[0112] The alloy component 6 three-axis laser gyroscope housing is prepared by using the same alloy powder and method as in Example 1, except that:
[0113] In step (3), the scanning speed is set to 1200 mm / s, and the laser power is set to 260 W, to obtain the alloy component 6, wherein the linear expansion coefficients of the alloy component 6 in the horizontal direction and the vertical direction at -60 to 100 ° C are 0.71×10 -6 / ℃、0.75×10 -6 / ℃, the tensile strength of alloy component 6 in horizontal and vertical directions are 426MPa and 392MPa respectively, the yield strength is 285MPa and 263MPa respectively, and the elongation after fracture is 33% and 36% respectively;
[0114] The linear expansion coefficients of the alloy component 6 obtained after heat treatment in the horizontal and vertical directions at -60 to 100 °C are 0.98×10 -6 / ℃、1.12×10 -6 / ℃; after heat treatment, the tensile strength of alloy component 6 in horizontal and vertical directions are 423MPa and 379MPa respectively, the yield strength is 265MPa and 238MPa respectively, and the elongation after fracture is 32.5% and 37% respectively.
[0115] Comparative Example 4
[0116] (1) The alloy powder 1 same as that in Example 1 is used to manufacture the alloy component 7 by a conventional casting method;
[0117] (2) Through testing, the linear expansion coefficient of component 7 at 20-100°C is 0.85×10 -6 / ℃, tensile strength is 446MPa, yield strength is 265MPa, and elongation at break is 46%.
[0118] The preparation process cycle of Comparative Example 5 requires 2-3 weeks. Compared with Example 1, the process conditions are higher and the process cycle is longer.
[0119] Comparative Example 5
[0120] The alloy component 8 three-axis laser gyroscope housing is prepared by using the same alloy powder 1 and method as in Example 1, except that:
[0121] The heat treatment process parameters in step (4) are as follows: heating the alloy component 8 obtained in step (3) to 1000°C, keeping it at that temperature for 1 hour, water quenching, and then keeping it at 260°C for 1 hour, and cooling it in the furnace to obtain the alloy component 8 after heat treatment.
[0122] After heat treatment, the linear expansion coefficients of alloy component 8 in the horizontal and vertical directions at -60 to 100 °C are 1.08 × 10 -6 / ℃、1.25×10 -6 / ℃; after heat treatment, the tensile strength of alloy component 8 in horizontal and vertical directions are 395MPa and 370MPa respectively, the yield strength are 254MPa and 230MPa respectively, and the elongation after fracture are 30% and 33% respectively.
[0123] Comparative Example 6
[0124] The alloy component 9 of the three-axis laser gyroscope shell is prepared by using the same alloy powder 1 and method as in Example 1, except that the heat treatment process parameters in step (4) are used. Specifically, the alloy component 9 obtained in step (3) is heated to 840°C, kept warm for 1 hour, and cooled in the furnace to obtain the alloy component 9 after heat treatment.
[0125] After heat treatment, the linear expansion coefficients of the alloy component 9 in the horizontal and vertical directions at -60 to 100 °C are 0.91 × 10 -6 / ℃、1.08×10 -6 / ℃; after heat treatment, the tensile strength of alloy component 9 in horizontal and vertical directions are 443MPa and 397MPa respectively, the yield strength is 283MPa and 265MPa respectively, and the elongation after fracture is 32% and 37% respectively.
[0126] Comparative Example 7
[0127] The alloy component 10 of the three-axis laser gyroscope shell is prepared by using the same alloy powder 1 and method as in Example 1, except that the heat treatment process parameters in step (4) are used. Specifically, the alloy component 10 obtained in step (3) is heated to 320°C, kept warm for 1 hour, and air-cooled to obtain the alloy component 10 after heat treatment.
[0128] After heat treatment, the linear expansion coefficients of the alloy component 10 in the horizontal and vertical directions at -60 to 100 °C are 0.87×10 -6 / ℃、1.02×10 -6 / ℃; after heat treatment, the tensile strengths of the alloy component 10 in the horizontal and vertical directions are 442MPa and 410MPa, respectively, the yield strengths are 289MPa and 269MPa, respectively, and the elongations after fracture are 32.5% and 37%, respectively.
[0129] Comparative Example 8
[0130] An alloy component was prepared by the same method as in Example 1, except that the mass fractions of the main alloying elements in the alloy powder were: C: 0.015%, Mn: 0.39%, Si: 0.14%, P: 0.003%, S: 0.001%, Ni: 32.60%, and the rest was Fe, to obtain alloy component 11.
[0131] The linear expansion coefficients of alloy component 11 in the horizontal and vertical directions at -60 to 100 °C are 0.91×10 -6 / ℃、1.12×10 -6 / ℃; the tensile strengths of alloy component 11 in horizontal and vertical directions are 423MPa and 387MPa respectively, the yield strengths are 276MPa and 257MPa respectively, and the elongations after fracture are 32% and 36.5% respectively.
[0132] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A 3D printing method for a laser gyroscope housing, characterized in that: The method comprises: (1) Preparing laser gyroscope shell alloy powder; (2) importing the three-dimensional design drawing of the laser gyroscope shell into an SLM printing device, placing the alloy powder in a powder cylinder of the SLM printer, setting process parameters, and printing to obtain an alloy component; (3) The alloy member is subjected to heat treatment.
2. The method according to claim 1, characterized in that In terms of mass percentage, the composition of the alloy powder specifically includes: C: 0-0.05%, Mn: 0.2-0.6%, Si: 0-0.3%, P: 0-0.02%, S: 0-0.002%, Ni: 35-37%, and the rest is Fe.
3. The method according to claim 1, characterized in that The alloy powder has a particle size of 15-63 μm, a powder hollow rate of ≤1%, and an oxygen content of ≤200 ppm.
4. The method according to claim 1, characterized in that In step (1), the alloy powder is prepared by smelting + supersonic inert gas vacuum atomization method.
5. The method according to claim 4, characterized in that The smelting conditions are: vacuum degree <10 -2 Pa, the refining temperature is 1550-1650℃, and the time is 10-20min; the conditions of the supersonic inert gas vacuum atomization are: the insulation temperature is 1680±25℃, the insulation time is 15min, the leakage bag temperature is 1250±20℃, the leakage nozzle aperture is 4mm, the annular gap is 0.9mm, and the atomization pressure is 3-4MPa.
6. The method according to claim 1, characterized in that In step (2), the process parameters include: scanning speed of 950-1150 mm / s, line spacing of 0.12-0.18 mm, layer thickness of 30 μm, and output power of 190-220 W.
7. The method according to claim 1, characterized in that The heat treatment step comprises: heating the alloy component obtained in step (2) to 820-860° C., keeping the temperature for 1-2 hours, and water quenching; keeping the temperature at 305-325° C. for 1-2 hours, and cooling.
8. A laser gyro housing, characterized in that: The laser gyro housing is manufactured by the method described in any one of claims 1-7.
9. The laser gyro housing according to claim 8, characterized in that: The linear expansion coefficients of the gyro shell in the horizontal direction and the vertical direction at -60 to 100°C are ≤1×10 -6 / ℃,≤1×10 -6 / ℃; And / or, the tensile strength of the component in the horizontal and vertical directions is ≥450MPa and ≥410MPa respectively, the yield strength of the component in the horizontal and vertical directions is ≥290MPa and ≥270MPa respectively, and the elongation after fracture of the component in the horizontal and vertical directions is ≥33% and ≥37% respectively.
10. Application of a laser gyroscope housing in aerospace, navigation, military field, earth science research, industrial automation, and automatic driving, characterized in that: The laser gyro housing is manufactured by the method according to any one of claims 1 to 7.