High-rate and high-capacity hard carbon negative electrode material and preparation method and application thereof
By using inexpensive nitrogen-containing hard carbon precursor, zinc source and acid solution in the hard carbon anode material of sodium ion battery, the solvent-thermal reaction of the zinc source and acid solution, the active pore structure surrounding the micrographite domain is formed, and the medium and high capacity and high magnification of sodium ion battery are solved. The problem improves the performance stability and efficiency of the battery.
Patent Information
- Application Number
- CN202411019774.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The existing hard carbon anode materials for sodium ion batteries are difficult to take into account both high capacity and high magnification, and there are problems such as slow reaction kinetics and poor cycle stability.
The solvothermal reaction is carried out by using inexpensive nitrogen-containing hard carbon precursor, zinc source and acid solution. The active pore structure surrounding the micrograph domain is formed through two steps of pre-carbonization and carbonization, and doped nitrogen atoms are located to improve the storage kinetics of sodium ions.
It significantly improves the platform capacity and rate performance of the hard carbon anode of sodium ion batteries, improves the first Coulomb efficiency and cycle stability, and is suitable for large-scale production.
Smart Images

Figure BDA0004966867660000061 
Figure BDA0004966867660000071 
Figure BDA0004966867660000101
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery materials, and in particular to a hard carbon negative electrode material with high rate and high capacity, and a preparation method and application thereof. Background Art
[0002] Limited by the high cost and low lithium resource reserves, the large-scale energy storage development of lithium-ion batteries is restricted, and there is an urgent need to develop low-cost large-scale energy storage technology. Due to the abundant and low-cost sodium resources and the similar physical and chemical properties to lithium, sodium-ion batteries are one of the most promising alternatives to lithium-ion batteries. Existing sodium-ion battery materials generally have the problem of not being able to take into account both high capacity and high rate at the same time. During the first charge and discharge process, the electrolyte is prone to decompose at the surface of the open pore structure, which reduces the first coulombic efficiency. At present, the materials that have been successfully developed and applied to the negative electrode of sodium-ion batteries include carbon-based materials, alloys, organic materials, and titanium-based materials. Relatively speaking, hard carbon is considered to be the most commercially promising sodium-ion negative electrode material due to its excellent performance and low cost. The specific capacity of the most widely used commercial hard carbon can reach 300mAh / g. At present, the hard carbon materials for practical sodium-ion battery negative electrodes are divided into two capacity regions: "platform" and "slope" based on the adsorption, intercalation and pore-filling sodium storage mechanisms. The existing technology obtains high-capacity hard carbon materials by increasing the capacity of the platform region. Due to the large radius of sodium ions, the platform capacity of the hard carbon negative electrode materials reported so far has certain irreversibility, especially rapid decay under high-rate charge and discharge, poor cycle stability, and slow reaction kinetics, which seriously limits the application of hard carbon negative electrode materials in sodium ion batteries. Some existing technologies increase the capacity of the slope region with faster kinetics, but the high and constantly changing sodium storage voltage in the slope region makes it difficult to output this part of the capacity stably in the full battery, making it difficult to realize the practical application of sodium ion batteries. Summary of the invention
[0003] In order to overcome at least one technical problem existing in the above-mentioned prior art, one of the objectives of the present invention is to provide a method for preparing a hard carbon negative electrode material.
[0004] A second object of the present invention is to provide a hard carbon negative electrode material.
[0005] A third object of the present invention is to provide an electrode.
[0006] A fourth object of the present invention is to provide a sodium ion battery.
[0007] A fifth object of the present invention is to provide a method for preparing the above-mentioned hard carbon negative electrode material and / or the application of the hard carbon negative electrode material in the battery field.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is:
[0009] A first aspect of the present invention provides a method for preparing a hard carbon negative electrode material, comprising the following steps:
[0010] S1: firstly mixing a nitrogen-containing hard carbon precursor, a zinc source, and a solvent for reaction, and then mixing with an acid solution for reaction to obtain a mixture;
[0011] S2: removing the liquid from the mixture to obtain a solid product;
[0012] S3: pre-carbonizing the solid product and then carbonizing it to obtain the hard carbon negative electrode material.
[0013] The present invention uses a cheap nitrogen-containing hard carbon precursor, a zinc source, and an acid solution as raw materials for preparation, forms a carbon-nitrogen-zinc-anion group structure in a solvent thermal reaction process, first pre-carbonizes at a low temperature, and then carbonizes at a high temperature. In the step-by-step carbonization process, nitrogen atoms are positioned and doped around the hard carbon active pores to obtain a hard carbon negative electrode material with a large number of active pore structures with rapid sodium ion storage dynamics. Specifically, the active pores are surrounded by micro-graphite domains, and a layer of heteroatom nitrogen is distributed around the pores to accelerate the transmission dynamics of sodium ions in and out of the pores. The hard carbon negative electrode material with sodium storage active pores greatly improves the platform capacity of the hard carbon negative electrode of the sodium ion battery. During the mixing process, zinc ions can target the nitrogen-containing groups in the nitrogen-containing hard carbon precursor under the action of acid, and induce the formation of micro-graphite domains during the carbonization process, thereby forming active pores formed around the micro-graphite domains. Due to the targeting effect of zinc ions on nitrogen, heteroatom nitrogen is positioned and distributed around the active pores after carbonization, and the delocalized electrons derived from the heteroatom nitrogen can accelerate the transmission dynamics of sodium ions in and out of the pores, and the derived defect sites can simultaneously improve the defect adsorption capacity of sodium ions. Since the hard carbon material of the present invention has only a few surface open pore structures, this greatly reduces the decomposition of electrolyte solvent molecules on the surface, thereby improving the first coulombic efficiency and cycle stability of the negative electrode of the sodium ion battery.
[0014] Preferably, the nitrogen-containing hard carbon precursor is selected from a nitrogen-containing biomass hard carbon precursor, a nitrogen-containing synthetic polymer hard carbon precursor or a combination thereof; further preferably, the nitrogen-containing hard carbon precursor is a nitrogen-containing biomass hard carbon precursor. In the present invention, natural biomass materials are used as nitrogen-containing hard carbon precursors, and the raw material sources are wide and the cost is low.
[0015] Preferably, the nitrogen-containing biomass hard carbon precursor is selected from at least one of chitosan, bean dregs, coconut shell, walnut shell, pistachio shell, rape, wheat, sisal, peanut, seaweed, enoki mushroom, shiitake mushroom, mushroom, gelatin, silkworm cocoon, shrimp shell, crab shell, and shell; further preferably, the nitrogen-containing biomass hard carbon precursor is chitosan. In the present invention, the raw material of the nitrogen-containing hard carbon precursor can be biomass such as fruit shell, chitosan, lignin, etc., so it is low-cost and green and environmentally friendly.
[0016] Preferably, the nitrogen-containing synthetic polymer hard carbon precursor is selected from at least one of melamine, polyacrylonitrile, polyamide, polyurethane, polydimethylsilazane, polyaniline, polypyrrole, polypyrrolidone, polymethacrylamide, polyphthalamide, polyvinylcarbazole and polyethyleneimine.
[0017] Preferably, the zinc source is selected from zinc salts, hydrates of zinc salts or combinations thereof; the zinc salt is selected from at least one of zinc borate, zinc tartrate, zinc thiocyanate, zinc bromate, zinc chloride, zinc sulfate, zinc acetate, zinc nitrate, zinc nitrite, zinc carbonate, zinc phosphate, zinc phosphite, zinc thiosulfate and zinc citrate; further preferably, the zinc source is a zinc salt; more preferably, the zinc salt is selected from zinc acetate.
[0018] Preferably, the acid is selected from at least one of hydrochloric acid, sulfuric acid, nitric acid, acetic acid, phosphoric acid, hydrofluoric acid, oxalic acid, and nitrous acid; more preferably, the acid is selected from hydrochloric acid. In the present invention, the acid is used to activate the zinc source, and the addition of the acid can also adjust the pH of the mixture to promote the coupling of the zinc salt and the hard carbon precursor.
[0019] Preferably, the solvent is selected from at least one of toluene, chlorobenzene, dimethyl sulfoxide, water, methanol, ethanol, ether, acetone, chloroform, tetrahydrofuran, ethyl acetate, dichloromethane, and benzene; more preferably, the solvent is water; more preferably, the solvent is deionized water. Water is used as the solvent because the source of the solvent is wide, the cost is low, and it does not pollute the environment.
[0020] Preferably, based on the total volume percentage of the acid solution and the solvent as 100%, the volume percentage of the acid solution is 0.05-0.8%; further preferably, based on the total volume percentage of the acid solution and the solvent as 100%, the volume percentage of the acid solution is 0.1-0.4%; further preferably, based on the total volume percentage of the acid solution and the solvent as 100%, the volume percentage of the acid solution is 0.1-0.3%.
[0021] Preferably, based on the total mass percentage of the nitrogen-containing hard carbon precursor and the zinc source as 100%, the mass percentage of the zinc source is 5-75%; further preferably, based on the total mass percentage of the nitrogen-containing hard carbon precursor and the zinc source as 100%, the mass percentage of the zinc source is 20-40%; more preferably, based on the total mass percentage of the nitrogen-containing hard carbon precursor and the zinc source as 100%, the mass percentage of the zinc source is 25-35%.
[0022] Preferably, in the step S3, the pre-carbonization temperature is 200-800°C; further preferably, in the step S3, the pre-carbonization temperature is 500-800°C; more preferably, in the step S3, the pre-carbonization temperature is 600-800°C.
[0023] Preferably, the pre-carbonization time is 2 to 8 hours; further preferably, the pre-carbonization time is 4 to 7 hours; more preferably, the pre-carbonization time is 4 to 6 hours.
[0024] Preferably, the carbonization temperature is 1000-1800°C; further preferably, the carbonization temperature is 1100-1500°C; more preferably, the carbonization temperature is 1200-1400°C.
[0025] Preferably, the carbonization time is 1 to 6 hours; further preferably, the carbonization time is 1 to 4 hours; more preferably, the carbonization time is 1 to 3 hours.
[0026] The present invention adopts step-by-step carbonization. In the pre-carbonization process, the nitrogen-containing hard carbon precursor is initially carbonized at medium and low temperatures, acetate ions are decomposed at high temperatures, and zinc ions are assisted to induce micro-graphite domains to form abundant pores. Then, high temperature is used for carbonization, and the carbon layer structure, defects and pore structure are continuously optimized, thereby obtaining a hard carbon negative electrode material with a large number of sodium storage active pores.
[0027] Preferably, the heating rates in the pre-carbonization step and the carbonization step are independently selected from 3 to 8° C. / min.
[0028] Preferably, the pre-carbonization step and the carbonization step are both performed under the protection of an inert atmosphere.
[0029] Preferably, the inert gas is selected from nitrogen, argon or a combination thereof.
[0030] Preferably, the step S2 is: freeze-drying the mixture for 6 to 48 hours to remove the liquid (ie, the solvent and water) in the mixture to obtain a solid product.
[0031] Preferably, the step S2 comprises: heating and stirring the mixture, removing the liquid, and obtaining a solid product.
[0032] Preferably, the step S2 comprises: removing the liquid in the mixture by a rotary evaporator to obtain a solid product.
[0033] Preferably, the step S2 comprises: separating the mixture into solid and liquid, removing the liquid in the mixture, and obtaining a solid product.
[0034] Preferably, in the step S1, the nitrogen-containing hard carbon precursor, the zinc source and the solvent are first mixed and reacted at 15-85°C for 1-72 hours, and then mixed and reacted with acid solution at 15-85°C for 1-72 hours to obtain a mixture; further preferably, in the step S1, the nitrogen-containing hard carbon precursor, the zinc source and the solvent are first mixed and reacted at 15-45°C for 5-20 hours, and then mixed and reacted with acid solution at 50-85°C for 1-10 hours to obtain a mixture.
[0035] Preferably, in step S1, the mixing reaction step adopts any one of stirring mixing, wet ball milling, dry ball milling, freeze drying, and ultrasonic mixing.
[0036] The second aspect of the present invention provides a hard carbon negative electrode material, which is prepared by the preparation method described in the first aspect of the present invention.
[0037] When the hard carbon negative electrode material of the present invention is applied to a sodium ion battery, the sodium ion battery can have both high rate and high capacity.
[0038] The third aspect of the present invention provides an electrode, comprising the hard carbon negative electrode material described in the second aspect of the present invention.
[0039] The fourth aspect of the present invention provides a sodium ion battery, comprising the hard carbon negative electrode material described in the second aspect of the present invention, or the electrode described in the third aspect of the present invention.
[0040] Preferably, the sodium ion battery comprises a positive electrode, a negative electrode, a separator and an electrolyte; the negative electrode contains the hard carbon negative electrode material described in the second aspect of the present invention.
[0041] The sodium ion battery in the present invention adopts the hard carbon negative electrode material prepared by the preparation method described in the first aspect of the present invention. Since the hard carbon negative electrode platform area capacity has the advantages of fast kinetics, low and stable discharge voltage, a high energy density and high power density sodium ion battery can be realized.
[0042] The fifth aspect of the present invention provides a method for preparing the hard carbon negative electrode material according to the first aspect of the present invention and / or an application of the hard carbon negative electrode material according to the second aspect of the present invention in the field of batteries.
[0043] The beneficial effects of the present invention are as follows: the preparation method of the hard carbon negative electrode material of the present invention adopts low-cost and widely available nitrogen-containing hard carbon precursors, zinc sources, acid solutions and the like to prepare raw materials, firstly undergoes a solvent thermal reaction, and then the solid product obtained by the solvent thermal reaction undergoes a two-step carbonization process of pre-carbonization and carbonization. In the two-step carbonization process, some components in the solid product are decomposed or released to form a large number of active sodium storage pores, and the nitrogen atoms in the nitrogen-containing hard carbon precursor are positioned and doped around the active sodium storage pores, which can accelerate the transport kinetics of sodium ions in and out of the pores, thereby obtaining a hard carbon negative electrode material with both high rate and high capacity. The preparation method is simple, pollution-free, green and environmentally friendly, low-cost, and suitable for large-scale production.
[0044] The sodium ion battery of the present invention adopts the hard carbon negative electrode material prepared by the above-mentioned preparation method. The hard carbon negative electrode material has abundant localized nitrogen-doped active pores, which can make the sodium ion battery have high specific capacity, high rate, high first charge and discharge efficiency, good cycle stability, and still have a high capacity retention rate at high current density. Since the hard carbon negative electrode material has only a few surface open pore structures, this greatly reduces the decomposition of electrolyte solvent molecules on the surface of the hard carbon negative electrode material, while improving the first coulomb efficiency and cycle stability of the hard carbon negative electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 Schematic diagram of the structure of active pores of the hard carbon negative electrode material in an embodiment of the present invention.
[0046] Figure 2 This is the SEM image of the hard carbon negative electrode material in Example 1.
[0047] Figure 3 These are the XRD test diagrams of the hard carbon negative electrode materials in Example 1 and Comparative Example 1.
[0048] Figure 4 These are Raman test graphs of the hard carbon negative electrode materials in Example 1 and Comparative Example 1.
[0049] Figure 5 This is the WAXS curve diagram of the hard carbon negative electrode material in Example 1.
[0050] Figure 6 This is a pore size distribution curve of the hard carbon negative electrode material in Example 1.
[0051] Figure 7 This is a constant current charge and discharge curve of the sodium ion half-cell assembled from the hard carbon negative electrode material in Example 1 at 0.1C.
[0052] Figure 8 This is a long cycle curve of the sodium ion half-cell assembled with the hard carbon negative electrode material in Example 1 at 0.1C.
[0053] Fig. 9 This is a rate performance test diagram of the sodium ion half-cell assembled from the hard carbon negative electrode material in Example 1. DETAILED DESCRIPTION
[0054] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. The reagents or instruments used that do not indicate the manufacturer are all conventional products that can be purchased commercially.
[0055] The present invention uses cheap hard carbon precursors and zinc salts as raw materials, and obtains hard carbon with abundant sodium storage active pores after step-by-step carbonization, and realizes the localized nitrogen doping of the active pores, thereby improving the storage kinetics of sodium ions. The platform capacity of the hard carbon negative electrode material of the sodium ion battery is greatly improved based on the derived sodium storage active pores. During the mixing process of the hard carbon precursor and the zinc salt, the zinc ions can target the nitrogen-containing groups under the action of the acid, and induce the formation of micro-graphite domains during the carbonization process, thereby forming active pores surrounded by the micro-graphite domains, as shown in the following figure. Figure 1 As shown, due to the targeting effect of zinc ions on nitrogen, heteroatom nitrogen is positioned and distributed around the active pores after carbonization, and the delocalized electrons derived from the heteroatom nitrogen can accelerate the transport kinetics of sodium ions in and out of the pores, and the derived defect sites can simultaneously increase the defect adsorption capacity of sodium ions. Since the hard carbon negative electrode material in the present invention has only a few surface open pore structures, this greatly reduces the decomposition of electrolyte solvent molecules on its surface, and improves the first coulombic efficiency and cycle stability of the hard carbon negative electrode material for sodium ion batteries.
[0056] The present invention is further described below by means of specific examples and comparative examples. However, it should be understood that these examples are only used for more detailed description and should not be construed as limiting the present invention in any form.
[0057] Example 1
[0058] This example provides a method for preparing a hard carbon negative electrode material for a sodium ion battery, and the specific steps are as follows:
[0059] Disperse 1.6g of hard carbon material precursor chitosan in deionized water, gradually add 0.8g (the total mass percentage of the hard carbon material precursor and zinc acetate is 100%, and the mass percentage of zinc acetate is 30%) zinc acetate, and continue stirring at 25°C for 12 hours. Add 200μL (the volume percentage of dilute hydrochloric acid is 0.2%, based on the total volume percentage of deionized water and dilute hydrochloric acid is 100%) dilute HCl dropwise, and continue stirring in a water bath at 70°C for 2h. Freeze-dry the obtained paste intermediate for 48h. Place the dried intermediate in a tubular furnace, and in a high-purity argon protective atmosphere, first raise the temperature to 700°C at a heating rate of 5°C / min for pre-carbonization for 5h, and then raise the temperature to 1300°C at a heating rate of 5°C / min for carbonization for 2h to obtain the sodium ion battery hard carbon negative electrode material in this example.
[0060] The raw materials and process parameters for preparing the hard carbon negative electrode material for the sodium ion battery in this example are shown in Table 1 below.
[0061] Table 1 Preparation raw materials and preparation process parameters
[0062]
[0063] Comparative Example 1
[0064] This example provides a method for preparing a hard carbon negative electrode material for a sodium ion battery, and the specific steps are as follows:
[0065] 1.6 g of hard carbon material precursor chitosan was placed in a tubular furnace. Under a high-purity argon protective atmosphere, the temperature was first raised to 700°C at a heating rate of 5°C / min for pre-carbonization for 5 hours, and then the temperature was raised to 1300°C at a heating rate of 5°C / min for carbonization for 2 hours to obtain the sodium ion battery hard carbon negative electrode material in this example.
[0066] The surface morphology of the hard carbon negative electrode material prepared in Example 1 was tested using a scanning electron microscope. The specific test results are as follows: Figure 2 As shown, Figure 2 (a) Figure 2 (b) and Figure 2 (c) SEM images of the hard carbon negative electrode material prepared in Example 1 with scales of 100 μm, 30 μm and 20 μm respectively. Figure 2 It can be seen that the hard carbon negative electrode material prepared in Example 1 has a uniform microscopic morphology and a uniform flaky structure. The hard carbon negative electrode material has abundant active pores, which are surrounded by micrographite domains, and a layer of heteroatom nitrogen is gathered and distributed around the pores, which are active sodium storage pores with localized nitrogen doping.
[0067] The XRD curves of the hard carbon negative electrode materials prepared in Example 1 and Comparative Example 1 were tested by X-ray diffractometer. The specific test results are as follows: Figure 3 As shown by Figure 3 It can be seen that compared with Comparative Example 1, the XRD curve of the hard carbon negative electrode material prepared in Example 1 shows that the (002) peak near 24° and the (100) peak near 44° are broadened, indicating that the order of the carbon layer of the hard carbon negative electrode material prepared in Example 1 is increased.
[0068] The Raman curves of the hard carbon negative electrode materials prepared in Example 1 and Comparative Example 1 were tested respectively. The specific test results are as follows: Figure 4 As shown by Figure 4 It can be seen that the Raman peak of the hard carbon negative electrode material in Example 1 shows a larger ID / IG value, indicating that the defects and pore structure of the hard carbon negative electrode material prepared in Example 1 are richer, and the hard carbon negative electrode material obtained after high-temperature calcination has abundant active sodium storage pores and fewer open pore structures, that is, fewer invalid pores.
[0069] The WAXS curve of the hard carbon negative electrode material prepared in Example 1 was tested by wide angle X-ray scattering (WAXS). The specific test results are as follows: Figure 5 shown. Figure 5 The WAXS curve in the scattering intensity Q is 1~8nm -1 There is an obvious peak package at the point, indicating that the hard carbon negative electrode material of Example 1 has rich active sodium storage pore structure.
[0070] The pore size distribution curve of the hard carbon negative electrode material prepared in Example 1 was tested by the BET specific surface area test method. The specific test results are as follows: Figure 6 As shown by Figure 6 It can be seen that the specific surface area of the hard carbon negative electrode material of Example 1 is only 10 to 30 m 2 / g, and the pores are mainly nanoscale, indicating that the prepared hard carbon negative electrode material has very few invalid pores.
[0071] The hard carbon negative electrode material prepared in Example 1 and Comparative Example 1 was mixed with polyvinylidene fluoride (PVDF) binder and conductive carbon black (SP conductive agent) in a mass ratio of 8:1:1, ground for 30 minutes, added with methyl pyrrolidone (NMP) and stirred until it was in a paste state, and coated on aluminum foil to prepare an electrode. A sodium sheet was used as a counter electrode, and a 1 mol / L NaClO4 electrolyte (the solvent was a mixture of EC and DMC in a volume ratio of 1:1) was used to assemble a sodium half-cell, and charge and discharge tests were performed at different rates, and a long cycle test was performed at 0.1C. The specific test results are shown in FIG. Figures 7 to 9 And as shown in Table 2.
[0072] Table 2 Electrochemical performance test results of hard carbon negative electrode materials
[0073]
[0074] As can be seen from Table 2, compared with Comparative Example 1, the hard carbon negative electrode material prepared in Example 1 has better electrochemical performance, and the specific capacity when cycled at 0.1C and 5C rates has been significantly improved. The reason is that: Example 1 uses chitosan as a nitrogen-containing hard carbon precursor. After adding dilute hydrochloric acid to the chitosan aqueous solution, the amino groups in the chitosan are activated. Under the action of the lone electron pair of the nitrogen atom, the zinc ions can be adsorbed around the amino group to achieve nitrogen targeting. Under the electrostatic adsorption of zinc ions, the acetate ions move closer to the group to form a carbon-nitrogen-zinc-acetate structure. During the carbonization process, zinc ions and acetate ions synergistically induce the formation of active pores surrounded by micro-graphite domains. After the amino groups are carbonized, they are derived into heteroatom nitrogen around the pores, thereby achieving localized nitrogen doping. It is worth noting that due to the low boiling point of zinc, the carbonized hard carbon negative electrode material does not contain zinc. Under the action of this active pore with localized nitrogen doping, the platform capacity of the hard carbon negative electrode material is greatly improved, and the platform capacity has excellent rate performance.
[0075] Depend on Figure 8 It can be seen that the sodium ion half-cell assembled with the hard carbon negative electrode material in Example 1 has a specific capacity of 380 mAh / g when cycled 2600 times at a rate of 0.1C, and the capacity retention rate is 76.92%.
[0076] Depend on Fig. 9 It can be seen that the first coulombic efficiency of the sodium ion half-cell assembled with the hard carbon negative electrode material in Example 1 reaches 91.5%, the specific capacity reaches 494 mAh / g, and the capacity retention rate reaches 80% after the charge and discharge rate is increased from 0.1C to 5C. After it is reduced to 0.1C again, the capacity recovers to 453 mAh / g, and the rate performance is significantly improved.
[0077] Example 2
[0078] The preparation method of the hard carbon negative electrode material for sodium ion batteries in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by dregs of the same mass in this example.
[0079] Example 3
[0080] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by coconut shell of the same mass.
[0081] Example 4
[0082] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by walnut shells of the same mass.
[0083] Example 5
[0084] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by pistachio shells of the same mass.
[0085] Example 6
[0086] The preparation method of the hard carbon negative electrode material for sodium ion batteries in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by rapeseed of the same mass in this example.
[0087] Example 7
[0088] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by wheat of the same mass in this example.
[0089] Example 8
[0090] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by peanuts of the same mass.
[0091] Example 9
[0092] The preparation method of the hard carbon negative electrode material for sodium ion batteries in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by seaweed of the same mass.
[0093] Example 10
[0094] The preparation method of the hard carbon negative electrode material for sodium ion batteries in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by the same mass of Flammulina velutipes.
[0095] Embodiment 11
[0096] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by shiitake mushrooms of the same mass.
[0097] Example 12
[0098] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by mushrooms of the same mass.
[0099] Embodiment 13
[0100] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by gelatin of the same mass in this example.
[0101] Embodiment 14
[0102] The preparation method of the hard carbon negative electrode material for sodium ion batteries in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by silkworm cocoons of the same mass.
[0103] Embodiment 15
[0104] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by melamine of the same mass in this example.
[0105] Example 16
[0106] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by polyacrylonitrile of the same mass in this example.
[0107] Embodiment 17
[0108] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by polyamide of the same mass in this example.
[0109] Embodiment 18
[0110] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by polyurethane of the same mass in this example.
[0111] Embodiment 19
[0112] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by polydimethylsilazane of the same mass.
[0113] Embodiment 20
[0114] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by polyaniline of the same mass in this example.
[0115] Embodiment 21
[0116] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by polypyrrole of the same mass in this example.
[0117] Embodiment 22
[0118] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the chitosan in Example 1 is replaced by polyethyleneimine of the same mass in this example.
[0119] The hard carbon negative electrode materials prepared in Examples 1 to 22 were mixed with polyvinylidene fluoride (PVDF) binder and conductive carbon black (SP conductive agent) in a mass ratio of 8:1:1, ground for 30 minutes, added with methyl pyrrolidone (NMP) and stirred until paste-like, and coated on aluminum foil to prepare electrodes. Sodium sheets were used as counter electrodes, and 1 mol / L NaClO4 electrolyte (the solvent was a mixture of EC and DMC in a volume ratio of 1:1) was used to assemble a sodium half-cell, and charge and discharge tests were performed at different rates, and long cycle tests were performed at 0.1C. The specific test results are shown in Table 3 below.
[0120] Table 3 Electrochemical performance test results of the hard carbon negative electrode materials prepared in Examples 1 to 22
[0121]
[0122]
[0123] It can be seen from Table 3 that there are certain differences in the microstructure and battery cycle performance of hard carbon negative electrode materials prepared from different hard carbon material precursors. Compared with other hard carbon material precursors, the hard carbon negative electrode material prepared from chitosan as a hard carbon material precursor has better performance.
[0124] Embodiment 23
[0125] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the same amount of sulfuric acid is used in this example instead of the hydrochloric acid in Example 1.
[0126] Embodiment 24
[0127] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the same amount of nitric acid is used in this example instead of the hydrochloric acid in Example 1.
[0128] Embodiment 25
[0129] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the same amount of acetic acid is used in this example instead of the hydrochloric acid in Example 1.
[0130] Embodiment 26
[0131] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the same amount of phosphoric acid is used in this example instead of the hydrochloric acid in Example 1.
[0132] The hard carbon negative electrode materials prepared in Examples 23 to 26 were mixed with polyvinylidene fluoride (PVDF) binder and conductive carbon black (SP conductive agent) in a mass ratio of 8:1:1, ground for 30 minutes, added with methyl pyrrolidone (NMP) and stirred until paste-like, and coated on aluminum foil to prepare electrodes. Sodium sheets were used as counter electrodes, and 1 mol / L NaClO4 electrolyte (the solvent was a mixture of EC and DMC in a volume ratio of 1:1) was used to assemble a sodium half-cell, and charge and discharge tests were performed at different rates, and long cycle tests were performed at 0.1C. The specific test results are shown in Table 4 below.
[0133] Table 4 Electrochemical performance test results of the hard carbon negative electrode materials prepared in Examples 23 to 26
[0134]
[0135] It can be seen from Table 4 that compared with other acidic solutions, the performance of the hard carbon negative electrode material prepared using hydrochloric acid is better.
[0136] Embodiment 27
[0137] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the same amount of zinc chloride is used in this example instead of the zinc acetate in Example 1.
[0138] Embodiment 28
[0139] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the same amount of zinc carbonate is used in this example instead of the zinc acetate in Example 1.
[0140] Embodiment 29
[0141] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the same amount of zinc sulfate is used in this example instead of the zinc acetate in Example 1.
[0142] Embodiment 30
[0143] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the zinc acetate in Example 1 is replaced by the same amount of zinc phosphate in this example.
[0144] Embodiment 31
[0145] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the same amount of zinc phosphite is used in this example instead of the zinc acetate in Example 1.
[0146] Embodiment 32
[0147] The preparation method of the hard carbon negative electrode material for sodium ion batteries in this example is different from that in Example 1 only in that the same amount of zinc nitrate is used in this example instead of the zinc acetate in Example 1.
[0148] Embodiment 33
[0149] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the same amount of zinc thiosulfate is used in this example instead of the zinc acetate in Example 1.
[0150] Embodiment 34
[0151] The preparation method of the hard carbon negative electrode material for sodium ion batteries in this example is different from that in Example 1 only in that the same amount of zinc nitrite is used in this example instead of the zinc acetate in Example 1.
[0152] Embodiment 35
[0153] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the same amount of zinc citrate is used in this example instead of the zinc acetate in Example 1.
[0154] The hard carbon negative electrode materials prepared in Examples 27 to 35 were mixed with polyvinylidene fluoride (PVDF) binder and conductive carbon black (SP conductive agent) at a mass ratio of 8:1:1, ground for 30 minutes, added with methyl pyrrolidone (NMP) and stirred until paste-like, and coated on aluminum foil to prepare electrodes. Sodium sheets were used as counter electrodes, and 1 mol / L NaClO4 electrolyte (the solvent was a mixture of EC and DMC in a volume ratio of 1:1) was used to assemble a sodium half-cell, and charge and discharge tests were performed at different rates, and long cycle tests were performed at 0.1C. The specific test results are shown in Table 5 below.
[0155] Table 5 Electrochemical performance test results of the hard carbon negative electrode materials prepared in Examples 27 to 35
[0156]
[0157] It can be seen from Table 5 that compared with other zinc salts, the hard carbon negative electrode material prepared using zinc acetate as raw material has better performance. The reason may be that zinc acetate has a stronger ability to transform invalid pores into effective active pores with high sodium ion transport kinetics when performing targeted doping on the hard carbon material precursor.
[0158] Embodiment 36
[0159] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the mass percentage of zinc acetate in this example is 5%.
[0160] Embodiment 37
[0161] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the mass percentage of zinc acetate in this example is 20%.
[0162] Embodiment 38
[0163] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the mass percentage of zinc acetate in this example is 25%.
[0164] Embodiment 39
[0165] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the mass percentage of zinc acetate in this example is 35%.
[0166] Embodiment 40
[0167] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the mass percentage of zinc acetate in this example is 40%.
[0168] Embodiment 41
[0169] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the mass percentage of zinc acetate in this example is 55%.
[0170] Embodiment 42
[0171] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the mass percentage of zinc acetate in this example is 70%.
[0172] The hard carbon negative electrode materials prepared in Examples 36 to 42 were mixed with polyvinylidene fluoride (PVDF) binder and conductive carbon black (SP conductive agent) at a mass ratio of 8:1:1, ground for 30 minutes, added with methyl pyrrolidone (NMP) and stirred until paste-like, and coated on aluminum foil to prepare electrodes. Sodium sheets were used as counter electrodes, and 1 mol / L NaClO4 electrolyte (the solvent was a mixture of EC and DMC in a volume ratio of 1:1) was used to assemble a sodium half-cell, and charge and discharge tests were performed at different rates, and long cycle tests were performed at 0.1C. The specific test results are shown in Table 6 below.
[0173] Table 6 Electrochemical performance test results of the hard carbon negative electrode materials prepared in Examples 36 to 42
[0174]
[0175]
[0176] It can be seen from Table 6 that with the increase of the mass percentage of zinc acetate, the electrochemical performance of the prepared hard carbon negative electrode material first increases and then decreases. When the mass percentage of zinc acetate is about 25-35%, especially 30%, the performance of the prepared hard carbon negative electrode material is better.
[0177] Embodiment 43
[0178] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that ethanol is used in this example instead of the deionized water in Example 1.
[0179] Embodiment 44
[0180] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that acetone is used in this example instead of the deionized water in Example 1.
[0181] Embodiment 45
[0182] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that benzene is used in this example instead of the deionized water in Example 1.
[0183] Embodiment 46
[0184] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that toluene is used in this example instead of the deionized water in Example 1.
[0185] Embodiment 47
[0186] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that chlorobenzene is used in this example instead of the deionized water in Example 1.
[0187] Embodiment 48
[0188] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that styrene is used in this example instead of the deionized water in Example 1.
[0189] Embodiment 49
[0190] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that methanol is used in this example instead of the deionized water in Example 1.
[0191] Embodiment 50
[0192] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that ether is used in this example instead of the deionized water in Example 1.
[0193] Embodiment 51
[0194] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that tetrahydrofuran is used in this example instead of the deionized water in Example 1.
[0195] The hard carbon negative electrode materials prepared in Examples 43 to 51 were mixed with PVDF binder and SP conductive agent at a mass ratio of 8:1:1, ground for 30 minutes, added with NMP and stirred until paste-like, and coated on aluminum foil to prepare electrodes. Sodium sheet was used as the counter electrode, and 1 mol / L NaClO4 electrolyte (the solvent was a mixture of EC and DMC in a volume ratio of 1:1) was used to assemble a sodium half-cell, and charge and discharge tests were performed at different rates, and long cycle tests were performed at 0.1C. The specific test results are shown in Table 7 below.
[0196] Table 7 Electrochemical performance test results of the hard carbon negative electrode materials prepared in Examples 43 to 51
[0197]
[0198] It can be seen from Table 7 that compared with other solvents, using deionized water as the solvent in conjunction with the freeze-drying treatment step makes the doping more uniform, and the first coulombic efficiency and specific capacity of the hard carbon negative electrode material obtained are improved overall.
[0199] Embodiment 52
[0200] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 300° C. and the pre-carbonization time is 3 h.
[0201] Embodiment 53
[0202] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 300° C. and the pre-carbonization time is 4 h.
[0203] Embodiment 54
[0204] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 300° C. and the pre-carbonization time is 5 h.
[0205] Embodiment 55
[0206] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 300° C. and the pre-carbonization time is 6 h.
[0207] Embodiment 56
[0208] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 300° C. and the pre-carbonization time is 7 h.
[0209] Embodiment 57
[0210] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 300° C. and the pre-carbonization time is 8 h.
[0211] Embodiment 58
[0212] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 400° C. and the pre-carbonization time is 3 h.
[0213] Embodiment 59
[0214] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 400° C. and the pre-carbonization time is 4 hours.
[0215] Embodiment 60
[0216] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 400° C. and the pre-carbonization time is 5 h.
[0217] Embodiment 61
[0218] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 400° C. and the pre-carbonization time is 6 h.
[0219] Embodiment 62
[0220] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 400° C. and the pre-carbonization time is 7 h.
[0221] Embodiment 63
[0222] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 400° C. and the pre-carbonization time is 8 h.
[0223] Embodiment 64
[0224] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 500° C. and the pre-carbonization time is 3 h.
[0225] Embodiment 65
[0226] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 500° C. and the pre-carbonization time is 4 h.
[0227] Embodiment 66
[0228] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 500° C. and the pre-carbonization time is 5 h.
[0229] Embodiment 67
[0230] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 500° C. and the pre-carbonization time is 6 h.
[0231] Embodiment 68
[0232] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 500° C. and the pre-carbonization time is 7 h.
[0233] Embodiment 69
[0234] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 500° C. and the pre-carbonization time is 8 h.
[0235] Embodiment 70
[0236] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 600° C. and the pre-carbonization time is 3 h.
[0237] Embodiment 71
[0238] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 600° C. and the pre-carbonization time is 4 hours.
[0239] Embodiment 72
[0240] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 600° C. and the pre-carbonization time is 5 h.
[0241] Embodiment 73
[0242] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 600° C. and the pre-carbonization time is 6 h.
[0243] Embodiment 74
[0244] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 600° C. and the pre-carbonization time is 7 hours.
[0245] Embodiment 75
[0246] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 600° C. and the pre-carbonization time is 8 h.
[0247] Embodiment 76
[0248] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 700° C. and the pre-carbonization time is 3 h.
[0249] Embodiment 77
[0250] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 700° C. and the pre-carbonization time is 4 hours.
[0251] Embodiment 78
[0252] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 700° C. and the pre-carbonization time is 6 h.
[0253] Embodiment 79
[0254] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 700° C. and the pre-carbonization time is 7 h.
[0255] Embodiment 80
[0256] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 700° C. and the pre-carbonization time is 8 h.
[0257] Embodiment 81
[0258] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 800° C. and the pre-carbonization time is 3 h.
[0259] Embodiment 82
[0260] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 800° C. and the pre-carbonization time is 4 h.
[0261] Embodiment 83
[0262] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 800° C. and the pre-carbonization time is 5 h.
[0263] Embodiment 84
[0264] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 800° C. and the pre-carbonization time is 6 h.
[0265] Embodiment 85
[0266] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 800° C. and the pre-carbonization time is 7 h.
[0267] Embodiment 86
[0268] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the pre-carbonization temperature in this example is 800° C. and the pre-carbonization time is 8 hours.
[0269] The hard carbon negative electrode materials prepared in Examples 52 to 86 were mixed with PVDF binder and SP conductive agent at a mass ratio of 8:1:1, ground for 30 minutes, added with NMP and stirred until paste-like, and coated on aluminum foil to prepare electrodes. Sodium sheet was used as the counter electrode, and 1 mol / L NaClO4 electrolyte (the solvent was a mixture of EC and DMC in a volume ratio of 1:1) was used to assemble a sodium half-cell, and charge and discharge tests were performed at different rates, and long cycle tests were performed at 0.1C. The specific test results are shown in Table 8 below.
[0270] Table 8 Electrochemical performance test results of the hard carbon negative electrode materials prepared in Examples 52 to 86
[0271]
[0272]
[0273] Depend on Figure 8 It can be seen that the pre-carbonization temperature and time parameters have a great influence on the performance of the prepared hard carbon negative electrode material. The performance of the hard carbon negative electrode material prepared by pre-carbonization at around 700°C for about 5 hours is better.
[0274] Embodiment 87
[0275] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1100° C. and the carbonization time is 1 h.
[0276] Embodiment 88
[0277] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1100° C. and the carbonization time is 2 h.
[0278] Embodiment 89
[0279] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1100° C. and the carbonization time is 3 h.
[0280] Embodiment 90
[0281] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1100° C. and the carbonization time is 4 hours.
[0282] Embodiment 91
[0283] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1200° C. and the carbonization time is 1 h.
[0284] Embodiment 92
[0285] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1200° C. and the carbonization time is 2 h.
[0286] Embodiment 93
[0287] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1200° C. and the carbonization time is 3 h.
[0288] Embodiment 94
[0289] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1200° C. and the carbonization time is 4 hours.
[0290] Embodiment 95
[0291] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1300° C. and the carbonization time is 1 h.
[0292] Embodiment 96
[0293] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1300° C. and the carbonization time is 3 h.
[0294] Embodiment 97
[0295] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1300° C. and the carbonization time is 4 hours.
[0296] Embodiment 98
[0297] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1400° C. and the carbonization time is 1 hour.
[0298] Embodiment 99
[0299] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1400° C. and the carbonization time is 2 h.
[0300] Embodiment 100
[0301] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1400° C. and the carbonization time is 3 h.
[0302] Embodiment 101
[0303] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1400° C. and the carbonization time is 4 hours.
[0304] Embodiment 102
[0305] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1500° C. and the carbonization time is 1 h.
[0306] Embodiment 103
[0307] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1500° C. and the carbonization time is 2 h.
[0308] Embodiment 104
[0309] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1500° C. and the carbonization time is 3 h.
[0310] Embodiment 105
[0311] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1500° C. and the carbonization time is 4 hours.
[0312] Embodiment 106
[0313] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1700° C. and the carbonization time is 1 h.
[0314] Embodiment 107
[0315] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1700° C. and the carbonization time is 2 h.
[0316] Embodiment 108
[0317] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1700° C. and the carbonization time is 3 h.
[0318] Embodiment 109
[0319] The preparation method of the sodium ion battery hard carbon negative electrode material in this example is different from that in Example 1 only in that the carbonization temperature in this example is 1700° C. and the carbonization time is 4 hours.
[0320] The hard carbon negative electrode materials prepared in Examples 87 to 109 were mixed with PVDF binder and SP conductive agent at a mass ratio of 8:1:1, ground for 30 minutes, added with NMP and stirred until paste-like, and coated on aluminum foil to prepare electrodes. Sodium sheets were used as counter electrodes, and 1 mol / L NaClO4 electrolyte (the solvent was a mixture of EC and DMC in a volume ratio of 1:1) was used to assemble a sodium half-cell, and charge and discharge tests were performed at different rates, and long cycle tests were performed at 0.1C. The specific test results are shown in Table 9 below.
[0321] Table 9 Electrochemical performance test results of the hard carbon negative electrode materials prepared in Examples 87 to 109
[0322]
[0323]
[0324] As can be seen from Table 9, the carbonization temperature and carbonization time parameters have a great influence on the performance of the prepared hard carbon negative electrode material. The main reason is that the appropriate carbonization temperature and carbonization time can optimize the carbon layer structure, defects and partial pore structure, thereby improving the specific capacity and first coulombic efficiency of the prepared hard carbon negative electrode material. By comparing Examples 87 to 109, it can be seen that the performance of the hard carbon negative electrode material obtained by carbonizing at about 1300°C for about 2 hours is better.
[0325] In summary, the present invention is to fully mix the hard carbon precursor and the zinc salt, add an acidic solution to couple and solidify the zinc salt and the hard carbon precursor, and obtain an intermediate product after drying. The intermediate product is placed in an inert atmosphere for step-by-step carbonization. During the carbonization process, the nitrogen atoms in the hard carbon precursor are positioned and doped around the active pores of the hard carbon material to obtain an active pore structure with fast sodium ion storage kinetics. The hard carbon negative electrode material prepared in the present invention has high capacity, high rate, high first coulomb efficiency and stable cycle. Among them, the first coulomb efficiency of the sodium ion half-cell assembled with the hard carbon negative electrode material in Example 1 reaches 91.5%, and the specific capacity reaches 494mAh / g. After the charge and discharge rate is increased from 0.1C to 5C, the capacity retention rate reaches 80%, and the capacity is restored to 453mAh / g after it is reduced to 0.1C again, and the rate performance is significantly improved. The preparation process of the hard carbon negative electrode material in the present invention is simple, the raw material source is wide and cheap, it is pollution-free to the environment, does not require large-scale equipment, is suitable for large-scale production, conforms to my country's sustainable development strategy, and can be widely used in the field of energy storage.
[0326] During the discharge process of the sodium half-cell, the hard carbon negative electrode material in the present invention positions and distributes heteroatomic nitrogen around the active pores after carbonization due to the nitrogen targeting effect of zinc ions. The delocalized electrons derived from the heteroatomic nitrogen can accelerate the transport dynamics of sodium ions in and out of the pores, and the derived defect sites can simultaneously increase the defect adsorption capacity of sodium ions, thereby improving the rate performance and capacity of the sodium ion battery. After the active pores are formed, the solvated ion groups dissolve on the surface of the active pores, which greatly reduces the decomposition of the electrolyte solvent molecules and the occurrence of side reactions, and improves the first coulombic efficiency and cycle stability of the sodium ion battery. The sodium half-cell prepared using the hard carbon negative electrode material in the present invention has high capacity, high rate, high first coulombic efficiency, high first charge and discharge efficiency, and good cycle stability.
[0327] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A method for preparing a hard carbon negative electrode material, Features: The following steps are involved: S1: firstly mixing a nitrogen-containing hard carbon precursor, a zinc source, and a solvent for reaction, and then mixing with an acid solution for reaction to obtain a mixture; S2: removing the liquid from the mixture to obtain a solid product; S3: pre-carbonizing the solid product and then carbonizing it to obtain the hard carbon negative electrode material.
2. The method for preparing the hard carbon negative electrode material according to claim 1, Features: The nitrogen-containing hard carbon precursor is selected from a nitrogen-containing biomass hard carbon precursor, a nitrogen-containing synthetic polymer hard carbon precursor or a combination thereof.
3. The method for preparing the hard carbon negative electrode material according to claim 2, Features: The nitrogen-containing biomass hard carbon precursor is selected from at least one of chitosan, bean dregs, coconut shells, walnut shells, pistachio shells, rapeseed, wheat, sisal, peanuts, seaweed, enoki mushrooms, shiitake mushrooms, mushrooms, gelatin, silkworm cocoons, shrimp shells, crab shells, and shells; And / or, the nitrogen-containing synthetic polymer hard carbon precursor is selected from at least one of melamine, polyacrylonitrile, polyamide, polyurethane, polydimethylsilazane, polyaniline, polypyrrole, polypyrrolidone, polymethacrylamide, polyphthalamide, polyvinyl carbazole and polyethyleneimine.
4. The method for preparing the hard carbon negative electrode material according to claim 1, Features: The zinc source is selected from zinc salts, hydrates of zinc salts or combinations thereof; the zinc salt is selected from at least one of zinc borate, zinc tartrate, zinc thiocyanate, zinc bromate, zinc chloride, zinc sulfate, zinc acetate, zinc nitrate, zinc nitrite, zinc carbonate, zinc phosphate, zinc phosphite, zinc thiosulfate and zinc citrate; And / or, the acid solution is selected from at least one of hydrochloric acid, sulfuric acid, nitric acid, acetic acid, phosphoric acid, hydrofluoric acid, oxalic acid, and nitrous acid; And / or, the solvent is selected from at least one of toluene, chlorobenzene, dimethyl sulfoxide, water, methanol, ethanol, ether, acetone, chloroform, tetrahydrofuran, ethyl acetate, dichloromethane and benzene.
5. The method for preparing the hard carbon negative electrode material according to any one of claims 1 to 4, Features: Taking the total volume percentage of the acid solution and the solvent as 100%, the volume percentage of the acid solution is 0.05-0.8%.
6. The method for preparing the hard carbon negative electrode material according to any one of claims 1 to 4, Features: Taking the total mass percentage of the nitrogen-containing hard carbon precursor and the zinc source as 100%, the mass percentage of the zinc source is 5-75%.
7. The method for preparing the hard carbon negative electrode material according to any one of claims 1 to 4, Features: In the step S3, the pre-carbonization temperature is 200-800°C; And / or, the pre-carbonization time is 2 to 8 hours; And / or, the carbonization temperature is 1000-1800°C; And / or, the carbonization time is 1 to 6 hours; And / or, the heating rates in the pre-carbonization step and the carbonization step are independently selected from 3 to 8° C. / min.
8. The method for preparing the hard carbon negative electrode material according to claim 1, Features: The pre-carbonization step and the carbonization step are both carried out under the protection of an inert atmosphere.
9. The method for preparing the hard carbon negative electrode material according to claim 1, Features: The step S2 is: freeze-drying the mixture for 6 to 48 hours to obtain a solid product.
10. The method for preparing the hard carbon negative electrode material according to claim 1, Features: In the step S1, the temperature of the mixed reaction is 15 to 85° C., and the time of the mixed reaction is 1 to 72 hours.
11. A hard carbon negative electrode material, Features: The method is prepared by the method according to any one of claims 1 to 10.
12. An electrode, Features: The invention comprises the hard carbon negative electrode material according to claim 11, or the hard carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 10.
13. A sodium ion battery, Features: Comprising the hard carbon negative electrode material according to claim 11, or the electrode according to claim 12.
14. A method for preparing the hard carbon negative electrode material according to any one of claims 1 to 10 and / or use of the hard carbon negative electrode material according to claim 11 in the field of batteries.
Citation Information
Patent Citations
Preparation method of high-rate and low-temperature-resistant hard carbon negative electrode material and application of high-rate and low-temperature-resistant hard carbon negative electrode material in sodium-ion battery
CN116161643A
Preparation method of high-yield biomass-based sodium ion battery hard carbon negative electrode material
CN118343735A
Cited By
High-capacity hard carbon material and preparation method and application thereof
CN120589731A
A high-capacity hard carbon material, and a preparation method and application thereof
CN120589731B