Preparation method of silicon-carbon negative electrode material and silicon-carbon negative electrode material reactor

By depositing silicon coating on the surface of the carbon powder and removing agglomerated particles using a screening filter, then carrying out carbon coating, combined with the multi-reaction device centralized processing and stir dispersion technology, the agglomeration problem of nano-silicon materials is solved and the silicon-carbon negative electrode material is improved The stability and production efficiency achieve efficient battery cycle performance.

CN118954516AInactive Publication Date: 2024-11-15SHANGHAI RHYME NEW ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411015325.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing lithium battery silicon carbon anode material process, nano-silicon materials are prone to agglomeration in the reactor, resulting in structural damage to the electrode material and deterioration in cycling performance, and low production efficiency.

Method used

Silicon coated particles are formed by depositing silicon on the surface of the carbon powder, and agglomerated particles are removed by using a screening filter, and then carbon coated. Multiple small-capacity reaction devices are used to concentrate on the large-capacity reaction device for carbon coating, combined with forced stirring and airflow dispersion technology to ensure sufficient dispersion and uniform deposition of reactant particles.

Benefits of technology

It significantly improves the uniformity and stability of silicon-carbon anode materials, improves production efficiency and product quality, extends the cycle life, and avoids the occurrence of agglomeration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954516A_ABST
    Figure CN118954516A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a silicon-carbon negative electrode material and a silicon-carbon negative electrode material reactor. The method comprises the following steps: depositing silicon on the surface of carbon powder by decomposing a silicon source gas to form silicon-coated particles; screening and filtering the silicon coated particles; and carrying out carbon coating on the screened silicon-coated particles to obtain the silicon-carbon negative electrode material. The number of the silicon-coated particles capable of completing carbon coating is determined by performing silicon coating on carbon powder in multiple batches to form the silicon-coated particles every time the silicon-carbon negative electrode material obtained by performing carbon coating on the screened silicon-coated particles is obtained. The silicon-carbon negative electrode material prepared by the preparation method of the silicon-carbon negative electrode material is tight in component connection and strong in binding force, and has excellent cycle life and stability; the silicon-carbon negative electrode material reactor provided by the invention not only can realize continuous production, but also can ensure the overall product quality and obviously improve the production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of silicon-carbon negative electrode materials for lithium batteries, and in particular to a method for preparing silicon-carbon negative electrode materials and a silicon-carbon negative electrode material reactor. Background Art

[0002] At present, the domestic lithium battery industry is developing rapidly, and society's expectations for the energy density of lithium-ion batteries are also increasing. Therefore, the development of positive and negative battery materials with high specific energy has become a top priority. Currently, commercialized graphite negative electrode materials are close to their theoretical specific capacity limit (372mAh / g). Therefore, in order to further improve the energy density of batteries, finding negative electrode materials with higher specific capacity has become the focus of industry research. Silicon alloys with lithium during charging, and its theoretical specific capacity is as high as 4200mAh / g, which is more than ten times that of current graphite negative electrode materials. It is not easy to produce lithium precipitation hazards, and its safety is better than that of graphite negative electrode materials. It has abundant reserves and low cost, and is the most promising new generation of lithium battery negative electrode materials.

[0003] However, the volume of silicon itself expands by more than 300% during the charge and discharge cycle. When lithium ions are embedded in and released from silicon during the charge and discharge process, the volume of silicon particles changes, resulting in structural damage to the electrode material. This expansion phenomenon leads to capacity decay and deterioration of the cycle performance of the electrode material. In addition, the diffusion rate of lithium ions in silicon materials is slow, resulting in a low charge and discharge rate. In order to improve the performance of silicon negative electrode materials, carbon materials are usually used to form composite materials with them. This method can enhance the mechanical stability of the electrode material and reduce the impact of volume expansion. At present, the commonly used method is to use carbon to coat silicon particles, that is, to form a protective layer on the surface of silicon. However, the direct use of nano-silicon powder has obvious disadvantages: first, in terms of particle size, and second, it is difficult to prepare, disperse, and prevent surface oxidation of nano-silicon on a large scale. Moreover, the easy agglomeration of nano-silicon, low compaction density, and huge volume changes in the silicon material itself pose challenges to the maturity of this technology.

[0004] The existing production process often uses a single fluidized bed for vapor deposition, and silicon and carbon deposition and coating are carried out successively in the reactor. However, the environments required for the reactions of silicon deposition and carbon coating are not completely consistent, and there are differences in the equipment and temperature requirements. At the same time, nano-silicon is particularly easy to aggregate together during chemical vapor deposition in the reactor, forming lumps and agglomerations. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the current silicon-carbon negative electrode material process, the present invention provides a method for preparing a silicon-carbon negative electrode material and a silicon-carbon negative electrode material reactor, wherein the silicon-carbon negative electrode material is formed by coating carbon powder with silicon and then coating it with carbon, and the coating is more uniform, the components are tightly connected, agglomeration is not easy to occur, and the production efficiency is greatly improved; the reactor is provided with a first reaction device, a second reaction device, a reaction supporting system and a screening filter, which can not only realize continuous production, but also ensure the overall product quality and realize a significant improvement in production efficiency

[0006] To achieve the above object, the embodiments of the present invention adopt the following technical solutions:

[0007] A method for preparing a silicon-carbon negative electrode material, the method comprising the following steps:

[0008] Depositing silicon on the surface of carbon powder by decomposing silicon source gas to form silicon-coated particles;

[0009] Screening and filtering the silicon-coated particles;

[0010] Carbon coating the screened silicon-coated particles to obtain a silicon-carbon negative electrode material;

[0011] Each time the sieved silicon-coated particles are carbon-coated to obtain the silicon-carbon negative electrode material, the number of silicon-coated particles that can be carbon-coated is obtained by performing silicon-coating on carbon powder in multiple batches to form silicon-coated particles.

[0012] According to one aspect of the present invention, the step of forming silicon-coated particles by decomposing a silicon source gas to deposit silicon on the surface of carbon powder includes: stirring the carbon powder; heating the silicon source gas to a temperature of 400-600°C to decompose the silicon source gas; and the silicon source gas decomposes and deposits silicon on the surface of the carbon powder to form silicon-coated particles.

[0013] According to one aspect of the present invention, the step of forming silicon-coated particles by depositing silicon on the surface of carbon powder by decomposing silicon source gas includes: introducing a mixed gas of silicon source gas and carrier gas, wherein the ratio of silicon source gas to carrier gas is 1:1 to 1:10.

[0014] According to one aspect of the present invention, the carbon-coating of the screened silicon-coated particles to obtain the silicon-carbon negative electrode material comprises: decomposing a carbon source gas to deposit carbon on the surface of the screened silicon-coated particles to obtain the silicon-carbon negative electrode material.

[0015] According to one aspect of the present invention, the step of obtaining a silicon-carbon negative electrode material by decomposing a carbon source gas to deposit carbon on the surface of screened silicon-coated particles includes: stirring the screened silicon-coated particles; heating the carbon source gas to a temperature of 600-1200°C to decompose the carbon source gas; and decomposing and depositing the carbon source gas on the surface of the screened silicon-coated particles to obtain a silicon-carbon negative electrode material.

[0016] According to one aspect of the present invention, the step of obtaining a silicon-carbon negative electrode material by decomposing a carbon source gas to deposit carbon on the surface of silicon-coated particles includes: introducing a mixed gas of a carbon source gas and a carrier gas, wherein the ratio of the carbon source gas to the carrier gas is 1:1 to 1:15.

[0017] According to one aspect of the present invention, the method further comprises the following steps: drying the carbon powder and activating the surface activity of the carbon powder before decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form silicon-coated particles.

[0018] A silicon-carbon negative electrode material reactor, comprising:

[0019] The first reaction device is used to decompose the silicon source gas to deposit silicon on the surface of the carbon powder to form silicon-coated particles;

[0020] A second reaction device, connected to at least one of the first reaction devices, is used to carbon-coat the silicon-coated particles formed by the first reaction device to form a silicon-carbon negative electrode material;

[0021] The reaction supporting system is used to supply materials for silicon coating to the first reaction device, and to supply materials for carbon coating to the second reaction device.

[0022] A screening filter is provided between the first reaction device and the second reaction device, and the screening filter is used to screen and filter the silicon-coated particles formed by the first reaction device.

[0023] According to one aspect of the present invention, the reaction supporting system includes a gas supply device, a heating system, a stirring system and a control system. The gas supply device is used to supply silicon source gas and carrier gas to the first reaction device and to supply carbon source gas and carrier gas to the second reaction device. The heating system is used to heat the first reaction device and the second reaction device respectively; the stirring system is used to stir the first reaction device and the second reaction device respectively; and the control system is used to control the operation of the gas supply device, the heating system and the stirring system respectively.

[0024] According to one aspect of the present invention, it also includes a mixed gas preheating system, which is respectively connected to the first reaction device, the second reaction device and the gas supply device, and is used to preheat the gas supplied by the gas supply device.

[0025] According to one aspect of the present invention, it further comprises a vacuum system, wherein the vacuum system is used to evacuate the first reaction device and the second reaction device respectively.

[0026] According to one aspect of the present invention, it further comprises an exhaust gas treatment system, wherein the exhaust gas treatment system is respectively connected to the first reaction device, the second reaction device and the vacuum system.

[0027] The advantages of the implementation of the present invention are as follows: silicon-coated carbon powder is coated with silicon to form silicon-coated particles; the silicon-coated particles are screened and filtered; the screened silicon-coated particles are carbon-coated to obtain silicon-carbon negative electrode materials. During the silicon coating and carbon coating process, forced stirring and airflow are used to ensure the full dispersion of the reactant particles and the formation of fluidization, effectively preventing the accumulation of reaction particles, thereby significantly improving the agglomeration problem of the silicon-carbon negative electrode material, and improving the uniformity and stability of the prepared silicon-carbon negative electrode material. After the silicon-coated particles are completed, a screening filter is used to screen out and filter the agglomerated and over-agglomerated silicon-coated particles, and then the carbon coating process is carried out, which can not only improve production efficiency but also improve quality consistency. The silicon-carbon negative electrode material prepared by this method has more uniform performance, and the components are tightly connected and have strong bonding. During the charge and discharge process, the active material is not easy to fall off, showing excellent cycle stability, and agglomeration is not easy to occur in the finished product. The silicon-carbon negative electrode material prepared by this method has excellent cycle life and stability.

[0028] Furthermore, by setting up multiple small-capacity first reaction devices to silicon-coat the carbon powder, and then concentrating it in a large-capacity second reaction device for carbon coating, it is beneficial to ensure the quality of the silicon-coated particles, realize centralized processing of carbon coating, achieve consistency and stability of silicon-carbon negative electrode materials, and improve production efficiency; by setting up a screening filter, it is possible to effectively remove large particles that are agglomerated and agglomerated, and only the screened silicon-coated particles are subjected to carbon coating reaction, so that both production efficiency and product quality can achieve a qualitative leap; by setting up a reaction supporting system, it is possible to achieve precise control of the gas supply device, reaction temperature, stirring speed and reaction time, and ensure that the equipment, temperature and other conditions are individually and accurately controlled during the silicon deposition and carbon coating processes, so that the entire reaction process is efficient and stable, thereby further improving product quality and production efficiency; by setting up a vacuum system, the gas pressure in the reactor can be accurately controlled and the air can be effectively removed. Through the setting of the tail gas treatment system, environmental pollution is greatly reduced and the environmental protection performance of the overall production process is improved; through the setting of the mixed gas preheating system, not only the decomposition rate of the gas in the reactor is accelerated and the product quality is improved, but also the waste gas emissions are effectively reduced, which has made a positive contribution to reducing environmental pollution; the silicon-carbon negative electrode material reactor provided by the present invention can not only realize continuous production, but also ensure the overall product quality and achieve a significant improvement in production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 This is a flow chart of a method for preparing a silicon-carbon negative electrode material according to the present invention;

[0031] Figure 2 It is a schematic diagram of the layout of a silicon-carbon negative electrode material reactor according to the present invention;

[0032] Figure 3 This is an experimental data table of the silicon-carbon negative electrode material described in the present invention.

[0033] The numbers in the figure are as follows: 1. First reaction device; 2. Screening filter; 3. Second reaction device; 4. Gas supply device; 5. Mixed gas preheating system; 6. Vacuum system; 7. Exhaust gas treatment system; 8. Finished product tank. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] A method for preparing a silicon-carbon negative electrode material comprises the following steps:

[0037] Step S1: Decomposing silicon source gas to deposit silicon on the surface of carbon powder to form silicon-coated particles;

[0038] Step S11: decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form a silicon coating layer;

[0039] The silicon source gas and the carrier gas are introduced into the first reaction device in proportion, and the first reaction device is heated to a preset temperature to decompose the silicon source gas. The decomposed silicon is uniformly deposited on the surface of the carbon powder under the stirring of the stirring system to form a silicon coating layer. The ratio of the silicon source gas to the carrier gas is 1:1 to 1:10; the preset temperature is 400°C to 600°C; the silicon source gas can be a mixture of one or more gases selected from silane, disilane, dimethylsilane, etc.; the carrier gas can be one or more selected from nitrogen or argon, and can also be other inert gases.

[0040] Step S12: decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form uniform silicon-coated particles;

[0041] The ratio of silicon source gas to carrier gas introduced into the first reaction device is increased, the temperature in the first reaction device is adjusted, the reaction time of the first reaction device is adjusted, and a silicon coating layer is formed on the surface of the carbon powder until silicon is deposited on the surface of the carbon powder to form uniform silicon-coated particles. The ratio of silicon source gas to carrier gas is 1:1 to 1:2; the temperature is preferably 600°C; and the reaction time is preferably 5-20 hours.

[0042] Step S2: screening and filtering the silicon-coated particles;

[0043] The silicon-coated particles after the reaction in the first reaction device are input into a screening filter for screening to remove agglomerated and overly large particles.

[0044] Step S3: carbon-coating the screened silicon-coated particles to obtain a silicon-carbon negative electrode material;

[0045] Step S31: carbon-coating the screened silicon-coated particles to form a carbon-coated layer;

[0046] Passing the screened silicon-coated particles into a second reaction device;

[0047] A carbon source gas and a carrier gas are introduced into the second reaction device in proportion, and the second reaction device is heated to a preset temperature to decompose the carbon source gas. Under the stirring of the stirring device, the carbon source gas is decomposed and deposited on the surface of the screened silicon-coated particles by chemical vapor deposition to form a carbon coating layer. The ratio of the carbon source gas to the carrier gas is 1:1 to 1:15; the preset temperature is 600°C to 1200°C. The carbon source gas can be selected from one or more mixed gases including acetylene, propyne, butyne, propylene, etc.; the carrier gas can be selected from one or more of nitrogen or argon, and can also be other inert gases.

[0048] Step S32: carbon-coating the screened silicon-coated particles to form a uniform silicon-carbon negative electrode material;

[0049] The ratio of the carbon source gas and the carrier gas introduced into the second reaction device is regulated, the temperature in the second reaction device is regulated, the reaction time of the second reaction device is regulated, and the particles are fully stirred and dispersed under the stirring of the stirring system. A carbon coating layer is formed on the surface of the sieved silicon-coated particles until the surface of the sieved silicon-coated particles is coated with carbon to form a uniform silicon-carbon negative electrode material. The ratio of the carbon source gas and the carrier gas is 1:1 to 1:2; the temperature is preferably 800°C; and the reaction time is preferably 5-20h.

[0050] A large amount of carrier gas is introduced into the second reaction device, and the carrier gas can be one or more of nitrogen or argon, to transport the uniformly coated silicon-carbon negative electrode material to the finished product tank.

[0051] The advantages of this embodiment include: after the silicon-coated particles are completed, a screening filter is used to screen out the agglomerated and agglomerated silicon-coated particles, and then the carbon coating process is carried out, which can not only improve the production efficiency but also improve the consistency of quality. During the silicon coating and carbon coating process, the use of forced stirring and airflow ensures the full dispersion of the reactant particles and the formation of fluidization, effectively preventing the reaction particles from accumulating below, thereby significantly improving the agglomeration problem of the silicon-carbon negative electrode material, and improving the uniformity and stability of the prepared silicon-carbon negative electrode material. This makes the silicon-carbon negative electrode material after the entire deposition coating reaction have more uniform performance, and the components are tightly connected and have strong bonding. During the charge and discharge process, the active material is not easy to fall off, showing excellent cycle stability. During the charge and discharge process, the active material is not easy to fall off, showing excellent cycle stability, and agglomeration is not easy to occur in the finished product. The silicon-carbon negative electrode material prepared by this method performs well in terms of cycle life and stability.

[0052] Example 2

[0053] A method for preparing a silicon-carbon negative electrode material comprises the following steps:

[0054] Step S1: drying the carbon powder and activating the carbon powder surface activity;

[0055] The carbon powder is introduced into the first reaction device, and the gas inside the entire reactor is evacuated using a vacuum system to a vacuum degree of 10Pa, and a carrier gas is introduced. The carrier gas can be one or more of nitrogen or argon, and can also be other inert gases, and the carbon powder is fully stirred.

[0056] The first reaction device is heated to a preset temperature, and the carbon powder is stirred at the same time to dry and activate the surface activity of the carbon powder. The preset temperature is 200°C to 400°C.

[0057] Step S2: Decomposing silicon source gas to deposit silicon on the surface of carbon powder to form silicon-coated particles;

[0058] Step S21: decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form a silicon coating layer;

[0059] The silicon source gas and the carrier gas are introduced into the first reaction device in proportion, and the first reaction device is heated to a preset temperature to decompose the silicon source gas. The decomposed silicon is uniformly deposited on the surface of the carbon powder under the stirring of the stirring system to form a silicon coating layer. The ratio of the silicon source gas to the carrier gas is 1:1 to 1:10; the preset temperature is 400°C to 600°C; the silicon source gas can be a mixture of one or more gases selected from silane, disilane, dimethylsilane, etc.; the carrier gas can be one or more selected from nitrogen or argon, and can also be other inert gases.

[0060] Step S22: decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form uniform silicon-coated particles;

[0061] The ratio of silicon source gas to carrier gas introduced into the first reaction device is increased, the temperature in the first reaction device is adjusted, the reaction time of the first reaction device is adjusted, and a silicon coating layer is formed on the surface of the carbon powder until silicon is deposited on the surface of the carbon powder to form uniform silicon-coated particles. The ratio of silicon source gas to carrier gas is 1:1 to 1:2; the temperature is preferably 600°C; and the reaction time is preferably 5-20 hours.

[0062] Step S3: screening and filtering the silicon-coated particles;

[0063] The silicon-coated particles after the reaction in the first reaction device are input into a screening filter for screening to remove agglomerated and overly large particles.

[0064] Step S4: carbon-coating the screened silicon-coated particles to obtain a silicon-carbon negative electrode material;

[0065] Step S41: carbon-coating the screened silicon-coated particles to form a carbon-coated layer;

[0066] Passing the screened silicon-coated particles into a second reaction device;

[0067] A carbon source gas and a carrier gas are introduced into the second reaction device in proportion, and the second reaction device is heated to a preset temperature to decompose the carbon source gas. Under the stirring of the stirring device, the carbon source gas is decomposed and deposited on the surface of the screened silicon-coated particles by chemical vapor deposition to form a carbon coating layer. The ratio of the carbon source gas to the carrier gas is 1:1 to 1:15; the preset temperature is 600°C to 1200°C. The carbon source gas can be selected from one or more mixed gases including acetylene, propyne, butyne, propylene, etc.; the carrier gas can be selected from one or more of nitrogen or argon, and can also be other inert gases.

[0068] Step S42: carbon-coating the screened silicon-coated particles to form a uniform silicon-carbon negative electrode material;

[0069] The ratio of the carbon source gas and the carrier gas introduced into the second reaction device is regulated, the temperature in the second reaction device is regulated, the reaction time of the second reaction device is regulated, and the particles are fully stirred and dispersed under the stirring of the stirring system. A carbon coating layer is formed on the surface of the sieved silicon-coated particles until the surface of the sieved silicon-coated particles is coated with carbon to form a uniform silicon-carbon negative electrode material. The ratio of the carbon source gas and the carrier gas is 1:1 to 1:2; the temperature is preferably 800°C; and the reaction time is preferably 5-20h.

[0070] A large amount of carrier gas is introduced into the second reaction device, and the carrier gas can be one or more of nitrogen or argon, to transport the uniformly coated silicon-carbon negative electrode material to the finished product tank.

[0071] The advantages of this embodiment include: by drying the carbon powder and performing a surface active activation treatment on the carbon powder, impurities and oxides on the surface of the carbon powder can be removed, the surface quality can be improved, and it is easier to chemically adsorb and interfacially bind with silicon, which helps to form more uniform and dense silicon-coated particles, thereby improving the weather resistance and durability of the silicon-carbon negative electrode material; by forced stirring and airflow, the reactant particles are fully dispersed and fluidized, and the reaction particles are effectively prevented from accumulating, thereby significantly improving the agglomeration problem of the silicon-carbon negative electrode material, and improving the uniformity and stability of the prepared silicon-carbon negative electrode material. After the silicon-coated particles are completed, the agglomerated and agglomerated silicon-coated particles are screened out by a screening filter, and then the carbon coating process is carried out, which can not only improve the production efficiency but also improve the consistency of quality. The silicon-carbon negative electrode material prepared by this method has more uniform performance, and the components are closely connected and have strong bonding. During the charge and discharge process, the active material is not easy to fall off, showing excellent cycle stability and it is not easy to agglomerate in the finished product. The silicon-carbon negative electrode material prepared by this method performs well in terms of cycle life and stability.

[0072] Example 3

[0073] A method for preparing a silicon-carbon negative electrode material comprises the following steps:

[0074] Step S1: drying the carbon powder and activating the carbon powder surface activity;

[0075] The carbon powder is introduced into the first reaction device, and the gas inside the entire reactor is evacuated using a vacuum system to a vacuum degree of 10Pa, and a carrier gas is introduced. The carrier gas can be one or more of nitrogen or argon, and can also be other inert gases, and the carbon powder is fully stirred.

[0076] The first reaction device is heated to a preset temperature, and the carbon powder is stirred at the same time to dry and activate the surface activity of the carbon powder. The preset temperature is 200°C to 400°C.

[0077] Step S2: Decomposing silicon source gas to deposit silicon on the surface of carbon powder to form silicon-coated particles;

[0078] Step S21: decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form a silicon coating layer;

[0079] The silicon source gas and the carrier gas are introduced into the first reaction device in proportion, and the first reaction device is heated to a preset temperature to decompose the silicon source gas. The decomposed silicon is uniformly deposited on the surface of the carbon powder under the stirring of the stirring system to form a silicon coating layer. The ratio of the silicon source gas to the carrier gas is 1:1 to 1:10; the preset temperature is 400°C to 600°C; the silicon source gas can be a mixture of one or more gases selected from silane, disilane, dimethylsilane, etc.; the carrier gas can be one or more selected from nitrogen or argon, and can also be other inert gases.

[0080] Step S22: decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form uniform silicon-coated particles;

[0081] The ratio of silicon source gas to carrier gas introduced into the first reaction device is increased, the temperature in the first reaction device is adjusted, the reaction time of the first reaction device is adjusted, and a silicon coating layer is formed on the surface of the carbon powder until silicon is deposited on the surface of the carbon powder to form uniform silicon-coated particles. The ratio of silicon source gas to carrier gas is 1:1 to 1:2; the temperature is preferably 600°C; and the reaction time is preferably 5-20 hours.

[0082] Step S3: the step of coating carbon powder with silicon by decomposing the silicon source gas to form silicon-coated particles is repeated multiple times;

[0083] The ratio of the silicon source gas and the carrier gas introduced into the first reaction device is regulated, the temperature in the first reaction device is regulated, and the reaction time of the first reaction device is regulated to form a silicon coating layer on the surface of the carbon powder until uniform silicon-coated particles are formed on the surface of the carbon powder. The ratio of the silicon source gas and the carrier gas is 1:1 to 1:2; the temperature is preferably 600°C; and the reaction time is preferably 5-20 hours.

[0084] Step S4: screening and filtering the silicon-coated particles;

[0085] The deposited coated particles after the reaction in the first reaction device are input into a screening filter for screening to remove agglomerated and overly large reaction particles.

[0086] Step S5: carbon-coating the screened silicon-coated particles to obtain a silicon-carbon negative electrode material;

[0087] Step S51: carbon-coating the screened silicon-coated particles to form a carbon-coated layer;

[0088] Passing the screened silicon-coated particles into a second reaction device;

[0089] A carbon source gas and a carrier gas are introduced into the second reaction device in proportion, and the second reaction device is heated to a preset temperature to decompose the carbon source gas. Under the stirring of the stirring device, the carbon source gas is decomposed and deposited on the surface of the screened silicon-coated particles by chemical vapor deposition to form a carbon coating layer. The ratio of the carbon source gas to the carrier gas is 1:1 to 1:15; the preset temperature is 600°C to 1200°C. The carbon source gas can be selected from one or more mixed gases including acetylene, propyne, butyne, propylene, etc.; the carrier gas can be selected from one or more of nitrogen or argon, and can also be other inert gases.

[0090] Step S52: carbon-coating the screened silicon-coated particles to form a uniform silicon-carbon negative electrode material;

[0091] The ratio of the carbon source gas and the carrier gas introduced into the second reaction device is regulated, the temperature in the second reaction device is regulated, the reaction time of the second reaction device is regulated, and the particles are fully stirred and dispersed under the stirring of the stirring system. A carbon coating layer is formed on the surface of the sieved silicon-coated particles until the surface of the sieved silicon-coated particles is coated with carbon to form a uniform silicon-carbon negative electrode material. The ratio of the carbon source gas and the carrier gas is 1:1 to 1:2; the temperature is preferably 800°C; and the reaction time is preferably 5-20h.

[0092] Step S6: performing carbon coating on the screened silicon-coated particles to obtain silicon-carbon negative electrode materials multiple times;

[0093] The ratio of the carbon source gas and the carrier gas introduced into the second reaction device is regulated, the temperature in the second reaction device is regulated, and the reaction time of the second reaction device is regulated to form a carbon coating layer on the surface of the sieved silicon-coated particles, and this deposition stage is repeated many times until a silicon-carbon negative electrode material with a uniform carbon coating layer is formed on the surface of the silicon-coated particles. The ratio of the carbon source gas and the carrier gas is 1:1 to 1:2; the temperature is preferably 800°C; and the reaction time is preferably 5-20 hours.

[0094] A large amount of carrier gas is introduced into the second reaction device, and the carrier gas can be one or more of nitrogen or argon, to transport the uniformly coated silicon-carbon negative electrode material to the finished product tank.

[0095] The advantages of this embodiment include: the steps of forming silicon-coated particles by decomposing silicon source gas to deposit silicon on the surface of carbon powder and carbon-coating the screened silicon-coated particles to obtain silicon-carbon negative electrode materials are performed multiple times respectively. Through multiple deposition and coating reactions, the interfacial bonding force between silicon and carbon can be significantly enhanced, and the thickness of the silicon coating layer and the carbon coating layer can be increased, so that the silicon coating layer and the carbon coating layer become more uniform and dense, thereby helping to improve the performance and stability of the silicon-carbon negative electrode material. The stirring and airflow ensure that the reactant particles are fully dispersed and fluidized, effectively preventing the accumulation of reaction particles, thereby significantly improving the agglomeration problem of the silicon-carbon negative electrode material, and improving the uniformity and stability of the prepared silicon-carbon negative electrode material. After the silicon-coated particles are completed, the agglomerated and agglomerated silicon-coated particles are screened out by a screening filter, and then the carbon coating process is carried out, which can not only improve the production efficiency but also improve the consistency of quality. The silicon-carbon negative electrode material prepared by this method has more uniform performance, and the components are tightly connected and have strong bonding. During the charge and discharge process, the active material is not easy to fall off, showing excellent cycle stability, and it is not easy to agglomerate in the finished product. The silicon-carbon negative electrode material prepared by this method performs well in terms of cycle life and stability.

[0096] Example 4

[0097] A method for preparing a silicon-carbon negative electrode material comprises the following steps:

[0098] Step S1: drying the carbon powder and activating the carbon powder surface activity;

[0099] The carbon powder is introduced into the first reaction device, and the gas inside the entire device is evacuated using a vacuum system to a vacuum degree of 10Pa, and a carrier gas is introduced. The carrier gas can be one or more of nitrogen or argon, and can also be other inert gases, and the carbon powder is fully stirred.

[0100] The first reaction device is heated to a preset temperature, and the carbon powder is stirred at the same time to dry and activate the surface activity of the carbon powder. The preset temperature is 200°C to 400°C.

[0101] Step S2: Decomposing silicon source gas to deposit silicon on the surface of carbon powder to form silicon-coated particles;

[0102] Step S21: decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form a silicon coating layer;

[0103] The silicon source gas and the carrier gas are introduced into the first reaction device in proportion, and the first reaction device is heated to a preset temperature to decompose the silicon source gas. The decomposed silicon is uniformly deposited on the surface of the carbon powder under the stirring of the stirring system to form a silicon coating layer. The ratio of the silicon source gas to the carrier gas is 1:1 to 1:10; the preset temperature is 400°C to 600°C; the silicon source gas can be a mixture of one or more gases selected from silane, disilane, dimethylsilane, etc.; the carrier gas can be one or more selected from nitrogen or argon, and can also be other inert gases.

[0104] Step S22: decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form uniform silicon-coated particles;

[0105] The ratio of silicon source gas to carrier gas introduced into the first reaction device is increased, the temperature in the first reaction device is adjusted, the reaction time of the first reaction device is adjusted, and a silicon coating layer is formed on the surface of the carbon powder until silicon is deposited on the surface of the carbon powder to form uniform silicon-coated particles. The ratio of silicon source gas to carrier gas is 1:1 to 1:2; the temperature is preferably 600°C; and the reaction time is preferably 5-20 hours.

[0106] S3: coating carbon powder with silicon in multiple batches to form uniform silicon-coated particles;

[0107] The first reaction device is used to silicon-coat the carbon powder in multiple batches to form uniform silicon-coated particles. Alternatively, multiple first reaction devices are used in parallel to silicon-coat the carbon powder to form uniform silicon-coated particles, and the silicon-coated particles are carbon-coated after the multiple batches of silicon-coated particles are concentrated together.

[0108] Step S4: screening and filtering the silicon-coated particles;

[0109] The silicon-coated particles collected in multiple batches are input into a screening filter for screening to remove agglomerated and overly large reaction particles.

[0110] Step S5: centrally carbon-coating the screened silicon-coated particles to obtain silicon-carbon negative electrode materials;

[0111] Step S51: centrally carbon-coating the screened silicon-coated particles to form a carbon-coated layer;

[0112] The sieved silicon-coated particles are collected together and introduced into a second reaction device;

[0113] The carbon source gas and the carrier gas are introduced into the second reaction device in proportion, and the second reaction device is heated to a preset temperature to decompose the carbon source gas. Under the stirring of the stirring device, the carbon source gas is decomposed and deposited on the surface of the screened silicon-coated particles by chemical vapor deposition to form a carbon coating layer. The ratio of the carbon source gas to the carrier gas is 1:1 to 1:15; the preset temperature is 600°C to 1200°C. The carbon source gas can be selected from one or more mixed gases including acetylene, propyne, butyne, propylene, etc.; the carrier gas can be selected from one or more of nitrogen or argon, and can also be other inert gases.

[0114] Step S52: carbon-coating the screened silicon-coated particles to form a uniform silicon-carbon negative electrode material;

[0115] Regulate the ratio of the carbon source gas and the carrier gas introduced into the second reaction device, regulate the temperature in the second reaction device, regulate the reaction time of the second reaction device, and

[0116] Under stirring, the particles are fully stirred and dispersed. A carbon coating layer is formed on the surface of the silicon-coated particles until the surface of the screened silicon-coated particles is coated with carbon to form a uniform silicon-carbon negative electrode material. The ratio of the carbon source gas to the carrier gas is 1:1 to 1:2; the temperature is preferably 800°C; and the reaction time is preferably 5-20 hours.

[0117] A large amount of carrier gas is introduced into the second reaction device, and the carrier gas can be one or more of nitrogen or argon, to transport the uniformly coated silicon-carbon negative electrode material to the finished product tank.

[0118] The advantages of this embodiment include: the steps of forming silicon-coated particles by decomposing silicon source gas to deposit silicon on the surface of carbon powder and carbon-coating the screened silicon-coated particles to obtain silicon-carbon negative electrode materials are carried out in two steps, so that the silicon deposition coating and the carbon deposition coating become more uniform and dense, which helps to improve the capacity and high specific performance of the silicon-carbon negative electrode material. The full dispersion and fluidization of the reactant particles are ensured by the action of forced stirring and airflow, and the accumulation of reaction particles is effectively prevented, thereby significantly improving the agglomeration problem of the silicon-carbon negative electrode material, and improving the uniformity and stability of the prepared silicon-carbon negative electrode material. After the silicon-coated particles are completed, the caking and agglomerated silicon-coated particles are screened out by a screening filter, and then the carbon coating process is carried out, which can not only improve the production efficiency but also improve the consistency of quality. The silicon-carbon negative electrode material prepared by this method has more uniform performance, and the components are tightly connected and have strong bonding. The process of decomposing silicon source gas in multiple batches to deposit silicon on the surface of carbon powder to form uniform silicon-coated particles and then concentrating on carbon coating the sieved silicon-coated particles is beneficial to ensuring the quality of silicon-coated particles. The carbon coating reaction is easier to concentrate, achieving the consistency and stability of silicon-carbon negative electrode materials, and at the same time, improving production efficiency. During the charge and discharge process, the active material is not easy to fall off, showing excellent cycle stability, and agglomeration is not easy to occur in the finished product. The silicon-carbon negative electrode material prepared by this method performs well in terms of cycle life and stability.

[0119] Example 5

[0120] A method for preparing a silicon-carbon negative electrode material comprises the following steps:

[0121] Step S1: drying the carbon powder and activating the carbon powder surface activity;

[0122] The carbon powder is introduced into the first reaction device, and the gas inside the entire reactor is evacuated using a vacuum system to a vacuum degree of 10Pa, and a carrier gas is introduced. The carrier gas can be one or more of nitrogen or argon, and can also be other inert gases, and the carbon powder is fully stirred.

[0123] The first reaction device is heated to a preset temperature, and the carbon powder is stirred at the same time to dry and activate the surface activity of the carbon powder. The preset temperature is 200°C to 400°C.

[0124] Step S2: Decomposing silicon source gas to deposit silicon on the surface of carbon powder to form silicon-coated particles;

[0125] Step S21: decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form a silicon coating layer;

[0126] The silicon source gas and the carrier gas are introduced into the first reaction device in proportion, and the first reaction device is heated to a preset temperature to decompose the silicon source gas. The decomposed silicon is uniformly deposited on the surface of the carbon powder under the stirring of the stirring system to form a silicon coating layer. The ratio of the silicon source gas to the carrier gas is 1:1 to 1:10; the preset temperature is 400°C to 600°C; the silicon source gas can be a mixture of one or more gases selected from silane, disilane, dimethylsilane, etc.; the carrier gas can be one or more selected from nitrogen or argon, and can also be other inert gases.

[0127] Step S22: decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form uniform silicon-coated particles;

[0128] Increase the ratio of silicon source gas and carrier gas introduced into the first reaction device, adjust the temperature in the first reaction device, adjust the reaction time of the first reaction device, and form a silicon coating layer on the surface of the carbon powder until silicon is deposited on the surface of the carbon powder to form uniform silicon-coated particles.

[0129] Step S3: the step of depositing silicon on the surface of the carbon powder to form uniform silicon-coated particles by decomposing the silicon source gas is repeated multiple times;

[0130] The ratio of the silicon source gas and the carrier gas introduced into the first reaction device is regulated, the temperature in the first reaction device is regulated, and the reaction time of the first reaction device is regulated to form a silicon deposition layer on the surface of the carbon powder until silicon is deposited on the surface of the carbon powder to form uniform silicon-coated particles. The ratio of the silicon source gas and the carrier gas is 1:1 to 1:2; the temperature is preferably 600°C; and the reaction time is preferably 5-20 hours.

[0131] Step S4: screening and filtering the silicon-coated particles;

[0132] The silicon-coated particles after the reaction in the first reaction device are input into a screening filter for screening to remove the agglomerated and overly large reaction particles.

[0133] Step S5: carbon-coating the screened silicon-coated particles to obtain a silicon-carbon negative electrode material;

[0134] Step S51: carbon-coating the screened silicon-coated particles to form a carbon-coated layer;

[0135] Passing the screened silicon-coated particles into a second reaction device;

[0136] The carbon source gas and the carrier gas are introduced into the second reaction device in proportion, and the second reaction device is heated to a preset temperature to decompose the carbon source gas. Under the stirring of the stirring device, the carbon source gas is decomposed and deposited on the surface of the screened silicon-coated particles by chemical vapor deposition to form a carbon coating layer. The ratio of the carbon source gas to the carrier gas is 1:1 to 1:15; the preset temperature is 600°C to 1200°C. The carbon source gas can be selected from one or more mixed gases including acetylene, propyne, butyne, propylene, etc.; the carrier gas can be selected from one or more of nitrogen or argon, and can also be other inert gases.

[0137] Step S52: carbon-coating the screened silicon-coated particles to form a uniform silicon-carbon negative electrode material;

[0138] The ratio of the carbon source gas and the carrier gas introduced into the second reaction device is regulated, the temperature in the second reaction device is regulated, the reaction time of the second reaction device is regulated, and the particles are fully stirred and dispersed under the stirring of the stirring system. A carbon coating layer is formed on the surface of the sieved silicon-coated particles until the surface of the sieved silicon-coated particles is coated with carbon to form a uniform silicon-carbon negative electrode material.

[0139] Step S6: performing carbon coating on the screened silicon-coated particles to form a uniform silicon-carbon negative electrode material for multiple times;

[0140] The ratio of the carbon source gas and the carrier gas introduced into the second reaction device is regulated, the temperature in the second reaction device is regulated, and the reaction time of the second reaction device is regulated to form a carbon deposition layer on the surface of the sieved silicon-coated particles until carbon is deposited on the surface of the silicon-coated particles to form a uniform silicon-carbon negative electrode material. The ratio of the carbon source gas and the carrier gas is 1:1 to 1:2; the temperature is preferably 800°C; and the reaction time is preferably 5-20 hours.

[0141] A large amount of carrier gas is introduced into the second reaction device, and the carrier gas can be one or more of nitrogen or argon, to transport the uniformly coated silicon-carbon negative electrode material to the finished product tank.

[0142] Step S7: Treating the exhaust gas

[0143] By adding an exhaust gas treatment system to the reactor, the exhaust gas treatment system is used to treat the gas in the reactor, and the treatment steps include one or more of exhaust gas collection, exhaust gas pretreatment, harmful substance adsorption, catalytic oxidation and combustion. The silicon source gas, carbon source gas, carrier gas and their decomposition products in the above steps are treated by the exhaust gas treatment system and discharged after meeting the environmental emission standards.

[0144] The advantages of this embodiment include: the gas in the production process of silicon-carbon negative electrode materials is collected and treated by the tail gas treatment system, thereby significantly reducing the emission of waste gas, helping to reduce pollution to the environment, improve air quality, and reduce damage to the ecosystem. The stirring and airflow ensure that the reactant particles are fully dispersed and fluidized, effectively preventing the accumulation of reaction particles, thereby significantly improving the agglomeration problem of silicon-carbon negative electrode materials, and improving the uniformity and stability of the prepared silicon-carbon negative electrode materials. After the silicon-coated particles are completed, a screening filter is used to screen out the agglomerated and overagglomerated silicon-coated particles, and then the carbon coating process is carried out, which can not only improve production efficiency but also improve quality consistency. The silicon-carbon negative electrode material prepared by this method has more uniform performance, and the components are tightly connected and have strong bonding. During the charge and discharge process, the active material is not easy to fall off, showing excellent cycle stability, and agglomeration is not easy to occur in the finished product. The silicon-carbon negative electrode material prepared by this method performs well in terms of cycle life and stability.

[0145] Example 6

[0146] like Figure 1As shown, a silicon-carbon negative electrode material reactor comprises a first reaction device 1 for decomposing silicon source gas to deposit silicon on the surface of carbon powder to form silicon-coated particles and a second reaction device 3 for carbon-coating the silicon-coated particles to form silicon-carbon negative electrode materials. The first reaction device 1 is connected to the second reaction device 3; and also comprises a gas supply device 4, which is respectively connected to the first reaction device 1 and the second reaction device 3, and supplies gas to the first reaction device 1 and the second reaction device 3. The gas supply device 4 is provided with an air intake valve for controlling the on-off of the gas. Preferably, multiple air intake valves can be provided to control the on-off of different gases. The gas can be a carrier gas, a silicon source gas, a carbon source gas, etc. The reactor is also provided with a heating system, a stirring system and a control system. The heating system can heat the first reaction device 1 and the second reaction device 3 respectively, the stirring system can stir the reactants in the first reaction device 1 and the second reaction device 3 respectively, and the control system can control the operation of the gas supply device, the heating system and the stirring system respectively. The control system can control the gas, heating temperature and stirring speed required in the first reaction device 1 and the second reaction device 3 respectively, so that the first reaction device 1 and the second reaction device 3 can control the temperature, gas and stirring speed separately. Preferably, the heating system and stirring system are both arranged inside the first reaction device 1, and the heating system and stirring system are both arranged inside the second reaction device 3. The control system is used to control the heating temperature of the heating system and the stirring speed of the stirring system as well as the gas content and proportion of the gas supply device. A screening filter 2 is arranged between the first reaction device 1 and the second reaction device 3, and the silicon-coated particles that have reacted completely in the first reaction device 1 are transported to the screening filter 2 for screening, and the screened silicon-coated particles are transported to the second reaction device 3 for carbon coating. The screening filter mainly screens the agglomerated and agglomerated particles to prevent them from further growing and adhering to the inside of the reactor in the subsequent second reaction device 3, so as to ensure the smooth progress of the subsequent reaction. Preferably, a valve is arranged between the first reaction device 1 and the screening filter 2 to control the input of the silicon-coated particles into the screening filter 2. Preferably, the first reaction device 1 can be provided with at least one small-capacity first reaction device 1, and the second reaction device is configured with a large capacity. The multiple first reaction devices are respectively connected to the second reaction device 3, and the silicon-coated particles in at least one first reaction device 1 are concentrated in the second reaction device 3 for centralized carbon coating. The small capacity of the first reaction device 1 helps to ensure the quality of the silicon-coated particles and ensure the consistency and stability of the product. The carbon coating reaction is easier to concentrate and is more suitable for being carried out in a large-capacity reactor, so that the silicon-coated particles generated by the previous multiple small first reaction devices can be centrally processed to achieve efficient carbon coating, thereby significantly improving production efficiency.

[0147] In practical applications, the silicon-carbon negative electrode material reactor also includes a vacuum system 6, and the first reaction device 1 and the second reaction device 3 are respectively connected to the vacuum system 6, and the vacuum system 6 is used to evacuate the first reaction device 1 and the second reaction device 3 respectively.

[0148] In practical applications, the silicon-carbon negative electrode material reactor also includes an exhaust gas treatment system 7, and the first reaction device 1 and the second reaction device 3 are respectively connected to the exhaust gas treatment system 7. Preferably, the vacuum system 6 is arranged between the exhaust gas treatment system 7 and the first reaction device 1 and the second reaction device 3. The exhaust gas treatment system 7 can treat the exhaust gas generated after the reaction between the first reaction device 1 and the second reaction device 3 to prevent environmental pollution.

[0149] In practical applications, the silicon-carbon negative electrode material reactor further includes a finished product tank 8, which is connected to the second reaction device 3. The prepared silicon-carbon negative electrode material is transported from the second reaction device 3 to the finished product tank 8. Preferably, the second reaction device 3 is connected to the finished product tank 8 through a discharge pipe, and a discharge valve is provided on the discharge pipe.

[0150] The working principle is briefly described as follows:

[0151] First, carbon powder is introduced into the first reaction device 1. Subsequently, the vacuum system 6 is used to evacuate the gas in the first reaction device 1 and the second reaction device 3. Next, the control system controls the gas supply device 4 to fill with carrier gas. At this time, the heating system and the stirring system are started under the control of the control system to gradually dry the carbon powder and activate its surface activity. After that, the gas supply device 4 is controlled to fill with silicon source gas and carrier gas in a certain proportion. The control system will adjust the temperature of the heating system so that the silicon source gas decomposes and deposits on the surface of the carbon powder, thereby generating silicon-coated particles. After the generation of silicon-coated particles is completed, the silicon-coated particles will be transported to the screening filter 2 for screening. The screened silicon-coated particles will be sent to the second reaction device. At the same time, the control system in the second reaction device starts the heating system and the stirring system, and fills the carbon source gas through the gas supply device 4, and the carbon source gas will decompose and deposit on the surface of the silicon-coated particles to form a carbon coating layer. Finally, the prepared material will be transported from the second reaction device 3 to the finished product tank 8. During the whole process, the tail gas treatment system 7 will be started at the same time to treat the gas generated during the reaction and then discharge it.

[0152] Advantages of this embodiment:

[0153] By setting up multiple small-capacity first reaction devices and large-capacity second reaction devices, the product quality and production efficiency can be significantly improved, and a stable and continuous production process can be achieved; by setting up a screening filter, the large particles that are agglomerated and agglomerated can be effectively removed before the carbon coating reaction is carried out, thereby optimizing the carbon coating reaction effect and improving the production efficiency and product quality; by setting up a reaction supporting system, the gas supply device, reaction temperature, stirring speed and reaction time can be accurately controlled to ensure the high efficiency and stability of the reaction process, thereby further improving the product quality and production efficiency; by setting up a vacuum system, the gas pressure in the reactor can be accurately controlled and the air can be effectively removed. By setting up the tail gas treatment system, environmental pollution is effectively reduced and the environmental protection performance of the overall production process is improved; the reactor of this embodiment can not only achieve continuous production, but also ensure the overall product quality and achieve a significant improvement in production efficiency.

[0154] Example 7

[0155] like Figure 1As shown, a silicon-carbon negative electrode material reactor comprises a first reaction device 1 for decomposing silicon source gas to deposit silicon on the surface of carbon powder to form silicon-coated particles and a second reaction device 3 for carbon-coating the silicon-coated particles to form silicon-carbon negative electrode materials. The first reaction device 1 is connected to the second reaction device 3; and also comprises a gas supply device 4, which is respectively connected to the first reaction device 1 and the second reaction device 3, and supplies gas to the first reaction device 1 and the second reaction device 3. The gas supply device 4 is provided with an air intake valve for controlling the on-off of the gas. Preferably, multiple air intake valves can be provided to control the on-off of different gases. The gas can be a carrier gas, a silicon source gas, a carbon source gas, etc. The reactor is also provided with a heating system, a stirring system and a control system. The heating system can heat the first reaction device 1 and the second reaction device 3 respectively, the stirring system can stir the reactants in the first reaction device 1 and the second reaction device 3 respectively, and the control system can control the operation of the gas supply device, the heating system and the stirring system respectively. The control system can control the gas, heating temperature and stirring speed required in the first reaction device 1 and the second reaction device 3 respectively, so that the first reaction device 1 and the second reaction device 3 can control the temperature, gas and stirring speed separately. Preferably, the heating system and stirring system are both arranged inside the first reaction device 1, and the heating system and stirring system are both arranged inside the second reaction device 3. The control system is used to control the heating temperature of the heating system and the stirring speed of the stirring system as well as the gas content and proportion of the gas supply device. A screening filter 2 is arranged between the first reaction device 1 and the second reaction device 3, and the silicon-coated particles that have reacted completely in the first reaction device 1 are transported to the screening filter 2 for screening, and the screened silicon-coated particles are transported to the second reaction device 3 for carbon coating. The screening filter mainly screens the agglomerated and agglomerated particles to prevent them from further growing and adhering to the inside of the reactor in the subsequent second reaction device 3, so as to ensure the smooth progress of the subsequent reaction. Preferably, a valve is arranged between the first reaction device 1 and the screening filter 2 to control the input of the silicon-coated particles into the screening filter 2. Preferably, the first reaction device 1 can be provided with at least one small-capacity first reaction device 1, and the second reaction device is configured with a large capacity, and the plurality of first reaction devices are respectively connected to the second reaction device 3, and the silicon-coated particles in at least one first reaction device 1 are concentrated in the second reaction device 3 for centralized carbon coating. The second reaction device is configured with a large capacity, and the small capacity of the first reaction device 1 helps to ensure the quality of the silicon-coated particles and ensure the consistency and stability of the product.The carbon coating reaction is easier to concentrate and is more suitable to be carried out in a large-capacity reactor, so that the silicon-coated particles generated by the previous multiple small-capacity first reaction devices can be centrally processed to achieve efficient carbon coating, thereby significantly improving production efficiency.

[0156] In practical applications, the silicon-carbon negative electrode material reactor also includes a vacuum system 6, and the first reaction device 1 and the second reaction device 3 are respectively connected to the vacuum system 6, and the vacuum system 6 is used to evacuate the first reaction device 1 and the second reaction device 3.

[0157] In practical applications, the silicon-carbon negative electrode material reactor also includes an exhaust gas treatment system 7, and the first reaction device 1 and the second reaction device 3 are respectively connected to the exhaust gas treatment system 7. Preferably, the vacuum system 6 is arranged between the exhaust gas treatment system 7 and the first reaction device 1 and the second reaction device 3. The exhaust gas treatment system 7 can treat the exhaust gas generated after the reaction between the first reaction device 1 and the second reaction device 3 to prevent environmental pollution.

[0158] In practical applications, the silicon-carbon negative electrode material reactor further includes a gas mixing preheating system 5, the first reaction device 1 and the second reaction device 3 are respectively connected to the gas mixing preheating system 5, and the gas mixing preheating system 5 is connected to the gas supply device 4. The gas mixing preheating system 5 can mix the gas input by the gas supply device 4 and preheat it to the required temperature, which helps to speed up the decomposition rate of the gas in the reactor, thereby improving product quality and effectively reducing waste gas emissions, which not only improves production efficiency, but also makes a positive contribution to reducing environmental pollution.

[0159] In practical applications, the silicon-carbon negative electrode material reactor further includes a finished product tank 8, which is connected to the second reaction device 3. The prepared silicon-carbon negative electrode material is transported from the second reaction device 3 to the finished product tank 8. Preferably, the second reaction device 3 is connected to the finished product tank 8 through a discharge pipe, and a discharge valve is provided on the discharge pipe.

[0160] The working principle is briefly described as follows:

[0161] First, the carbon powder is introduced into the first reaction device 1. Subsequently, the vacuum system 6 is used to evacuate the gas in the first reaction device 1 and the second reaction device 3. Then, the carrier gas is filled through the gas supply device 4. At this time, the control system starts the heating system and the stirring system to gradually dry the carbon powder and activate its surface activity. After that, the silicon source gas and the carrier gas are filled in a certain proportion, and after the mixed preheating is completed under the mixed gas preheating system, they are passed into the first reaction device. The control system will regulate the temperature of the heating system so that the silicon source gas decomposes and deposits on the surface of the carbon powder to generate silicon-coated particles. After the generation of the silicon-coated particles is completed, these particles will be transported to the screening filter 2 for screening. The screened silicon-coated particles will be sent to the second reaction device. At the same time, the control system in the second reaction device starts the heating system and the stirring system, and fills the carbon source gas through the gas supply device 4, and the carbon source gas will decompose and deposit on the surface of the silicon-coated particles to form a carbon coating. Finally, the prepared material will be transported from the second reaction device 3 to the finished product tank 8. During the whole process, the tail gas treatment system 7 will be started at the same time to treat the gas generated during the reaction and then discharge it.

[0162] Advantages of this embodiment:

[0163] By setting up multiple small-capacity first reaction devices and large-capacity second reaction devices, the product quality and production efficiency can be significantly improved, and a stable and continuous production process can be achieved; by setting up a screening filter, the large particles of agglomeration and aggregation can be effectively removed before the carbon coating reaction is carried out, thereby optimizing the carbon coating reaction effect, and making a qualitative leap in production efficiency and product quality; by independently setting up a heating system, a stirring system and a control system in the first reaction device and the second reaction device, precise regulation of reaction temperature, stirring speed and reaction time can be achieved, ensuring that the equipment, temperature and other conditions are individually and precisely controlled during the silicon coating and carbon coating processes, so that the entire reaction process is efficient and stable, thereby further improving product quality and production efficiency; by setting up a vacuum system, the gas pressure in the reactor can be accurately controlled and air can be effectively removed. Through the setting of the exhaust gas treatment system, environmental pollution is greatly reduced and the environmental protection performance of the overall production process is improved; through the setting of the mixed gas preheating system, not only the decomposition rate of the gas in the reactor is accelerated and the product quality is improved, but also the waste gas emissions are effectively reduced, making a positive contribution to reducing environmental pollution; the reactor of this embodiment can not only realize continuous production, but also ensure the overall product quality and achieve a significant improvement in production efficiency.

[0164] Example 8

[0165] A method for preparing a silicon-carbon negative electrode material, which is illustrated by the device provided in Example 8, includes the following steps:

[0166] Step S1: introducing carbon powder into a first reaction device;

[0167] The carbon powder is introduced into multiple first reaction devices 1 respectively. After the gas inside the entire reactor is evacuated using the vacuum system 6, the vacuum degree is 10Pa, the air inlet valve on the gas supply device 4 is opened, and the carrier gas is introduced. The carrier gas can be one or more of nitrogen or argon, and can also be other inert gases, to fully stir the carbon powder.

[0168] Step S2: drying the carbon powder and activating the carbon powder surface.

[0169] The heating system heats each first reaction device 1 to a preset temperature, and stirs the carbon powder to dry and activate the surface activity of the carbon powder. The preset temperature is 200°C to 400°C.

[0170] Step S3: Decomposing silicon source gas to deposit silicon on the surface of carbon powder to form silicon-coated particles;

[0171] Step S31: decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form a silicon coating layer;

[0172] The silicon source gas and the carrier gas are introduced into a plurality of first reaction devices in proportion, and each first reaction device 1 is heated to a preset temperature to decompose the silicon source gas. The decomposed silicon is uniformly deposited on the surface of the carbon powder under the stirring of the stirring system to form a silicon coating layer. The ratio of the silicon source gas to the carrier gas is 1:1 to 1:10; the preset temperature is 400°C to 600°C; the silicon source gas can be a mixture of one or more gases such as silane, disilane, and dimethylsilane; the carrier gas can be one or more of nitrogen or argon, and can also be other inert gases.

[0173] Step S32: decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form uniform silicon-coated particles;

[0174] Increase the ratio of silicon source gas and carrier gas introduced into each first reaction device 1, adjust the temperature in each first reaction device 1, adjust the reaction time of the first reaction device 1, and form a silicon coating layer on the surface of the carbon powder until silicon is deposited on the surface of the carbon powder to form uniform silicon-coated particles.

[0175] Step S4: the step of depositing silicon on the surface of the carbon powder to form silicon-coated particles by decomposing the silicon source gas is repeated multiple times;

[0176] The ratio of silicon source gas to carrier gas introduced into each first reaction device is regulated, the temperature in the first reaction device 1 is regulated, and the reaction time of the first reaction device 1 is regulated to form a silicon coating layer on the surface of the carbon powder until silicon is deposited on the surface of the carbon powder to form uniform silicon-coated particles. The ratio of silicon source gas to carrier gas is 1:1 to 1:2; the temperature is preferably 600°C; and the reaction time is preferably 5-20 hours.

[0177] Step S5: screening and filtering the silicon-coated particles;

[0178] The valve between the silicon first reaction device 1 and the screening filter 2 is opened, and the silicon-coated particles that have been completely reacted in the multiple first reaction devices 1 are input into the screening filter 2 for screening to remove the agglomerated and overly large reaction particles.

[0179] Step S6: introducing the screened silicon-coated particles into a second reaction device;

[0180] Passing the sieved silicon-coated particles into the second reaction device 3;

[0181] Step S7: carbon-coating the screened silicon-coated particles to obtain a silicon-carbon negative electrode material;

[0182] Step S71: carbon-coating the screened silicon-coated particles to form a carbon-coated layer;

[0183] Passing the screened silicon-coated particles into a second reaction device;

[0184] A carbon source gas and a carrier gas are introduced into the second reaction device in proportion, and the second reaction device is heated to a preset temperature to decompose the carbon source gas. Under the stirring of the stirring device, the carbon source gas is decomposed and deposited on the surface of the screened silicon-coated particles by chemical vapor deposition to form a carbon coating layer. The ratio of the carbon source gas to the carrier gas is 1:1 to 1:15; the preset temperature is 600°C to 1200°C. The carbon source gas can be selected from one or more mixed gases including acetylene, propyne, butyne, propylene, etc.; the carrier gas can be selected from one or more of nitrogen or argon, and can also be other inert gases.

[0185] Step S72: carbon-coating the silicon-coated particles to form a uniform silicon-carbon negative electrode material;

[0186] The ratio of the carbon source gas and the carrier gas introduced into the second reaction device is regulated, the temperature in the second reaction device is regulated, the reaction time of the second reaction device is regulated, and the particles are fully stirred and dispersed under the stirring of the stirring system. A carbon coating layer is formed on the surface of the sieved silicon-coated particles until the surface of the sieved silicon-coated particles is coated with carbon to form a uniform silicon-carbon negative electrode material.

[0187] Step S8: performing carbon coating on the screened silicon-coated particles to obtain silicon-carbon negative electrode materials multiple times;

[0188] The ratio of the carbon source gas and the carrier gas introduced into the second reaction device 3 is regulated, the temperature in the second reaction device 3 is regulated, and the reaction time of the second reaction device 3 is regulated to form a carbon deposition layer on the surface of the silicon-coated particles until carbon is deposited on the surface of the sieved silicon-coated particles to form a uniform silicon-carbon negative electrode material. The ratio of the carbon source gas and the carrier gas is 1:1 to 1:2; the temperature is preferably 800°C; and the reaction time is preferably 5-20 hours.

[0189] Step S9: Treating the exhaust gas

[0190] The gas in the reactor is treated by the tail gas treatment system 7, and the treatment steps include one or more of waste gas collection, waste gas pretreatment, harmful substance adsorption, catalytic oxidation and combustion. The silicon source gas, carbon source gas, carrier gas and their decomposition products in the above steps are treated by the tail gas treatment system and discharged after meeting the environmental emission standards.

[0191] Step S10: Obtain the required silicon-carbon negative electrode material.

[0192] A large amount of carrier gas is introduced into the second reaction device 3 , and the carrier gas can be selected from one or more of nitrogen or argon. The discharge valve is opened to transport the evenly coated silicon-carbon negative electrode material after reaction to the finished product tank 8 .

[0193] The advantages of this embodiment include: the reactor in Example 2 can be used to continuously produce silicon-carbon negative electrode materials, improve the quality of silicon-carbon negative electrode materials, and improve production efficiency. The gas in the production process of silicon-carbon negative electrode materials is collected and treated by the tail gas treatment system, thereby significantly reducing the emission of waste gas, helping to reduce pollution to the environment, improve air quality, and reduce damage to the ecosystem. The stirring system, heating system and control system are respectively provided in the first reaction device and the second reaction device. The stirring system ensures that the reactant particles are fully dispersed and fluidized. The heating system ensures that the reactants in the reactor are heated evenly and maintains the temperature in the reactor. The control system accurately controls the stirring speed and temperature inside the reaction device, so that the silicon-carbon negative electrode material after the entire coating reaction is more uniform, and the quality and stability of the silicon-carbon negative electrode product are improved. After the silicon-coated particles are completed, the screening filter is used to screen out the silicon-coated particles that are too agglomerated and agglomerated. During the carbon coating process, not only can the production efficiency be improved, but also the quality consistency can be improved. By setting up multiple small-capacity first reaction devices to coat carbon powder with silicon, and then concentrating them in a large-capacity second reaction device for carbon coating, it is beneficial to ensure the quality of silicon-coated particles, realize centralized processing of carbon coating, achieve consistency and stability of silicon-carbon negative electrode materials, and improve production efficiency. The silicon-carbon negative electrode material prepared by this method has more uniform performance, and the components are tightly connected and have strong bonding force. During the charge and discharge process, the active material is not easy to fall off, showing excellent cycle stability, and agglomeration is not easy to occur in the finished product. The silicon-carbon negative electrode material prepared by this method performs well in terms of cycle life and stability.

[0194] The basic principle of the technical effect of the silicon-carbon negative electrode material of the present invention is explained as follows:

[0195] As a high-capacity negative electrode material, silicon expands by more than 300% in volume during the charging cycle, resulting in material pulverization and destruction of the electrode structure, which is the main reason for the decline in the battery's cycle performance. The present application first coats carbon with silicon, and then uses a carbon coating strategy to form a protective layer around silicon particles, effectively alleviating the mechanical stress caused by volume expansion and reducing the generation of cracks, thereby increasing the overall structural stability of the silicon-carbon negative electrode material and improving the cycle stability of the silicon-carbon negative electrode material.

[0196] Carbon-encapsulated silicon not only provides physical support for silicon particles, but also significantly improves the electron conduction efficiency inside the electrode material due to its good conductivity. This feature helps to quickly transfer electrons, reduce internal resistance during discharge, and ensure efficient energy conversion and transmission. In addition, the microporous structure of the carbon layer helps the rapid diffusion of lithium ions, reduces the resistance to lithium ion diffusion during charging, and contributes to the high rate performance and cycle stability of the battery.

[0197] Through forced stirring and airflow, the reaction particles are effectively prevented from accumulating at the bottom, and the particles are fully dispersed in the reactor, ensuring uniform dispersion during silicon coating and subsequent carbon coating, avoiding the aggregation of large particles, and forming a more compact and evenly distributed composite structure. This structure enhances the contact area and bonding force between the active material and the current collector, effectively preventing the active material from falling off during the cycle, and further improving the cycle stability of the battery.

[0198] The advantages of the implementation of the present invention are as follows: silicon-coated carbon powder is coated with silicon to form silicon-coated particles; the silicon-coated particles are screened and filtered; and the silicon-coated particles are carbon-coated to obtain silicon-carbon negative electrode materials. During the silicon coating and carbon coating process, forced stirring and airflow are used to ensure the full dispersion of the reactant particles and the formation of fluidization, effectively preventing the accumulation of reaction particles, thereby significantly improving the agglomeration problem of the silicon-carbon negative electrode material, and improving the uniformity and stability of the prepared silicon-carbon negative electrode material. After the silicon-coated particles are completed, a screening filter is used to screen out and filter the agglomerated and over-agglomerated silicon-coated particles, and then the carbon coating process is carried out, which can not only improve production efficiency but also improve quality consistency. The silicon-carbon negative electrode material prepared by this method has more uniform performance, and the components are tightly connected and have strong bonding. During the charge and discharge process, the active material is not easy to fall off, showing excellent cycle stability, and agglomeration is not easy to occur in the finished product. The silicon-carbon negative electrode material prepared by this method performs well in terms of cycle life and stability.

[0199] Furthermore, by setting up multiple small-capacity first reaction devices to silicon-coat the carbon powder, and then concentrating it in a large-capacity second reaction device for carbon coating, it is beneficial to ensure the quality of the silicon-coated particles, realize centralized processing of carbon coating, achieve consistency and stability of silicon-carbon negative electrode materials, and improve production efficiency; by setting up a screening filter, it is possible to effectively remove large particles that are agglomerated and agglomerated, and only the screened silicon-coated particles are subjected to carbon coating reaction, so that both production efficiency and product quality can achieve a qualitative leap; by setting up a reaction supporting system, it is possible to achieve precise control of the gas supply device, reaction temperature, stirring speed and reaction time, and ensure that the equipment, temperature and other conditions are individually and accurately controlled during the silicon deposition and carbon coating processes, so that the entire reaction process is efficient and stable, thereby further improving product quality and production efficiency; by setting up a vacuum system, the gas pressure in the reactor can be accurately controlled and the air can be effectively removed. Through the setting of the tail gas treatment system, environmental pollution is greatly reduced and the environmental protection performance of the overall production process is improved; through the setting of the mixed gas preheating system, not only the decomposition rate of the gas in the reactor is accelerated and the product quality is improved, but also the waste gas emissions are effectively reduced, which has made a positive contribution to reducing environmental pollution; the silicon-carbon negative electrode material reactor provided by the present invention can not only realize continuous production, but also ensure the overall product quality and achieve a significant improvement in production efficiency.

[0200] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A method for preparing a silicon-carbon negative electrode material, It is characterized in that The method comprises the following steps: Depositing silicon on the surface of carbon powder by decomposing silicon source gas to form silicon-coated particles; Screening and filtering the silicon-coated particles; Carbon coating the screened silicon-coated particles to obtain a silicon-carbon negative electrode material; Each time the screened silicon-coated particles are carbon-coated to obtain the silicon-carbon negative electrode material, the number of silicon-coated particles that can be carbon-coated is obtained by performing silicon coating on carbon powder in multiple batches to form silicon-coated particles.

2. The method for preparing the silicon-carbon negative electrode material according to claim 1, It is characterized in that The step of forming silicon-coated particles by decomposing silicon source gas to deposit silicon on the surface of carbon powder includes: stirring the carbon powder; heating the silicon source gas to a temperature of 400-600° C. to decompose the silicon source gas; and decomposing the silicon source gas to deposit silicon on the surface of the carbon powder to form silicon-coated particles.

3. The method for preparing the silicon-carbon negative electrode material according to claim 2, It is characterized in that The step of forming silicon-coated particles by depositing silicon on the surface of carbon powder by decomposing silicon source gas comprises: introducing a mixed gas of silicon source gas and carrier gas, wherein the ratio of silicon source gas to carrier gas is 1:1 to 1:

10.

4. The method for preparing the silicon-carbon negative electrode material according to claim 1, It is characterized in that The method of carbon-coating the screened silicon-coated particles to obtain the silicon-carbon negative electrode material comprises: depositing carbon on the surface of the screened silicon-coated particles by decomposing a carbon source gas to obtain the silicon-carbon negative electrode material.

5. The method for preparing the silicon-carbon negative electrode material according to claim 4, It is characterized in that The step of obtaining the silicon-carbon negative electrode material by decomposing the carbon source gas to deposit carbon on the surface of the screened silicon-coated particles includes: heating the carbon source gas to a temperature of 600-1200°C to decompose the carbon source gas; stirring the screened silicon-coated particles; and decomposing and depositing the carbon source gas on the surface of the screened silicon-coated particles to obtain the silicon-carbon negative electrode material.

6. The method for preparing the silicon-carbon negative electrode material according to claim 4, It is characterized in that The step of obtaining the silicon-carbon negative electrode material by decomposing the carbon source gas and depositing carbon on the surface of the screened silicon-coated particles comprises: introducing a mixed gas of the carbon source gas and the carrier gas, wherein the ratio of the carbon source gas to the carrier gas is 1:1 to 1:

15.

7. The method for preparing a silicon-carbon negative electrode material according to any one of claims 1 to 6, It is characterized in that The method further comprises the following steps: before decomposing silicon source gas to deposit silicon on the surface of carbon powder to form silicon-coated particles, drying the carbon powder and performing a surface activation treatment on the carbon powder.

8. A silicon-carbon negative electrode material reactor, It is characterized in that include: The first reaction device is used to decompose the silicon source gas to deposit silicon on the surface of the carbon powder to form silicon-coated particles; A second reaction device, connected to at least one of the first reaction devices, is used to carbon-coat the silicon-coated particles formed by the first reaction device to form a silicon-carbon negative electrode material; A reaction supporting system for supplying materials for silicon coating to the first reaction device, and for supplying materials for carbon coating to the second reaction device; A screening filter is provided between the first reaction device and the second reaction device, and the screening filter is used to screen and filter the silicon-coated particles formed by the first reaction device.

9. The silicon-carbon negative electrode material reactor according to claim 8, It is characterized in that The reaction supporting system includes a gas supply device, a heating system, a stirring system and a control system. The gas supply device is used to supply silicon source gas and carrier gas to the first reaction device and to supply carbon source gas and carrier gas to the second reaction device. The heating system is used to heat the first reaction device and the second reaction device respectively; the stirring system is used to stir the first reaction device and the second reaction device respectively; the control system is used to control the operation of the gas supply device, the heating system and the stirring system respectively.

10. The silicon-carbon negative electrode material reactor according to claim 9, It is characterized in that It also includes a mixed gas preheating system, which is connected to the first reaction device, the second reaction device and the gas supply device respectively, and is used to preheat the gas supplied by the gas supply device.

11. The silicon-carbon negative electrode material reactor according to any one of claims 7 to 10, It is characterized in that It also includes a vacuum system, which is used to evacuate the first reaction device and the second reaction device respectively.

12. The silicon-carbon negative electrode material reactor according to claim 11, It is characterized in that It also includes an exhaust gas treatment system, which is connected to the first reaction device, the second reaction device and the vacuum system respectively.

Citation Information

Patent Citations

  • Silicon negative electrode material and production system, production method and application thereof

    CN116544401A

  • Preparation method of multi-level silicon-carbon negative electrode material

    CN117352703A

  • Preparation method and device for producing silicon-carbon negative electrode material of lithium battery by utilizing two-stage reactor method

    CN117735530A

  • Silicon-carbon negative electrode material reactor and silicon-carbon negative electrode material preparation method

    CN117920069A

  • Fluidized macro-quantity preparation method of silicon-carbon negative electrode material

    CN118281192A

Cited By

  • System and process method for large-scale preparation of high-first-effect silicon-carbon material

    CN120054375A

  • A system and process for scalable preparation of high-initial-efficiency silicon-carbon materials

    CN120054375B

  • Preparation method and system of silicon carbon material

    CN121020558A

  • Silicon-carbon negative electrode material production system and silicon-carbon negative electrode material manufacturing method

    CN121565814A