Fiber-reinforced phenolic aldehyde-based carbon aerogel composite material and preparation method thereof
Through the preparation method of fiber-reinforced phenolic-based carbon aerogel composite, the problem of insufficient mechanical strength and cracking of carbon aerogel is solved, and fiber-reinforced carbon aerogel with high mechanical properties and low thermal conductivity is achieved, which is suitable for high-temperature kilns. and thermal protection engineering in aerospace.
Patent Information
- Application Number
- CN202411164732.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The mechanical strength of carbon aerogels is weak and prone to cracking when prepared in large sizes, which limits its industrial application.
By using the preparation method of fiber-reinforced phenolic-based carbon aerogel composite, the linear phenolic resin is dissolved with a crosslinking agent and a catalyst and impregnated the fiber mat, gelling and carbonizing, forming carbon nanoparticles with high mechanical properties. Three-dimensional structure.
The prepared fiber-reinforced phenolic carbon aerogel has a shrinkage, low density, good mechanical properties and low thermal conductivity. It is suitable for large-scale industrial production and is suitable for high-temperature thermal insulation materials.
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of aerogel material preparation, and relates to a fiber-reinforced phenolic-based carbon aerogel composite material and a preparation method thereof. Background Art
[0002] Carbon aerogel is a three-dimensional porous network structure material constructed by nano-scale carbon particles, with high specific surface area, low thermal conductivity and excellent high-temperature stability. Therefore, carbon aerogel has great application potential in many fields such as high-efficiency battery systems, high-performance catalyst carriers, advanced hydrogen storage technology, deep water treatment processes, thermal protection solutions in high-temperature environments, and thermal management technologies in the industrial field.
[0003] However, despite the many advantages of carbon aerogels, their mechanical strength is relatively weak, and they have large carbonization shrinkage and are prone to cracking when prepared in large sizes, which still poses significant challenges to their industrial application. Summary of the invention
[0004] The purpose of the present application is to provide a fiber-reinforced phenolic carbon aerogel composite material and a preparation method thereof. The prepared fiber-reinforced phenolic carbon aerogel has excellent properties such as small shrinkage, low density, good mechanical properties, and low thermal conductivity, and the fiber-reinforced phenolic carbon aerogel composite material can be industrially mass-produced using the method of the present application.
[0005] To achieve the above objectives, the present invention provides a fiber-reinforced phenolic-based carbon aerogel composite material and a preparation method thereof, wherein: A method for preparing a fiber-reinforced phenolic-based carbon aerogel composite material comprises the following steps: 1) Preparing a precursor solution: dissolving a linear phenolic resin, a crosslinking agent, and a catalyst in anhydrous ethanol in sequence to obtain a precursor solution; 2) Impregnation of fiber felt with precursor solution: Immersing the fiber felt in a mold filled with the precursor solution for impregnation treatment; 3) Gel, aging, and normal pressure drying: After impregnation, a portion of the precursor solution is pressed out, and after gelation, a fiber-reinforced phenolic organic wet alcohol gel is obtained; The fiber-reinforced phenolic organic wet alcohol gel is placed in an organic displacer for replacement, and then dried at normal pressure to obtain a fiber-reinforced phenolic organic aerogel; 4) Preparation of carbon aerogel: The fiber-reinforced phenolic organic aerogel is placed in a carbonization furnace and carbonized in a vacuum environment or a protective atmosphere to obtain a fiber-reinforced phenolic-based carbon aerogel composite material.
[0006] In one possible implementation manner, in the method for preparing a fiber-reinforced phenolic-based carbon aerogel composite material provided in an embodiment of the present application, in the step 1), the molecular weight of the linear phenolic resin is 500 g / mol to 2500 g / mol.
[0007] In one possible implementation, in the method for preparing a fiber-reinforced phenolic-based carbon aerogel composite material provided in an embodiment of the present application, in step 1): In terms of mass percentage, the amount of linear phenolic resin added is 5wt%~55wt% of the mass of anhydrous ethanol; The molar ratio of linear phenolic resin to crosslinking agent is (100-1000):1; The molar ratio of linear phenolic resin to catalyst is (0.1~1):1.
[0008] The crosslinking agent is a mixture of one or more of polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, polyoxyethylene polyoxypropylene ether (polyether F127) and sorbitan oleate (Span 80); The catalyst is hexamethylenetetramine.
[0009] In one possible implementation, in the method for preparing a fiber-reinforced phenolic-based carbon aerogel composite material provided in an embodiment of the present application, in step 1): After the linear phenolic resin is stirred and dissolved in anhydrous ethanol, a cross-linking agent is added and stirred at 20-50° C. for 0.5-5 hours. After cooling to room temperature, a catalyst hexamethylenetetramine is added and stirred for 1-2 hours.
[0010] In one possible implementation, in the method for preparing a fiber-reinforced phenolic-based carbon aerogel composite material provided in an embodiment of the present application, in step 2): The fiber felt is woven from one or more fibers of viscose, polyacrylonitrile and asphalt. The density of the fiber felt is 0.01~2g / cm 3 .
[0011] In one possible implementation, in the method for preparing a fiber-reinforced phenolic-based carbon aerogel composite material provided in an embodiment of the present application, in step 2): The liquid level of the precursor solution is 5 to 15 mm higher than the height of the fiber felt. The fiber felt is immersed in a normal pressure environment or in a vacuum environment for 0.5 to 4 hours.
[0012] In one possible implementation, in the method for preparing a fiber-reinforced phenolic-based carbon aerogel composite material provided in the embodiment of the present application, in the step 3): After the impregnation is completed, 0-90% volume ratio of the precursor solution is squeezed out and sealed in a mold, heated to 45-95°C in an oxygen-free environment, the gel time is 0.5-24h, and aged for 12-24h to obtain a fiber-reinforced phenolic organic wet alcohol gel.
[0013] In one possible implementation, in the method for preparing a fiber-reinforced phenolic-based carbon aerogel composite material provided in the embodiment of the present application, in the step 3): The replacement was carried out three times in total. In a single replacement process, an organic replacement agent with a volume of more than 1 times of the fiber-reinforced phenolic organic wet alcohol gel was added, and the mixture was sealed and placed in an oven at 80°C for replacement for 5 hours. After the three replacements were completed, the replaced products were placed in an oven for drying, successively at 30°C for 6 h, 50°C for 6 h, and 80°C for 12 h.
[0014] In one possible implementation, in the method for preparing a fiber-reinforced phenolic-based carbon aerogel composite material provided in an embodiment of the present application, in step 4): The carbonization procedure is to keep at 200℃ for 1h, keep at 500℃ for 2h, keep at the carbonization temperature for 30min~5h, and the carbonization temperature is 650~2300℃.
[0015] A fiber-reinforced phenolic-based carbon aerogel composite material is prepared by the preparation method of the fiber-reinforced phenolic-based carbon aerogel composite material.
[0016] The preparation method of the fiber-reinforced phenolic-based carbon aerogel composite material provided by the present application promotes the attachment of linear phenolic resin to the fiber by using a crosslinking agent, and can gel-coat the fiber in situ on the fiber. The three-dimensional structure composed of carbon nanoparticles subsequently carbonized not only reduces the thermal conductivity but also improves the mechanical properties. At the same time, it can shrink synergistically during the drying and carbonization process, greatly avoiding the overall shrinkage, which is conducive to the preparation of large-sized and special-shaped specimens with low thermal conductivity, no cracking, and low shrinkage.
[0017] Compared with the prior art, it has at least the following advantages: 1) This application uses low-cost linear phenolic resin and hexamethylenetetramine as raw materials to successfully prepare fiber-reinforced phenolic-based carbon aerogel composites under normal pressure; 2) The adhesion of phenolic gel on the fiber was promoted by adding cross-linking agent and controlling its addition amount; 3) Fiber-reinforced phenolic-based carbon aerogel composites with different densities were obtained by controlling the precursor content. The three-dimensional structure composed of carbon nanoparticles generated by subsequent carbonization not only reduces the thermal conductivity but also improves the mechanical properties. At the same time, it can shrink synergistically during the drying and carbonization process, greatly avoiding the overall shrinkage, which is conducive to the preparation of large-sized and special-shaped specimens with low thermal conductivity, no cracking, and small shrinkage. It is expected to be used on a large scale as a new type of high-temperature insulation material in high-temperature kilns and thermal protection projects in aerospace. DETAILED DESCRIPTION
[0018] Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making any creative work shall fall within the scope of protection of this application.
[0019] The present application provides a method for preparing a fiber-reinforced phenolic-based carbon aerogel composite material, comprising the following steps: 1) Prepare a precursor solution: Dissolve the linear phenolic resin in anhydrous ethanol with stirring, add a cross-linking agent, stir for 0.5 to 5 hours at 20 to 50°C, cool to room temperature, add a catalyst hexamethylenetetramine, stir for 1 to 2 hours, and obtain a precursor solution.
[0020] In step 1): The molecular weight of linear phenolic resin is 500g / mol~2500g / mol.
[0021] In terms of mass percentage, the amount of linear phenolic resin added is 5wt%~55wt% of the mass of anhydrous ethanol; The molar ratio of linear phenolic resin to crosslinking agent is (100-1000):1; The molar ratio of linear phenolic resin to catalyst is (0.1~1):1.
[0022] The crosslinking agent is a mixture of one or more of polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, polyoxyethylene polyoxypropylene ether (polyether F127) and sorbitan oleate (Span 80); The catalyst is hexamethylenetetramine.
[0023] 2) Impregnation of fiber felt with precursor solution: Immersing the fiber felt in a mold filled with the precursor solution for impregnation treatment.
[0024] In step 2): The liquid level of the precursor solution is 5 to 15 mm higher than the height of the fiber felt. The fiber felt is immersed in a normal pressure environment or in a vacuum environment for 0.5 to 4 hours.
[0025] The fiber felt is woven from one or more fibers of viscose, polyacrylonitrile and asphalt. The density of the fiber felt is 0.01~2g / cm 3 .
[0026] 3) Gel, aging, and drying at normal pressure: After the impregnation is completed, 0-90% volume ratio of the precursor solution is squeezed out ("0" means that no pressure is applied to squeeze out the precursor solution after impregnation) and then sealed in a mold, heated to 45-95°C in an oxygen-free environment, the gel time is 0.5-24h, and aged for 12-24h to obtain a fiber-reinforced phenolic organic wet alcohol gel.
[0027] The fiber-reinforced phenolic organic wet alcohol gel is placed in an organic displacing agent for replacement, and then dried at normal pressure to obtain the fiber-reinforced phenolic organic aerogel.
[0028] In step 3): The replacement was carried out three times in total. In a single replacement process, an organic replacement agent with a volume of more than 1 times of the fiber-reinforced phenolic organic wet alcohol gel was added, and the mixture was sealed and placed in an oven at 80°C for replacement for 5 hours. In the first displacement, anhydrous ethanol was used as the organic displacement agent; When performing the second and third displacements, a mixture of one or more of n-hexane, acetone, butanone, tert-butanol, and n-heptane solution is used as an organic displacement agent.
[0029] After the three replacements were completed, the replaced products were placed in an oven for drying, successively at 30°C for 6 h, 50°C for 6 h, and 80°C for 12 h.
[0030] 4) Preparation of carbon aerogel: Place the fiber-reinforced phenolic organic aerogel into a carbonization furnace and carbonize it in a vacuum environment or a protective atmosphere (inert gas environment such as nitrogen and argon). The carbonization procedure is to keep it at 200°C for 1 hour, keep it at 500°C for 2 hours, and keep it at the carbonization temperature for 30 minutes to 5 hours. The carbonization temperature is 650~2300°C to obtain a fiber-reinforced phenolic-based carbon aerogel composite material.
[0031] The present application provides a fiber-reinforced phenolic carbon aerogel composite material and a preparation method thereof. The prepared fiber-reinforced phenolic carbon aerogel has excellent properties such as small shrinkage, low density, good mechanical properties, and low thermal conductivity, and the fiber-reinforced phenolic carbon aerogel composite material can be industrially mass-produced using the method of the present application.
[0032] Compared with the prior art, it has at least the following advantages: 1) This application uses low-cost linear phenolic resin and hexamethylenetetramine as raw materials to successfully prepare fiber-reinforced phenolic-based carbon aerogel composites under normal pressure; 2) The adhesion of phenolic gel on the fiber was promoted by adding cross-linking agent and controlling its addition amount; 3) Fiber-reinforced phenolic-based carbon aerogel composites with different densities were obtained by controlling the precursor content. The three-dimensional structure composed of carbon nanoparticles generated by subsequent carbonization not only reduces the thermal conductivity but also improves the mechanical properties. At the same time, it can shrink synergistically during the drying and carbonization process, greatly avoiding the overall shrinkage, which is conducive to the preparation of large-sized and special-shaped specimens with low thermal conductivity, no cracking, and small shrinkage. It is expected to be used on a large scale as a new type of high-temperature insulation material in high-temperature kilns and thermal protection projects in aerospace.
[0033] The specific implementation methods of the technical solution of this application are as follows: Example
[0034] Prepare a 40wt% ethanol solution of linear phenolic resin, add polyvinyl alcohol at a molar ratio of 100:1 of linear phenolic resin: crosslinker, and stir for 5h at 25℃, then add hexamethylenetetramine at a molar ratio of 0.5:1 of linear phenolic resin: catalyst, and stir for 2h to obtain a precursor solution. 3 Viscose felt is used as a reinforcement. Under normal pressure, the fiber felt is immersed in the above-mentioned precursor solution for 1 hour, and the precursor with a volume ratio of 30% is taken out by uniform pressure and placed in a mold, and heated to 80°C in an oxygen-free environment to gel and age for 24 hours to obtain a viscose-based fiber-reinforced phenolic organic wet alcohol gel. The viscose-based fiber-reinforced phenolic organic wet alcohol gel is placed in a sealed container and replaced with ethanol three times in an oven at 80°C, and then dried in an oven to obtain a viscose-based fiber-reinforced phenolic organic dry alcohol gel. The drying procedure is 30°C for 6 hours, 50°C for 6 hours, and 80°C for 12 hours. Then the viscose-based fiber-reinforced phenolic organic dry alcohol gel is carbonized in a vacuum environment, and the carbonization procedure is 200°C for 1 hour, 500°C for 2 hours, and 900°C for 2 hours to obtain a viscose fiber felt-reinforced phenolic carbon aerogel composite material. Example
[0035] Prepare a 30wt% ethanol solution of linear phenolic resin, add polyvinyl alcohol at a molar ratio of 250:1 of linear phenolic resin: crosslinker, and stir for 3h at 40℃, then add hexamethylenetetramine at a molar ratio of 0.2:1 of linear phenolic resin: catalyst, and stir for 2h to obtain a precursor solution. 3Viscose felt is used as a reinforcement. Under normal pressure, the fiber felt is immersed in the above-mentioned precursor solution for 2 hours, and the precursor with a volume ratio of 40% is taken out by uniform pressure and placed in a mold, and heated to 80℃ in an oxygen-free environment to gel and age for 24 hours to obtain a viscose-based fiber-reinforced phenolic organic wet alcohol gel. The viscose-based fiber-reinforced phenolic organic wet alcohol gel is placed in a sealed container and replaced once with ethanol, once with ethanol: n-hexane (volume ratio 1:1), and once with n-hexane in an oven at 80℃, and then dried in an oven to obtain a viscose-based fiber-reinforced phenolic organic dry alcohol gel. The drying procedure is 30℃ for 6 hours, 50℃ for 6 hours, and 80℃ for 12 hours. Then, the viscose-based fiber-reinforced phenolic organic dry alcohol gel is carbonized in a vacuum environment, and the carbonization procedure is 200℃ for 1 hour, 500℃ for 2 hours, and 1200℃ for 2 hours to obtain a fiber felt-reinforced phenolic carbon aerogel composite material. Example
[0036] Prepare a 20wt% ethanol solution of linear phenolic resin, add polyvinyl alcohol at a molar ratio of 500:1 of linear phenolic resin: crosslinker, and stir for 0.5h at 50℃, then add hexamethylenetetramine at a molar ratio of 0.3:1 of linear phenolic resin: catalyst, and stir for 2h to obtain a precursor solution. 3 Viscose felt is used as reinforcement. Under normal pressure, the fiber felt is immersed in the above-mentioned precursor solution for 2 hours, and the precursor with a volume ratio of 15% is taken out by uniform pressure and placed in a mold, and heated to 95℃ in an oxygen-free environment to gel and aged for 24 hours to obtain a viscose-based fiber-reinforced phenolic organic wet alcohol gel. The viscose-based fiber-reinforced phenolic organic wet alcohol gel is placed in a sealed container and replaced once with ethanol, once with ethanol: n-hexane (volume ratio 1:1), and once with n-hexane in an oven at 80℃ for three times, and then dried in an oven to obtain a viscose-based fiber-reinforced phenolic organic dry alcohol gel. The drying procedure is 30℃ for 6 hours, 50℃ for 6 hours, and 80℃ for 12 hours. Then, the viscose-based fiber-reinforced phenolic organic dry alcohol gel is carbonized in a vacuum environment, and the carbonization procedure is 200℃ for 1 hour, 500℃ for 2 hours, and 1600℃ for 2 hours to obtain a fiber felt-reinforced phenolic carbon aerogel composite material. Example
[0037] Prepare a 10wt% ethanol solution of linear phenolic resin, add polyvinyl alcohol at a molar ratio of 700:1 of linear phenolic resin: crosslinker, and stir for 4h at 30℃, then add hexamethylenetetramine at a molar ratio of 0.5:1 of linear phenolic resin: catalyst, and stir for 2h to obtain a precursor solution. 3Viscose felt is used as reinforcement. Under normal pressure, the fiber felt is immersed in the above-mentioned precursor solution for 2 hours, and the precursor with a volume ratio of 30% is taken out by uniform pressure and placed in a mold, and heated to 85℃ in an oxygen-free environment to gel and aged for 24 hours to obtain a viscose-based fiber-reinforced phenolic organic wet alcohol gel. The viscose-based fiber-reinforced phenolic organic wet alcohol gel is placed in a sealed container and replaced once with ethanol, once with ethanol: n-hexane (volume ratio 1:1), and once with n-hexane in an oven at 80℃ for three times, and then dried in an oven to obtain a viscose-based fiber-reinforced phenolic organic dry alcohol gel. The drying procedure is 30℃ for 6 hours, 50℃ for 6 hours, and 80℃ for 12 hours. Then, the viscose-based fiber-reinforced phenolic organic dry alcohol gel is carbonized in a vacuum environment, and the carbonization procedure is 200℃ for 1 hour, 500℃ for 2 hours, and 600℃ for 2 hours to obtain a fiber felt-reinforced phenolic carbon aerogel composite material. Example
[0038] Prepare a 40wt% ethanol solution of linear phenolic resin, add polyvinyl alcohol at a molar ratio of 900:1 of linear phenolic resin: crosslinker, and stir for 5h at 25℃, then add hexamethylenetetramine at a molar ratio of 0.2:1 of linear phenolic resin: catalyst, and stir for 2h to obtain a precursor solution. 3 Viscose felt is used as a reinforcement. Under normal pressure, the fiber felt is immersed in the above-mentioned precursor solution for 1 hour, and the precursor with a volume ratio of 70% is taken out by uniform pressure and placed in a mold, and heated to 80°C in an oxygen-free environment to gel and age for 24 hours to obtain a viscose-based fiber-reinforced phenolic organic wet alcohol gel. The viscose-based fiber-reinforced phenolic organic wet alcohol gel is placed in a sealed container and replaced with ethanol three times in an oven at 80°C, and then dried in an oven to obtain a viscose-based fiber-reinforced phenolic organic dry alcohol gel. The drying procedure is 30°C for 6 hours, 50°C for 6 hours, and 80°C for 12 hours. Then the viscose-based fiber-reinforced phenolic organic dry alcohol gel is carbonized in a vacuum environment, and the carbonization procedure is 200°C for 1 hour, 500°C for 2 hours, and 1000°C for 2 hours to obtain a viscose fiber felt-reinforced phenolic carbon aerogel composite material. Example
[0039] Prepare a 55wt% ethanol solution of linear phenolic resin, add polyvinyl alcohol at a molar ratio of 900:1 of linear phenolic resin: crosslinker, and stir for 5h at 25℃, then add hexamethylenetetramine at a molar ratio of 0.2:1 of linear phenolic resin: catalyst, and stir for 2h to obtain a precursor solution. 3Viscose felt is used as a reinforcement. Under normal pressure, the fiber felt is immersed in the above-mentioned precursor solution for 1 hour, and the precursor with a volume ratio of 90% is taken out by uniform pressure and placed in a mold, and heated to 45°C in an oxygen-free environment to gel and aged for 24 hours to obtain a viscose-based fiber-reinforced phenolic organic wet alcohol gel. The viscose-based fiber-reinforced phenolic organic wet alcohol gel is placed in a sealed container and replaced with ethanol three times in an oven at 80°C, and then dried in an oven to obtain a viscose-based fiber-reinforced phenolic organic dry alcohol gel. The drying procedure is 30°C for 6 hours, 50°C for 6 hours, and 80°C for 12 hours. Then the viscose-based fiber-reinforced phenolic organic dry alcohol gel is carbonized in a vacuum environment, and the carbonization procedure is 200°C for 1 hour, 500°C for 2 hours, and 1000°C for 2 hours to obtain a viscose fiber felt-reinforced phenolic carbon aerogel composite material. Example
[0040] Prepare a 5wt% ethanol solution of linear phenolic resin, add polyvinyl alcohol at a molar ratio of 900:1 of linear phenolic resin: crosslinker, and stir for 1h at 25℃, then add hexamethylenetetramine at a molar ratio of 0.2:1 of linear phenolic resin: catalyst, and stir for 2h to obtain a precursor solution. 3 Viscose felt is used as a reinforcement. Under normal pressure, the fiber felt is immersed in the above-mentioned precursor solution for 1 hour, and the precursor with a volume ratio of 0% is taken out by uniform pressure and placed in a mold, and heated to 95°C in an oxygen-free environment to gel and aged for 24 hours to obtain a viscose-based fiber-reinforced phenolic organic wet alcohol gel. The viscose-based fiber-reinforced phenolic organic wet alcohol gel is placed in a sealed container and replaced with ethanol three times in an oven at 80°C, and then dried in an oven to obtain a viscose-based fiber-reinforced phenolic organic dry alcohol gel. The drying procedure is 30°C for 6 hours, 50°C for 6 hours, and 80°C for 12 hours. Then the viscose-based fiber-reinforced phenolic organic dry alcohol gel is carbonized in a vacuum environment, and the carbonization procedure is 200°C for 1 hour, 500°C for 2 hours, and 1000°C for 2 hours to obtain a viscose fiber felt-reinforced phenolic carbon aerogel composite material. Example
[0041] Prepare a 30wt% ethanol solution of linear phenolic resin, add polyvinyl pyrrolidone at a molar ratio of 700:1 of linear phenolic resin: crosslinker, and stir for 0.5h at 25℃, then add hexamethylenetetramine at a molar ratio of 0.2:1 of linear phenolic resin: catalyst, and stir for 2h to obtain a precursor solution. 3Viscose felt is used as a reinforcement. Under normal pressure, the fiber felt is immersed in the above-mentioned precursor solution for 2 hours, and the precursor with a volume ratio of 20% is taken out by uniform pressure and placed in a mold, and heated to 80℃ in an oxygen-free environment to gel and aged for 24 hours to obtain a viscose-based fiber-reinforced phenolic organic wet alcohol gel. The viscose-based fiber-reinforced phenolic organic wet alcohol gel is placed in a sealed container and replaced once with ethanol, once with ethanol: n-hexane (volume ratio 1:1), and once with n-hexane in an oven at 80℃, and then dried in an oven to obtain a viscose-based fiber-reinforced phenolic organic dry alcohol gel. The drying procedure is 30℃ for 6 hours, 50℃ for 6 hours, and 80℃ for 12 hours. Then, the viscose-based fiber-reinforced phenolic organic dry alcohol gel is carbonized in a vacuum environment, and the carbonization procedure is 200℃ for 1 hour, 500℃ for 2 hours, and 1200℃ for 2 hours to obtain a fiber felt-reinforced phenolic carbon aerogel composite material. Example
[0042] Prepare a 30wt% ethanol solution of linear phenolic resin, add polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer at a molar ratio of 800:1 of linear phenolic resin: crosslinker, and stir for 3 hours at 25°C, then add hexamethylenetetramine at a molar ratio of 0.1:1 of linear phenolic resin: catalyst, and stir for 2 hours to obtain a precursor solution. 3 Viscose felt is used as a reinforcement. Under normal pressure, the fiber felt is immersed in the above-mentioned precursor solution for 2 hours, and the precursor with a volume ratio of 20% is taken out by uniform pressure and placed in a mold, and heated to 80℃ in an oxygen-free environment to gel and aged for 24 hours to obtain a viscose-based fiber-reinforced phenolic organic wet alcohol gel. The viscose-based fiber-reinforced phenolic organic wet alcohol gel is placed in a sealed container and replaced once with ethanol, once with ethanol: n-hexane (volume ratio 1:1), and once with n-hexane in an oven at 80℃, and then dried in an oven to obtain a viscose-based fiber-reinforced phenolic organic dry alcohol gel. The drying procedure is 30℃ for 6 hours, 50℃ for 6 hours, and 80℃ for 12 hours. Then, the viscose-based fiber-reinforced phenolic organic dry alcohol gel is carbonized in a vacuum environment, and the carbonization procedure is 200℃ for 1 hour, 500℃ for 2 hours, and 1200℃ for 2 hours to obtain a fiber felt-reinforced phenolic carbon aerogel composite material. Example
[0043] Prepare a 30wt% ethanol solution of linear phenolic resin, add polyoxyethylene polyoxypropylene ether (polyether F127) at a molar ratio of 600:1 of linear phenolic resin: crosslinker, and stir for 3h at 25℃, then add hexamethylenetetramine at a molar ratio of 0.1:1 of linear phenolic resin: catalyst, and stir for 2h to obtain a precursor solution. 3Viscose felt is used as a reinforcement. Under normal pressure, the fiber felt is immersed in the above-mentioned precursor solution for 2 hours, and the precursor with a volume ratio of 20% is taken out by uniform pressure and placed in a mold, and heated to 80℃ in an oxygen-free environment to gel and aged for 24 hours to obtain a viscose-based fiber-reinforced phenolic organic wet alcohol gel. The viscose-based fiber-reinforced phenolic organic wet alcohol gel is placed in a sealed container and replaced once with ethanol, once with ethanol: n-hexane (volume ratio 1:1), and once with n-hexane in an oven at 80℃, and then dried in an oven to obtain a viscose-based fiber-reinforced phenolic organic dry alcohol gel. The drying procedure is 30℃ for 6 hours, 50℃ for 6 hours, and 80℃ for 12 hours. Then, the viscose-based fiber-reinforced phenolic organic dry alcohol gel is carbonized in a vacuum environment, and the carbonization procedure is 200℃ for 1 hour, 500℃ for 2 hours, and 1200℃ for 2 hours to obtain a fiber felt-reinforced phenolic carbon aerogel composite material. Example
[0044] Prepare a 30wt% ethanol solution of linear phenolic resin, add sorbitan oleate (Span80) at a molar ratio of 600:1 of linear phenolic resin: crosslinker, stir for 1h at 25℃, then add hexamethylenetetramine at a molar ratio of 0.1:1 of linear phenolic resin: catalyst, stir for 2h to obtain a precursor solution. 3 Viscose felt is used as a reinforcement. Under normal pressure, the fiber felt is immersed in the above-mentioned precursor solution for 2 hours, and the precursor with a volume ratio of 20% is taken out by uniform pressure and placed in a mold, and heated to 80℃ in an oxygen-free environment to gel and aged for 24 hours to obtain a viscose-based fiber-reinforced phenolic organic wet alcohol gel. The viscose-based fiber-reinforced phenolic organic wet alcohol gel is placed in a sealed container and replaced once with ethanol, once with ethanol: n-hexane (volume ratio 1:1), and once with n-hexane in an oven at 80℃, and then dried in an oven to obtain a viscose-based fiber-reinforced phenolic organic dry alcohol gel. The drying procedure is 30℃ for 6 hours, 50℃ for 6 hours, and 80℃ for 12 hours. Then, the viscose-based fiber-reinforced phenolic organic dry alcohol gel is carbonized in a vacuum environment, and the carbonization procedure is 200℃ for 1 hour, 500℃ for 2 hours, and 1200℃ for 2 hours to obtain a fiber felt-reinforced phenolic carbon aerogel composite material. Example
[0045] Prepare a 30wt% ethanol solution of linear phenolic resin, add polyvinyl pyrrolidone and polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer mixture (polyvinyl pyrrolidone: polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer molar ratio: 1:1) according to the linear phenolic resin: crosslinking agent at a molar ratio of 600:1, stir for 1h at 25°C, then add hexamethylenetetramine at a molar ratio of 0.1:1 according to the linear phenolic resin: catalyst, stir for 2h to obtain a precursor solution. Use 1.5g / cm 3 Viscose felt is used as a reinforcement. Under normal pressure, the fiber felt is immersed in the above-mentioned precursor solution for 2 hours, and the precursor with a volume ratio of 20% is taken out by uniform pressure and placed in a mold, and heated to 80℃ in an oxygen-free environment to gel and aged for 24 hours to obtain a viscose-based fiber-reinforced phenolic organic wet alcohol gel. The viscose-based fiber-reinforced phenolic organic wet alcohol gel is placed in a sealed container and replaced once with ethanol, once with ethanol: n-hexane (volume ratio 1:1), and once with n-hexane in an oven at 80℃, and then dried in an oven to obtain a viscose-based fiber-reinforced phenolic organic dry alcohol gel. The drying procedure is 30℃ for 6 hours, 50℃ for 6 hours, and 80℃ for 12 hours. Then, the viscose-based fiber-reinforced phenolic organic dry alcohol gel is carbonized in a vacuum environment, and the carbonization procedure is 200℃ for 1 hour, 500℃ for 2 hours, and 1200℃ for 2 hours to obtain a fiber felt-reinforced phenolic carbon aerogel composite material.
[0046] It is hereby noted that in this example, the crosslinking agent is added to the linear phenolic anhydrous ethanol solution in a molar ratio of polyvinyl pyrrolidone:polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer: 1:1, but is not limited to this molar ratio, and catalysts including polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, polyoxyethylene polyoxypropylene ether (polyether F127) and sorbitan oleate (Span80) can be used as crosslinking agents in any type and proportion, which will not be elaborated here.
[0047] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application, rather than to limit it. Although the present application has been described in detail with reference to the above embodiments, a person skilled in the art should understand that the technical solution described in the above embodiments can still be modified, or some or all of the technical features can be replaced by equivalents. These modifications or replacements are within the scope of protection of the present application.
Claims
1. A method for preparing a fiber-reinforced phenolic-based carbon aerogel composite material, It is characterized in that The steps include: 1) Preparing a precursor solution: dissolving a linear phenolic resin, a crosslinking agent, and a catalyst in anhydrous ethanol in sequence to obtain a precursor solution; 2) Impregnation of fiber felt with precursor solution: Immersing the fiber felt in a mold filled with the precursor solution for impregnation treatment; 3) Gel, aging, and normal pressure drying: After impregnation, a portion of the precursor solution is pressed out, and after gelation, a fiber-reinforced phenolic organic wet alcohol gel is obtained; The fiber-reinforced phenolic organic wet alcohol gel is placed in an organic displacer for replacement, and then dried at normal pressure to obtain a fiber-reinforced phenolic organic aerogel; 4) Preparation of carbon aerogel: The fiber-reinforced phenolic organic aerogel is placed in a carbonization furnace and carbonized in a vacuum environment or a protective atmosphere to obtain a fiber-reinforced phenolic-based carbon aerogel composite material.
2. The method for preparing the fiber-reinforced phenolic-based carbon aerogel composite material according to claim 1, It is characterized in that In the step 1), the molecular weight of the linear phenolic resin is 500 g / mol to 2500 g / mol.
3. The method for preparing the fiber-reinforced phenolic-based carbon aerogel composite material according to claim 1, It is characterized in that In the step 1): In terms of mass percentage, the amount of linear phenolic resin added is 5wt%~55wt% of the mass of anhydrous ethanol; The molar ratio of linear phenolic resin to crosslinking agent is (100-1000):1; The molar ratio of linear phenolic resin to catalyst is (0.1~1):1; The crosslinking agent is a mixture of one or more of polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, polyoxyethylene polyoxypropylene ether (polyether F127) and sorbitan oleate (Span 80); The catalyst is hexamethylenetetramine.
4. The method for preparing the fiber-reinforced phenolic-based carbon aerogel composite material according to claim 1, It is characterized in that In the step 1): After the linear phenolic resin is stirred and dissolved in anhydrous ethanol, a cross-linking agent is added and stirred at 20-50° C. for 0.5-5 hours. After cooling to room temperature, a catalyst hexamethylenetetramine is added and stirred for 1-2 hours.
5. The method for preparing the fiber-reinforced phenolic-based carbon aerogel composite material according to claim 1, It is characterized in that In the step 2): The fiber felt is woven from one or more fibers of viscose, polyacrylonitrile and asphalt. The density of the fiber felt is 0.01~2g / cm 3 .
6. The method for preparing the fiber-reinforced phenolic-based carbon aerogel composite material according to claim 1, It is characterized in that In the step 2): The liquid level of the precursor solution is 5 to 15 mm higher than the height of the fiber felt. The fiber felt is immersed in a normal pressure environment or in a vacuum environment for 0.5 to 4 hours.
7. The method for preparing the fiber-reinforced phenolic-based carbon aerogel composite material according to claim 1, It is characterized in that In the step 3): After the impregnation is completed, 0-90% volume ratio of the precursor solution is squeezed out and sealed in a mold, heated to 45-95°C in an oxygen-free environment, the gel time is 0.5-24h, and aged for 12-24h to obtain a fiber-reinforced phenolic organic wet alcohol gel.
8. The method for preparing the fiber-reinforced phenolic-based carbon aerogel composite material according to claim 1, It is characterized in that In the step 3): The replacement was carried out three times in total. In a single replacement process, an organic replacement agent with a volume of more than 1 times of the fiber-reinforced phenolic organic wet alcohol gel was added, and the mixture was sealed and placed in an oven at 80°C for 5 hours. After the three replacements were completed, the replaced products were placed in an oven for drying, successively at 30°C for 6 h, 50°C for 6 h, and 80°C for 12 h.
9. The method for preparing the fiber-reinforced phenolic-based carbon aerogel composite material according to claim 1, It is characterized in that In the step 4): The carbonization procedure is to keep at 200℃ for 1h, keep at 500℃ for 2h, keep at the carbonization temperature for 30min~5h, and the carbonization temperature is 650~2300℃.
10. A fiber-reinforced phenolic-based carbon aerogel composite material, It is characterized in that The fiber-reinforced phenolic-based carbon aerogel composite material is prepared by the preparation method of any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of fiber-reinforced phenolic resin composite material and fiber-reinforced phenolic resin composite material
CN112321989A
Preparation method of low-cost and high-strength fiber-reinforced nano porous carbon composite material
CN112341234A
Preparation method of heat insulation-bearing integrated light carbon-based composite material
CN113860909A
Process for making a reinforced fibrous mat and product made therefrom
US5302445A
Cited By
Polyacrylonitrile-itaconic acid fibrofelt reinforced carbon aerogel composite material as well as preparation method and application thereof
CN119569475A
A polyacrylonitrile-itaconic acid fiber felt reinforced carbon aerogel composite material, its preparation method and application
CN119569475B
Iron-carbon composite aerogel catalyst for preparing biofuel from synthesis gas as well as preparation method and application of iron-carbon composite aerogel catalyst
CN122230727A
Iron-carbon composite aerogel catalyst for preparing biofuel from syngas and preparation method and application thereof
CN122230727B