Green preparation method of high-purity magnetic refrigeration oxide powder GGG
By introducing Cl- and heating stirring in the Ga2O3 dissolution stage, combining oxalic acid co-precipitation and multi-gradient heat treatment process, the problem of Ga2O3 that is not completely reacted in GGG preparation is solved, the purity and efficiency of the powder are improved, and the efficiency and small size of the refrigeration equipment are promoted. change.
Patent Information
- Application Number
- CN202411147690.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-15
AI Technical Summary
There is a problem of Ga2O3 in the existing GGG preparation technology that is not fully reacted, resulting in low efficiency of refrigeration equipment and limited development of miniaturization.
High-purity GGG powder is prepared by introducing Cl- in the Ga2O3 dissolution stage and heating and stirring, combined with the oxalic acid co-precipitation process and the multi-gradient heat treatment process, ensuring sufficient dissociation of Ga-O bonds and complete precipitation of metal cations.
It effectively solves the problem of incomplete reaction Ga2O3, improves the purity and yield of GGG powder, simplifies the preparation process, and promotes the efficiency and miniaturization of refrigeration equipment.
Smart Images

Figure CN118954579A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ultra-low temperature magnetic refrigeration materials, and in particular relates to a green preparation method of high-purity magnetic refrigeration oxide powder GGG. Background Art
[0002] In recent years, the world has faced challenges such as energy shortage, climate warming and frequent catastrophic weather, which have posed severe challenges to the refrigeration industry. According to the latest data, about 25% of the world's electricity consumption is used for various refrigeration applications each year. However, traditional commercial refrigeration technology has exposed serious problems such as high energy consumption, low efficiency, high oxygen depletion potential, and dependence on scarce resources. Therefore, we urgently need to seek more environmentally friendly and efficient refrigeration technology to meet the current sustainable development needs of energy and environment.
[0003] In this context, solid magnetic refrigeration technology with the characteristics of high efficiency, low noise, zero carbon emissions, safety and reliability has attracted much attention. The core of this technology lies in the refrigerant, that is, the magnetocaloric material. We can achieve the purpose of refrigeration by regulating the magnetic order of the material. 3 Ga 5 O 12 (GGG) is a low-temperature magnetic refrigeration material that has become a research focus due to its simple chemical formula and low operating temperature range. However, the existing GGG preparation technology still faces challenges in producing high-quality powders, especially the presence of incompletely reacted Ga 2 O 3 This not only reduces its actual application efficiency, but also greatly limits the research and development of miniaturization of refrigeration equipment. Summary of the invention
[0004] The purpose of the present invention is to overcome the above-mentioned deficiencies in the prior art and provide a green preparation method for high-purity magnetic refrigeration oxide powder GGG. 2 O 3 Introduction of Cl in the dissolution stage - The heating and stirring were used to achieve rapid and sufficient dissociation of Ga-O bonds. Then, GGG (Gd 3 Ga 5 O 12 ) powder, which solves the problem of incompletely reacted Ga in the products obtained by the prior art. 2 O 3 problem.
[0005] To achieve the above object, the technical solution adopted by the present invention is: a green preparation method of high-purity magnetic refrigeration oxide powder GGG, characterized in that the method comprises the following steps:
[0006] Step 1: Gd2 O 3 Add nitric acid solution to dissolve Gd salt solution, and then 2 O 3 Adding to a mixed solution of a nitric acid solution and a hydrochloric acid solution and heating and stirring to dissolve to obtain a Ga salt solution, and then mixing the Gd salt solution and the Ga salt solution to obtain a clear metal salt solution;
[0007] Step 2, dissolving oxalic acid with anhydrous ethanol to obtain a clear oxalic acid solution;
[0008] Step 3, stirring the oxalic acid solution obtained in step 2, and adding dropwise the metal salt solution obtained in step 1, and then adding dropwise ammonia water to adjust the pH value to 7.5-10, to obtain a metal cation precipitate;
[0009] Step 4: Wash the metal cation precipitate obtained in step 3 with water, vacuum filter and then dry at a constant temperature to obtain oxalate precursor powder;
[0010] Step 5. Pre-decompose, pre-sinter and phase-sinter the oxalate precursor powder obtained in step 4 in sequence to obtain GGG powder; the pre-decomposition process is: heating to 400°C ~ 500°C and keeping warm for 5h ~ 20h, the pre-sintering process is: heating to 500°C ~ 800°C and keeping warm for 2h ~ 5h, and the phase-sintering process is: heating to 1100°C ~ 1300°C and keeping warm for 2h ~ 20h.
[0011] The above-mentioned green preparation method of high-purity magnetic refrigeration oxide powder GGG is characterized in that Ga in the metal salt solution in step 1 3+ and Gd 3+ The molar ratio is 4.9-5.1:3.
[0012] The present invention controls the Ga in the metal salt solution. 3+ and Gd 3+ The molar ratio of Ga is 0.04, and the pH value of the metal salt solution is adjusted to 7.5-10 by dropping ammonia water to completely precipitate the metal cations, so that Ga 3+ and Gd 3+ The molar ratio meets the requirements of GGG chemical composition and improves Ga 3+ and Gd 3+ The utilization rate and purity of the finished product GGG.
[0013] The above-mentioned green preparation method of high-purity magnetic refrigeration oxide powder GGG is characterized in that the volume ratio of nitric acid solution to hydrochloric acid solution in the mixed solution in step one is 3:0.1~1.
[0014] The above-mentioned green preparation method of high-purity magnetic refrigeration oxide powder GGG is characterized in that the heating temperature in step one is 60°C to 100°C, and the heating time is 2h to 5h.
[0015] The present invention sets the heating temperature and heating time to make Ga 2 O 3 Rapid and complete dissolution to increase Ga 2 O 3 utilization rate.
[0016] The above-mentioned green preparation method of high-purity magnetic refrigeration oxide powder GGG is characterized in that the concentration of the oxalic acid solution in step 2 is 0.9 mol / L to 1.5 mol / L.
[0017] The above-mentioned green preparation method of high-purity magnetic refrigeration oxide powder GGG is characterized in that the stirring in step three is electric stirring, and the stirring speed is 0.3kr / min to 0.5kr / min.
[0018] The present invention can make the metal salt solution disperse quickly and evenly in the oxalic acid solution by setting the stirring speed at 0.3kr / min to 0.5kr / min, so that the formed metal cations are precipitated in Ga 3+ and Gd 3+ At the same time, avoid stirring at a speed greater than 0.5 kr / min, which will cause the solution to splash and affect the precipitation of metal cations in Ga 3+ and Gd 3+ proportion.
[0019] The above-mentioned green preparation method of high-purity magnetic refrigeration oxide powder GGG is characterized in that constant low temperature aging is carried out after adjusting the pH value in step three, the constant low temperature aging temperature is 2°C to 8°C, and the constant low temperature aging time is not less than 10 hours.
[0020] The present invention is used to make Ga 3+ and Gd 3+ The reaction is complete and the precipitation is complete. Controlling the aging temperature at 2℃~8℃ can prevent the precipitation and dissociation of metal cations and ensure that the Ga in the metal cation precipitation 3+ and Gd 3+ Not reduced by aging process.
[0021] The above-mentioned green preparation method of high-purity magnetic refrigeration oxide powder GGG is characterized in that the constant temperature drying temperature in step 4 is less than 90°C.
[0022] The above-mentioned green preparation method of high-purity magnetic refrigeration oxide powder GGG is characterized in that the oxalate precursor powder is ground before the pre-decomposition in step five.
[0023] The green preparation method of the high-purity magnetic refrigeration oxide powder GGG is characterized in that the pre-decomposition, pre-sintering and phase sintering in step 5 are all in an environment of circulating air, and the volume fraction of the GGG phase in the GGG powder is not less than 90%.
[0024] The present invention grinds oxalate precursor powder to ensure the uniformity of the oxalate precursor powder, performs pre-decomposition in a circulating air environment to completely decompose the oxalate precursor powder into carbonate and oxide, then performs high-temperature pre-calcination in a circulating air environment to completely decompose the carbonate in the powder into uniform oxide powder, and finally performs sintering to ensure complete reaction of the oxide to generate GGG powder.
[0025] Compared with the prior art, the present invention has the following advantages:
[0026] 1. The present invention is achieved by 2 O 3 and Ga 2 O 3 Introduction of Cl in the dissolution stage - The Ga-O bond is rapidly and fully dissociated by heating and stirring. 2 O 3 The oxalate precursor powder is formed by reacting with oxalic acid solution and ammonia water, and the oxalate precursor powder is pre-decomposed, pre-sintered and phase-sintered to make the oxide react completely, thereby obtaining a Ga-free product. 2 O 3 The method can produce GGG powder and effectively simplify the steps and equipment for preparing GGG powder.
[0027] 2. The present invention controls the temperature and holding time of the pre-decomposition, pre-sintering and phase sintering stages in the multi-gradient heat treatment process and carries out the process in a circulating air environment, so that the oxalate precursor powder is completely decomposed into oxides, thereby effectively improving the purity and yield of the GGG powder.
[0028] 3. The present invention ensures that the metal cations are completely precipitated in the form of oxalate by adjusting the pH value and adopting a constant low temperature aging process, and controls the Ga content in the metal cation precipitation. 3+ and Gd 3+ ratio, further improving the purity and yield of GGG powder.
[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is the XRD pattern of the GGG powder prepared in Example 1. DETAILED DESCRIPTION
[0031] Example 1
[0032] The preparation method of this embodiment comprises the following steps:
[0033] Step 1: 13.92 g of Gd 2 O 3 Add nitric acid solution to dissolve Gd salt solution, and 11.72g of Ga 2 O 3 Adding into a mixed solution of a nitric acid solution and a hydrochloric acid solution and heating to 100° C. and stirring for 2 hours to dissolve, to obtain a Ga salt solution, and mixing the Gd salt solution and the Ga salt solution to obtain a clear metal salt solution; the volume ratio of the nitric acid solution to the hydrochloric acid solution in the mixed solution is 3:1, the concentration of the nitric acid solution in the mixed solution is 10.6 mol / L, and the concentration of the hydrochloric acid solution in the mixed solution is 11.9 mol / L;
[0034] Step 2: dissolving 300 g of oxalic acid in 3.25 L of anhydrous ethanol to obtain a clear oxalic acid solution;
[0035] Step 3: The oxalic acid solution obtained in step 2 is added dropwise to the metal salt solution obtained in step 1 under electric stirring at a stirring rate of 0.42 kr / min, and then ammonia water is added dropwise to adjust the pH value to 8.5, and then aged in a constant temperature environment of 2° C. for 10 hours to obtain a metal cation precipitate;
[0036] Step 4: Wash the metal cation precipitate obtained in step 3 with water for 5 times, vacuum filter it, and dry it at a constant temperature of 50° C. to obtain an oxalate precursor powder;
[0037] Step 5: Grind the oxalate precursor powder obtained in step 4 and place it in a box-type muffle furnace, heat it to 500°C in a circulating air environment and keep it warm for 5 hours; then transfer it to a high-temperature tube furnace, heat it to 500°C in a circulating air environment and keep it warm for 2 hours, heat it to 1200°C and keep it warm for 20 hours, cool it with the furnace, and obtain GGG powder.
[0038] The GGG powder prepared in this example was subjected to XRD detection. Figure 1 As shown, Bragg position is the Bragg diffraction peak of the GGG phase structure. obs. (Test the XRD diffraction peak intensity) to simulate and calculate, and get I cal. (theoretically calculated XRD diffraction peak intensity), by calculating I obs. -I cal. (The difference between the measured and theoretically calculated diffraction peak intensities) indicates that the phase volume fraction of the GGG powder prepared in this embodiment is 98.8%.
[0039] Example 2
[0040] The preparation method of this embodiment comprises the following steps:
[0041] Step 1: 13.59 g of Gd 2 O 3 Add nitric acid solution to dissolve Gd salt solution, and add 11.95g of Ga 2 O 3 Adding into a mixed solution of a nitric acid solution and a hydrochloric acid solution and heating to 80° C. and stirring for 3 hours to dissolve, to obtain a Ga salt solution, and mixing the Gd salt solution and the Ga salt solution to obtain a clear metal salt solution; the volume ratio of the nitric acid solution to the hydrochloric acid solution in the mixed solution is 3:0.1, the concentration of the nitric acid solution in the mixed solution is 10 mol / L, and the concentration of the hydrochloric acid solution in the mixed solution is 11 mol / L;
[0042] Step 2: dissolving 300 g of oxalic acid in 3.25 L of anhydrous ethanol to obtain a clear oxalic acid solution;
[0043] Step 3: The oxalic acid solution obtained in step 2 is added dropwise to the metal salt solution obtained in step 1 under electric stirring at a stirring rate of 0.50 kr / min, and then ammonia water is added dropwise to adjust the pH value to 7.5, and then aged in a constant temperature environment of 4° C. for 10 hours to obtain a metal cation precipitate;
[0044] Step 4: Wash the metal cation precipitate obtained in step 3 with water for 5 times, vacuum filter it, and dry it at a constant temperature of 50° C. to obtain an oxalate precursor powder;
[0045] Step 5: Grind the oxalate precursor powder obtained in step 4 and place it in a box-type muffle furnace, heat it to 500°C in an environment with circulating air and keep it warm for 5 hours; then transfer it to a high-temperature tube furnace, heat it to 800°C in an environment with circulating air and keep it warm for 2 hours, heat it to 1100°C and keep it warm for 8 hours, cool it with the furnace, and obtain GGG powder.
[0046] According to the test, the phase volume fraction of the GGG powder prepared in this example is 90.2%.
[0047] Example 3
[0048] The preparation method of this embodiment comprises the following steps:
[0049] Step 1: 5.857 g of Gd 2 O 3 Add nitric acid solution to dissolve Gd salt solution, and add 6.796g of Ga 2 O 3Adding into a mixed solution of a nitric acid solution and a hydrochloric acid solution and heating to 70° C. and stirring for 3 hours to dissolve, to obtain a Ga salt solution, and mixing the Gd salt solution and the Ga salt solution to obtain a clear metal salt solution; the volume ratio of the nitric acid solution to the hydrochloric acid solution in the mixed solution is 3:1, the concentration of the nitric acid solution in the mixed solution is 11 mol / L, and the concentration of the hydrochloric acid solution in the mixed solution is 12 mol / L;
[0050] Step 2: Dissolve 150 g of oxalic acid in 1.85 L of anhydrous ethanol to obtain a clear oxalic acid solution;
[0051] Step 3: The oxalic acid solution obtained in step 2 is added dropwise to the metal salt solution obtained in step 1 under electric stirring at a stirring rate of 0.30 kr / min, and then ammonia water is added dropwise to adjust the pH value to 8.0, and then aged in a constant temperature environment of 6° C. for 10 hours to obtain a metal cation precipitate;
[0052] Step 4: Wash the metal cation precipitate obtained in step 3 with water for 5 times, vacuum filter it, and dry it at a constant temperature of 50° C. to obtain an oxalate precursor powder;
[0053] Step 5: Grind the oxalate precursor powder obtained in step 4 and place it in a box-type muffle furnace, heat it to 450°C in a circulating air environment and keep it warm for 6 hours; then transfer it to a high-temperature tube furnace, heat it to 700°C in a circulating air environment and keep it warm for 5 hours, heat it to 1300°C and keep it warm for 2 hours, cool it with the furnace, and obtain GGG powder.
[0054] According to the test, the phase volume fraction of the GGG powder prepared in this example is 95.0%.
[0055] Comparative Example 1
[0056] The difference between this comparative example and Example 3 is that in step five, the oxalate precursor powder is ground and placed in a box-type muffle furnace, heated to 500°C in an environment of circulating air and kept warm for 5 hours; then transferred to a high-temperature tube furnace, heated to 900°C in an environment of circulating air, kept warm for 10 hours and then cooled with the furnace, and no GGG powder phase structure is formed.
[0057] In this comparative example, only a pre-decomposition stage at 500°C and a phase sintering stage at 900°C are set, and a pre-sintering stage is lacking, so that the carbonate cannot be completely decomposed after the oxalate precursor powder is pre-decomposed, and the temperature in the phase sintering stage is too low to make the oxide react to generate GGG powder; this shows that the temperature and insulation time in the multi-gradient heat treatment process set in the present invention can generate GGG powder.
[0058] Example 4
[0059] The preparation method of this embodiment comprises the following steps:
[0060] Step 1: 13.59 g of Gd 2 O 3 Add nitric acid solution to dissolve Gd salt solution, and 11.72g of Ga 2 O 3 Adding into a mixed solution of a nitric acid solution and a hydrochloric acid solution and heating to 60° C. and stirring for 5 hours to dissolve, to obtain a Ga salt solution, and mixing the Gd salt solution and the Ga salt solution to obtain a clear metal salt solution; the volume ratio of the nitric acid solution to the hydrochloric acid solution in the mixed solution is 3:1, the concentration of the nitric acid solution in the mixed solution is 10.6 mol / L, and the concentration of the hydrochloric acid solution in the mixed solution is 11.9 mol / L;
[0061] Step 2: dissolving 300 g of oxalic acid in 3.25 L of anhydrous ethanol to obtain a clear oxalic acid solution;
[0062] Step 3: The oxalic acid solution obtained in step 2 is added dropwise to the metal salt solution obtained in step 1 under electric stirring at a stirring rate of 0.42 kr / min, and then ammonia water is added dropwise to adjust the pH value to 8.5, and then aged in a constant temperature environment of 8° C. for 12 hours to obtain a metal cation precipitate;
[0063] Step 4: Wash the metal cation precipitate obtained in step 3 with water for 5 times, vacuum filter it, and dry it at a constant temperature of 50° C. to obtain an oxalate precursor powder;
[0064] Step 5: Grind the oxalate precursor powder obtained in step 4 and place it in a box-type muffle furnace, heat it to 400°C in a circulating air environment and keep it warm for 8 hours; then transfer it to a high-temperature tube furnace, heat it to 500°C in a circulating air environment and keep it warm for 2 hours, heat it to 1200°C and keep it warm for 10 hours, cool it with the furnace, and obtain GGG powder.
[0065] According to the test, the phase volume fraction of the GGG powder prepared in this example is 90.8%.
[0066] Comparative Example 2
[0067] The difference between this comparative example and Example 4 is that in step 5, the oxalate precursor powder is ground and placed in a box-type muffle furnace, heated to 400°C in a circulating air environment and kept warm for 8 hours, and then heated to 500°C and kept warm for 2 hours; then transferred to a high-temperature tube furnace, heated to 500°C in a circulating air environment and kept warm for 5 hours, and then heated to 1000°C and kept warm for 20 hours, to obtain a sintered product containing GGG and Ga. 2 O 3 Mixed phase powder.
[0068] In this comparative example, a pre-decomposition stage at 400°C and 500°C, a pre-sintering stage at 500°C, and a phase-forming sintering stage at 1000°C were set. The temperature and time of the pre-decomposition and pre-sintering stages were sufficient to completely decompose the oxalate precursor powder into oxides. However, since the temperature of the phase-forming sintering stage was too low, the oxides could not be completely reacted, and a portion of unreacted Ga 2 O 3 Mixed with GGG, it shows that the temperature and holding time of the multi-gradient heat treatment process set by the present invention can produce a product without Ga 2 O 3 of GGG powder.
[0069] Comparative Example 3
[0070] The difference between this comparative example and Example 4 is that in step 5, the oxalate precursor powder is ground and placed in a box-type muffle furnace, heated to 300°C in a circulating air environment and kept warm for 20 hours; then transferred to a high-temperature tube furnace, heated to 800°C in a circulating air environment and kept warm for 2 hours, and then heated to 1400°C and kept warm for 2 hours to obtain a sintered product containing GGG and Ga. 2 O 3 Mixed phase powder.
[0071] This comparative example sets a pre-decomposition stage, a pre-sintering stage, and a phase sintering stage, but due to the low pre-decomposition temperature, it is not enough to completely decompose the oxalate precursor powder, resulting in residual oxalate precursor powder and the generation of impure intermediate products, which will leave incompletely decomposed compounds or generate incomplete crystalline phases in the subsequent processing stage. In addition, the duration of the pre-sintering process in this comparative example is also short, and the residual oxalate precursor powder and the generated intermediate products in the pre-decomposition stage cannot be completely decomposed, which is not conducive to crystallization.
[0072] In summary, the incomplete phase transformation caused by insufficient heat treatment in the previous stage resulted in the formation of GGG powder and Ga 2 O 3 The mixed phase product indicates that the temperature and holding time of the multi-gradient heat treatment process set by the present invention can produce a product without Ga 2 O 3 of GGG powder.
[0073] Example 5
[0074] The difference between this embodiment and embodiment 4 is that in step 5, the oxalate precursor powder obtained in step 4 is ground and placed in a box-type muffle furnace, heated to 400°C in an environment of circulating air and kept warm for 20 hours; then transferred to a high-temperature tube furnace, heated to 500°C in an environment of circulating air and kept warm for 3 hours, heated to 1200°C and kept warm for 10 hours, and cooled with the furnace to obtain GGG powder.
[0075] After testing, the phase volume fraction of the GGG powder prepared in this example is 91.0%.
[0076] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A green preparation method of high-purity magnetic refrigeration oxide powder GGG, characterized in that: The method comprises the following steps: Step 1, adding Gd2O3 to a nitric acid solution to dissolve to obtain a Gd salt solution, adding Ga2O3 to a mixed solution of a nitric acid solution and a hydrochloric acid solution and heating and stirring to dissolve to obtain a Ga salt solution, and then mixing the Gd salt solution and the Ga salt solution to obtain a clear metal salt solution; Step 2, dissolving oxalic acid with anhydrous ethanol to obtain a clear oxalic acid solution; Step 3, stirring the oxalic acid solution obtained in step 2, and adding dropwise the metal salt solution obtained in step 1, and then adding dropwise ammonia water to adjust the pH value to 7.5-10, to obtain a metal cation precipitate; Step 4: Wash the metal cation precipitate obtained in step 3, vacuum filter it and dry it at a constant temperature to obtain an oxalate precursor powder; Step 5. Pre-decompose, pre-sinter and phase-sinter the oxalate precursor powder obtained in step 4 in sequence to obtain GGG powder; the pre-decomposition process is: heating to 400°C ~ 500°C and keeping warm for 5h ~ 20h, the pre-sintering process is: heating to 500°C ~ 800°C and keeping warm for 2h ~ 5h, and the phase-sintering process is: heating to 1100°C ~ 1300°C and keeping warm for 2h ~ 20h.
2. The green preparation method of high-purity magnetic refrigeration oxide powder GGG according to claim 1, characterized in that: In step 1, the Ga 3+ and Gd 3+ The molar ratio is 4.9-5.1:
3.
3. The green preparation method of high-purity magnetic refrigeration oxide powder GGG according to claim 1, characterized in that: The volume ratio of the nitric acid solution to the hydrochloric acid solution in the mixed solution in step 1 is 3:0.1-1.
4. The green preparation method of high-purity magnetic refrigeration oxide powder GGG according to claim 1, characterized in that: The heating temperature in step 1 is 60° C. to 100° C., and the heating time is 2 h to 5 h.
5. The green preparation method of high-purity magnetic refrigeration oxide powder GGG according to claim 1, characterized in that: The concentration of the oxalic acid solution in step 2 is 0.9 mol / L to 1.5 mol / L.
6. The green preparation method of high-purity magnetic refrigeration oxide powder GGG according to claim 1, characterized in that: The stirring in step 3 is electric stirring, and the stirring speed is 0.3kr / min to 0.5kr / min.
7. The green preparation method of high-purity magnetic refrigeration oxide powder GGG according to claim 1, characterized in that: After adjusting the pH value in step 3, constant low temperature aging is performed, the constant low temperature aging temperature is 2°C to 8°C, and the constant low temperature aging time is not less than 10 hours.
8. The green preparation method of high-purity magnetic refrigeration oxide powder GGG according to claim 1, characterized in that: The temperature of the constant temperature drying in step 4 is less than 90°C.
9. The green preparation method of high-purity magnetic refrigeration oxide powder GGG according to claim 1, characterized in that: The oxalate precursor powder is ground before the pre-decomposition described in step five.
10. The green preparation method of high-purity magnetic refrigeration oxide powder GGG according to claim 1, characterized in that: The pre-decomposition, pre-sintering and phase sintering in step 5 are all carried out in an environment with circulating air, and the volume fraction of the GGG phase in the GGG powder is not less than 90%.