Stripping method of layered material
Through the mixing and stirring of molten metal and layered material and solvent dispersion centrifugal technology, the problems of many defects and impurities in the mechanical peeling method are solved, and the preparation of high-quality two-dimensional materials is realized, which simplifies the production process and is suitable for in-depth research. and application.
Patent Information
- Application Number
- CN202411188967.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-15
AI Technical Summary
The existing mechanical peeling method has many defects and impurities introduced when preparing two-dimensional materials, which is poor in universality and makes it difficult to produce high-quality two-dimensional materials efficiently and at low cost.
The molten metal and layered material powder are mixed and stirred, and then dispersed in the solvent and removed by centrifugation. The surface tension and intercalation effect are used to peel off the layered material to avoid high temperature and high pressure conditions and reduce the introduction of defects.
It realizes the preparation of defect-free and high-quality two-dimensional materials, which is simple and fast, and is suitable for in-depth research on the intrinsic characteristics and applications of two-dimensional materials.
Smart Images

Figure CN118954599A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of nano materials, and in particular to a method for stripping layered materials. Background Art
[0002] With the discovery of the bipolar electric field effect in single-layer graphene, researchers have discovered many unique properties of this material over the years, including its unique electronic structure, high electron mobility, high thermal conductivity, and optical transparency. Inspired by the progress in the field of graphene, scholars have begun to look for other layered materials as platforms for studying new physical and chemical phenomena. The field of two-dimensional materials has been expanded through the study of two-dimensional graphene analog crystals such as transition metal dichalcogenides (TMDs), hexagonal boron nitride (h-BN), silicene, and phosphorene.
[0003] For these applications, the prerequisite is the efficient and scalable production of high-quality and low-cost two-dimensional materials. The "top-down" exfoliation technique can achieve low-cost preparation of two-dimensional materials by overcoming the interlayer interactions of layered materials. At present, the two-dimensional materials prepared by traditional mechanical exfoliation methods have many defects and are prone to introduce impurities during the preparation process, which has poor universality.
[0004] It should be noted that the information disclosed in the above background technology section is only used for understanding the background of the present application, and therefore may include information that does not constitute prior art known to ordinary technicians in the field. Summary of the invention
[0005] The present invention provides a method for stripping layered materials, thereby realizing the preparation of high-quality two-dimensional materials.
[0006] The present invention adopts the following technical solution:
[0007] A method for stripping a layered material comprises the following steps:
[0008] (1) adding molten metal dropwise to layered material powder for mixing and stirring to obtain a mixture;
[0009] (2) dispersing the mixture in a solvent to exfoliate the layered material to obtain a dispersion;
[0010] (3) Centrifuging the dispersion to remove the molten metal and unpeeled layered materials to obtain a peeled two-dimensional material.
[0011] Preferably, in step (1), the layered material is at least one of transition metal sulfide powder, graphite, hexagonal boron nitride, and layered minerals.
[0012] Preferably, in step (1), the molten metal is at least one of indium, gallium indium tin alloy, and gallium.
[0013] Preferably, in step (2), the solvent is at least one of ethanol, isopropanol, DMF and water.
[0014] Preferably, in step (1), the stirring speed is 100-600 rpm, the stirring time is 1-48 hours, and the mixing temperature is 20-70°C.
[0015] Preferably, in step (2), the layered material is exfoliated by dispersing the mixture in a solvent under ultrasonic conditions, the ultrasonic time is 10-120 min, and the ultrasonic power is 10-100 W.
[0016] Preferably, step (3) comprises the following steps:
[0017] (3.1) centrifuging the dispersion at a low speed and collecting the supernatant;
[0018] (3.2) subjecting the supernatant of step (3.1) to high-speed centrifugation to collect the precipitate;
[0019] (3.3) Ultrasonic dispersion of the precipitate collected in step (3.2) in a solvent, and repeating steps (3.1) and (3.2) multiple times until a pure exfoliated two-dimensional material is obtained.
[0020] Preferably, the speed of the low-speed centrifugation in step (3.1) is 1000-3000 rpm, and the time is 5-10 min; the speed of the high-speed centrifugation in step (3.2) is 6000-9000 rpm, and the time is 10-30 min.
[0021] Preferably, in step (1), the molar ratio of the layered material to the molten metal is 5:1-1:1.
[0022] Preferably, in step (2), each milliliter of the solvent contains 2.5 mg-250 mg of the mixture.
[0023] The present invention has the following beneficial effects: the present invention utilizes the surface tension and intercalation effect between the molten metal and the layered material, and successfully peels off the layered material through the interface and interlayer force between the layered material and the molten metal to obtain high-quality two-dimensional material sheets. The method of the present invention is fast and simple, avoids extreme preparation conditions such as high temperature and high pressure, avoids the introduction of additional defects, and obtains defect-free high-quality two-dimensional materials without introducing additional polymers. It is helpful to explore the intrinsic properties of two-dimensional materials and is of great significance to the subsequent research on the intrinsic properties of two-dimensional materials and deeper applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of a method for stripping a layered material in a specific embodiment of the present invention.
[0025] Figure 2a is an atomic force microscope image of h-BN two-dimensional nanosheets obtained by peeling h-BN in Example 1 of the present invention;
[0026] Figure 2b is a transmission electron microscope image of h-BN two-dimensional nanosheets obtained by peeling h-BN in Example 1 of the present invention;
[0027] Figure 2c is a high-resolution transmission electron microscopy image of h-BN two-dimensional nanosheets obtained by peeling h-BN in Example 1 of the present invention;
[0028] Figure 3a is an atomic force microscope image of the two-dimensional sheet structure of MoS2 obtained by peeling off molybdenum disulfide in Example 2 of the present invention;
[0029] Figure 3b is a transmission electron microscope image of the two-dimensional sheet structure of MoS2 obtained by peeling off molybdenum disulfide in Example 2 of the present invention;
[0030] Figure 4a is an atomic force microscope image of the two-dimensional graphene sheet structure obtained by exfoliating graphite in Example 3 of the present invention;
[0031] Figure 4b It is a transmission electron microscope image of the two-dimensional graphene sheet structure obtained by exfoliating graphite in Example 3 of the present invention. DETAILED DESCRIPTION
[0032] The following is a detailed description of the embodiments of the present invention. It should be emphasized that the following description is only exemplary and is not intended to limit the scope and application of the present invention. In the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other.
[0033] The specific embodiment of the present invention provides a method for stripping a layered material, such as Figure 1 As shown, it includes the following steps:
[0034] (1) adding molten metal dropwise to layered material powder for mixing and stirring to obtain a mixture;
[0035] (2) dispersing the mixture in a solvent to exfoliate the layered material to obtain a dispersion;
[0036] (3) Centrifuging the dispersion to remove the molten metal and unpeeled layered materials to obtain a peeled two-dimensional material.
[0037] In a preferred embodiment, in step (1), the layered material is at least one of transition metal sulfide powder, graphite, hexagonal boron nitride, and layered minerals (such as rare earth materials).
[0038] In a preferred embodiment, in step (1), the molten metal is at least one of indium, gallium indium tin alloy, and gallium.
[0039] In a preferred embodiment, in step (2), the solvent is at least one of ethanol, isopropanol, DMF and water.
[0040] In a preferred embodiment, in step (1), the stirring speed is 100-600 rpm, the stirring time is 1-48 hours, and the mixing temperature is 20-70°C.
[0041] In a preferred embodiment, in step (2), the layered material is exfoliated by dispersing the mixture in a solvent under ultrasonic conditions, the ultrasonic time is 10-120 min, and the ultrasonic power is 10-100W.
[0042] In a preferred embodiment, step (3) comprises the following steps:
[0043] (3.1) centrifuging the dispersion at a low speed and collecting the supernatant;
[0044] (3.2) subjecting the supernatant of step (3.1) to high-speed centrifugation to collect the precipitate;
[0045] (3.3) Ultrasonic dispersion of the precipitate collected in step (3.2) in a solvent (preferably, the ultrasonic time is 10-120 min, the ultrasonic power is 10-100 W, and the solvent is at least one of ethanol, isopropanol, DMF, and water, with ethanol being more preferred), and steps (3.1) and (3.2) are repeated multiple times until a pure exfoliated two-dimensional material is obtained.
[0046] In a preferred embodiment, the speed of the low-speed centrifugation in step (3.1) is 1000-3000 rpm, and the time is 5-10 min; the speed of the high-speed centrifugation in step (3.2) is 6000-9000 rpm, and the time is 10-30 min.
[0047] In a preferred embodiment, the molar ratio of the layered material to the molten metal is 5:1-1:1.
[0048] In a preferred embodiment, in step (2), each milliliter of the solvent contains 2.5 mg-250 mg of the mixture.
[0049] In a preferred embodiment, the peeled two-dimensional material is processed (for example, by drop coating, spin coating, filtration, etc.) into a two-dimensional material film for application in wearable devices, electronic devices, hydrophobic dustproof coatings, etc.
[0050] The present invention is further described below.
[0051] Example 1
[0052] A method for stripping a hexagonal boron nitride (h-BN) layered material comprises the following steps:
[0053] (1) Weigh 300 mg of h-BN layered material powder, add 300 mg of liquid metal gallium (Ga) dropwise under stirring, mix thoroughly, and continue stirring for 24 h.
[0054] (2) exfoliating the layered material by ultrasonicating a mixed solution of 24 mL of ethanol and the above mixture at 50 W for 30 min to obtain a dispersion;
[0055] (3) The dispersion was centrifuged at 2000 rpm for 10 min, and the h-BN two-dimensional sheet clear solution was carefully removed;
[0056] (4) the clear solution was centrifuged at 8000 rpm for 30 min to obtain h-BN two-dimensional nanosheets;
[0057] (5) Ultrasonic dispersion of the h-BN two-dimensional nanosheets in ethanol, and repeating steps (3) and (4) multiple times to ensure complete removal of the liquid metal and the unpeeled h-BN layered material powder to obtain pure h-BN two-dimensional nanosheets.
[0058] The exfoliated h-BN two-dimensional nanosheets were characterized using atomic force microscopy (AFM), and the results showed that the h-BN two-dimensional nanosheets were large-sized thin layers (such as Figure 2a At the same time, Figure 2b and 2c It is demonstrated that the exfoliated h-BN two-dimensional nanosheets are defect-free and of high quality.
[0059] Example 2
[0060] The stripping method of molybdenum disulfide comprises the following steps:
[0061] (1) Weigh 300 mg of molybdenum disulfide powder, add 300 mg of liquid metal gallium (Ga) dropwise under stirring, mix thoroughly and continue stirring for 24 hours;
[0062] (2) a mixed solution of 24 ml of isopropanol and the above mixture was subjected to ultrasonic treatment at 50 W for 30 min to exfoliate the layered material to obtain a dispersion;
[0063] (3) The dispersion was centrifuged at 2000 rpm for 10 min, and the molybdenum disulfide two-dimensional sheet clear solution was carefully removed;
[0064] (4) high-speed centrifugation of the above clear liquid at 8000 rpm for 30 min to obtain a molybdenum disulfide two-dimensional material;
[0065] (5) Ultrasonic dispersion of the molybdenum disulfide two-dimensional material in ethanol, and repeating steps (3) and (4) multiple times to ensure complete removal of the liquid metal and unstripped molybdenum disulfide, thereby obtaining a pure molybdenum disulfide two-dimensional material.
[0066] like Figure 3a and 3b They are the AFM characterization results and TEM characterization results of the exfoliated MoS2, and the results show that the MoS2 two-dimensional layer structure is successfully prepared, and the exfoliated MoS2 two-dimensional layer structure is defect-free and high-quality.
[0067] Example 3
[0068] The graphite exfoliation method comprises the following steps:
[0069] (1) Weigh 100 mg of graphite powder, add 300 mg of liquid metal gallium (Ga) dropwise under stirring, mix thoroughly and continue stirring for 24 hours;
[0070] (2) a mixed solution of 16 mL of ethanol and the above mixture was subjected to ultrasonic treatment at 50 W for 30 min to exfoliate the layered material to obtain a dispersion;
[0071] (3) The dispersion was centrifuged at 1000 rpm for 10 min, and the graphene two-dimensional sheet clear solution was carefully removed;
[0072] (4) high-speed centrifugation of the above clear liquid at 7000 rpm for 30 min to obtain a graphene two-dimensional material;
[0073] (5) Ultrasonic dispersion of the graphene two-dimensional material in ethanol, and repeating steps (3) and (4) multiple times to ensure complete removal of liquid metal and unexfoliated graphite, thereby obtaining a pure graphene two-dimensional material.
[0074] like Figure 4a and 4b They are the AFM characterization results and TEM characterization results of the exfoliated graphene, and the results show that the two-dimensional graphene sheet structure is successfully prepared, and the exfoliated graphene two-dimensional sheet structure is defect-free and high-quality.
[0075] The above content is a further detailed description of the present invention in combination with specific / preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, it can also make several substitutions or modifications to these described embodiments, and these substitutions or modifications should be regarded as belonging to the protection scope of the present invention. In the description of this specification, the description of the reference terms "an embodiment", "some embodiments", "preferred embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in combination with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily target the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In the absence of mutual contradiction, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples. Although the embodiments of the present invention and their advantages have been described in detail, it should be understood that various changes, substitutions and modifications can be made herein without departing from the scope of protection of the patent application.
Claims
1. A method for stripping a layered material, characterized in that: The steps include: (1) adding molten metal dropwise to layered material powder for mixing and stirring to obtain a mixture; (2) dispersing the mixture in a solvent to exfoliate the layered material to obtain a dispersion; (3) Centrifuging the dispersion to remove the molten metal and unpeeled layered materials to obtain a peeled two-dimensional material.
2. The stripping method according to claim 1, characterized in that: In step (1), the layered material is at least one of transition metal sulfide powder, graphite, hexagonal boron nitride, and layered minerals.
3. The stripping method according to claim 1, characterized in that: In step (1), the molten metal is at least one of indium, gallium-indium-tin alloy, and gallium.
4. The stripping method according to claim 1, characterized in that: In step (2), the solvent is at least one of ethanol, isopropanol, DMF and water.
5. The stripping method according to any one of claims 1 to 4, characterized in that: In step (1), the stirring speed is 100-600 rpm, the stirring time is 1-48 hours, and the mixing temperature is 20-70°C.
6. The stripping method according to any one of claims 1 to 4, characterized in that: In step (2), the mixture is dispersed in a solvent under ultrasonic conditions to carry out the exfoliation of the layered material. The ultrasonic time is 10-120 min and the ultrasonic power is 10-100 W.
7. The stripping method according to any one of claims 1 to 4, characterized in that: Step (3) comprises the following steps: (3.1) centrifuging the dispersion at a low speed and collecting the supernatant; (3.2) subjecting the supernatant of step (3.1) to high-speed centrifugation to collect the precipitate; (3.3) Ultrasonic dispersion of the precipitate collected in step (3.2) in a solvent, and repeating steps (3.1) and (3.2) multiple times until a pure exfoliated two-dimensional material is obtained.
8. The stripping method according to claim 7, characterized in that: The speed of the low-speed centrifugation in step (3.1) is 1000-3000 rpm, and the time is 5-10 min; the speed of the high-speed centrifugation in step (3.2) is 6000-9000 rpm, and the time is 10-30 min.
9. The stripping method according to any one of claims 1 to 4, characterized in that: In step (1), the molar ratio of the layered material to the molten metal is 5:1-1:
1.
10. The stripping method according to any one of claims 1 to 4, characterized in that: In step (2), each milliliter of the solvent contains 2.5 mg to 250 mg of the mixture.
Citation Information
Cited By
Two-dimensional fullerene and alkali metal intercalation stripping method and application thereof
CN121020566A