O3, O2 and T2 type lithium battery positive electrode material as well as ultrasonic-assisted liquid-phase ion exchange preparation method and application thereof

By using an ultrasonic-assisted liquid-phase Li+/Na+ ion exchange method, the problem of controlling oxygen stacking mode in existing technologies has been solved, enabling the preparation of various layered structures and improving the performance and consistency of lithium-ion battery cathode materials.

CN118954627AActive Publication Date: 2024-11-15XI AN JIAOTONG UNIV +1

Patent Information

Application Number
CN202411033946.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Existing technologies cannot effectively control the oxygen stacking mode in layered structures, resulting in the production of lithium-ion battery materials with only one O3 configuration, which limits the improvement of material performance.

Method used

By employing an ultrasonic-assisted liquid-phase Li+/Na+ ion exchange method, sodium-containing layered oxides were synthesized through high-temperature calcination, and then subjected to liquid-phase ion exchange with lithium salt solutions under ultrasonic conditions to prepare O3, O2, and T2 type lithium battery cathode materials.

Benefits of technology

Effective control over the oxygen stacking mode in the layered structure was achieved, enabling the preparation of thermodynamically stable O3 phase, metastable O2 phase, and lithium-depleted T2 phase layered structures. The material has uniform particle distribution, controllable particle size, and excellent electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954627A_ABST
    Figure CN118954627A_ABST
Patent Text Reader

Abstract

The invention discloses an O3, O2 and T2 type lithium battery positive electrode material as well as an ultrasonic-assisted liquid-phase ion exchange preparation method and application thereof. According to the invention, a liquid-phase ion exchange method is adopted to ensure that the reaction temperature, time and ion concentration are highly controllable, and the exchange process is uniform and sufficient; and mechanical vibration is generated by utilizing ultrasonic waves to assist Li < + > / Na < + > ion exchange in a liquid phase environment, so that the ion transmission efficiency is enhanced, and the uniformity and consistency of the exchange process are ensured. Therefore, effective regulation and control of an oxygen accumulation mode in the layered structure can be realized, a thermodynamically stable O3 phase layered structure, a metastable O2 phase layered structure and a lithium-poor T2 phase layered structure can be prepared by changing conditions such as ultrasonic frequency and ultrasonic-assisted time, and the prepared oxide particles are all composed of micron-sized particles, so that the preparation method is simple and easy to implement. The prepared material has the advantages of controllable particle size, good consistency, excellent cycling stability and wide application range, and can be widely applied to the electronic product and power automobile market.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion battery positive electrode materials, and specifically relates to an O3, O2 and T2 type lithium battery positive electrode material and an ultrasonic-assisted liquid-phase ion exchange preparation method and application thereof. Background Art

[0002] Lithium-ion batteries have developed most rapidly in the field of electrochemical energy storage due to their advantages such as high energy density, low self-discharge and low memory effect. Among the various components of lithium-ion batteries, the positive electrode material controls the energy density of lithium electricity and occupies a high cost, which has a great impact on the overall performance and cost of lithium-ion batteries. Therefore, the development of positive electrode materials is the key to the success of lithium-ion batteries. Among the many positive electrode materials for lithium-ion batteries, lithium cobalt oxide (LiCoO2) exhibits good electrochemical performance, but its cost is high and it has certain toxicity; lithium nickel oxide (LiNiO2) has poor cycle performance and thermal stability; the three elements of nickel, cobalt and manganese in lithium nickel cobalt manganese oxide Li(Ni,Co,Mn)O2 can be balanced and regulated in terms of specific energy, cyclability, safety and cost. Different configurations will bring different performance to the material, but due to the removal and insertion of Li ions during the charge and discharge process, the structure of the positive electrode material will change, accompanied by irreversible Li loss, which will trigger a series of phase changes, resulting in voltage decay and poor rate performance, which seriously restricts the further application of this type of positive electrode material.

[0003] The preparation of layered positive electrode materials is generally divided into two steps: wet chemical method to prepare precursors and high-temperature solid-phase method to prepare the final lithium-embedded oxide. However, high-temperature calcination generally produces thermodynamically stable O3 phase layered materials, and the space for regulating the oxygen accumulation mode in the layered structure is limited. Summary of the invention

[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide an O3, O2 and T2 type lithium battery positive electrode material and an ultrasonic-assisted liquid-phase ion exchange preparation method and application thereof, which can effectively solve the technical problem that the existing method can only prepare an O3 configuration lithium ion battery material due to the inability to effectively regulate the oxygen accumulation mode in the layered structure.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The invention discloses a method for preparing O3, O2 and T2 type lithium battery positive electrode materials by ultrasonic assisted liquid phase ion exchange. + / Na + Ion exchange method, the method includes:

[0007] First, sodium-containing layered oxide Na is synthesized by high-temperature calcination.m [Li x Ni y Co z Mn 1-x-y-z ]O2, and then immersed it in a solution containing lithium salt, and carried out liquid phase ion exchange treatment under ultrasonic conditions. The product was filtered, washed and dried to obtain O3, O2 and T2 structure lithium ion battery positive electrode layered oxide material Li m [Li x Ni y Co z Mn 1-x-y-z ]O2;

[0008] Among them, 0.50≤m≤1.00, 0.00≤x≤0.33; 0.00≤y≤1.00; 0.00≤z≤1.00.

[0009] The present invention discloses a method for preparing O3, O2 and T2 type lithium battery positive electrode materials by ultrasonic-assisted liquid phase ion exchange, comprising the following steps:

[0010] 1) High temperature calcination

[0011] According to the chemical formula Na m [Li x Ni y Co z Mn 1-x-y-z ]O2 ratio, take sodium source, lithium source, nickel source, cobalt source and manganese source, mix them evenly, then pre-sinter at 400-600℃ for 2-8h, then calcine at 700-900℃ for 5-25h, and cool naturally to room temperature to obtain P3 and P2 type sodium ion battery layered oxide Na m [Li x Ni y Co z Mn 1-x-y-z ]O2; where 0.50≤m≤1.00, 0.00≤x≤0.33, 0.00≤y≤1.00; 0.00≤z≤1.00;

[0012] 2) Ion exchange

[0013] The sodium ion battery layered oxide Na prepared in step 1) m [Li x Ni y Co z Mn 1-x-y-z]O2 and a lithium salt solution with a concentration of 0.5 to 10 mol / L are treated with liquid phase ion exchange for 0.5 to 10 hours at a reaction temperature of 60 to 180°C with the assistance of ultrasound with a frequency of 15 to 120 kHz, and then centrifuged, washed and dried to collect the resulting products, namely O3, O2 and T2 type lithium battery positive electrode material Li m [Li x Ni y Co z Mn 1-x-y-z ]O2.

[0014] Preferably, in step 1), the sodium source is Na2CO3 or NaOH; the lithium source is Li2CO3 or LiOH·H2O; the nickel source is NiO or NiCO3; the cobalt source is Co3O4, Co2O3 or CoCO3; and the manganese source is MnO, MnO2 or MnCO3.

[0015] Preferably, in step 1), the sintering system is: starting from room temperature, heating to 400-600° C. at a heating rate of 3-10° C. / min, pre-burning for 2-8 hours, and then calcining at 700-900° C. for 5-25 hours.

[0016] Preferably, in step 2), the lithium salt is LiNO3, LiCl, LiOH·H2O or LiCH3COO.

[0017] Preferably, in step 2), the solvent of the lithium salt solution is water or ethanol.

[0018] Further preferably, the sodium ion battery layered oxide Na m [Li x Ni y Co z Mn 1-x-y-z ]The dosage ratio of O2 to lithium salt solution is 1 mg: (5~200) μL.

[0019] The present invention also discloses O3, O2 and T2 type lithium battery positive electrode materials prepared by the above method.

[0020] The oxygen accumulation mode in the layered structure of the positive electrode material for lithium-ion batteries has been effectively regulated, and it has a thermodynamically stable O3 phase layered structure, a metastable O2 phase layered structure, or a lithium-poor T2 phase layered structure.

[0021] Preferably, the ion exchange treatment is carried out under the assistance of ultrasound at a frequency of 75-120kHz to produce a thermodynamically stable O3 phase layered lithium battery positive electrode material;

[0022] Preferably, a metastable O2-phase layered lithium battery positive electrode material can be prepared by means of ultrasound with a frequency of 35-75kHz;

[0023] Preferably, a lithium-deficient T2-phase layered lithium battery positive electrode material can be prepared in less than 0.5 hours with the aid of low-frequency ultrasound of 15-35 kHz.

[0024] Preferably, O3, O2 and T2 type lithium battery positive electrode materials are all composed of micron-sized particles, the grain size distribution is between 1 and 10 microns, and the particle size is controllable.

[0025] The invention also discloses the application of the above-mentioned O3, O2 and T2 type lithium battery positive electrode materials in the preparation of lithium ion batteries.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The invention discloses a method for preparing the positive electrode material of lithium-ion batteries having O3, O2 and T2 structures, using liquid phase Li + / Na + Ion exchange method, firstly directly adopts the full dry method to mix and calcine at high temperature to produce sodium-containing layered oxide Na m [Li x Ni y Co z Mn 1-x-y-z ]O2, add it together with lithium salt solution into ultrasonic reactor for full mixing and liquid phase ion exchange treatment, and obtain O3, O2 and T2 type layered oxide Li after filtering, washing and drying. m [Li x Ni y Co z Mn 1-x-y-z On the one hand, directly preparing sodium oxide by mixing raw materials through a full dry method can improve the tap density of the material, and has the advantages of cheap and universal equipment, simple and mature process, energy saving, emission reduction, cost reduction and efficiency improvement; using liquid phase Li + / Na + The ion exchange preparation method provides an environment with highly controllable temperature, time and ion concentration, good ion diffusion effect, and fast, uniform and sufficient exchange process; on the other hand, ultrasonic wave is used to generate mechanical vibration to assist Li in the liquid environment. + / Na +Ion exchange enhances ion transfer efficiency, ensures the uniformity and consistency of the exchange process, reduces temperature and energy consumption, realizes controllable ion exchange at lower temperatures, and effectively regulates the oxygen accumulation mode in the layered structure by changing the ultrasonic frequency. It can not only prepare a thermodynamically stable O3 phase layered structure, but also a metastable O2 phase layered structure and a lithium-poor T2 phase layered structure, which are new structures that are difficult to prepare by traditional high-temperature solid-phase methods. The layered positive electrode material prepared by this method has excellent electrochemical properties, uniform particle distribution, controllable particle size, good batch uniformity, and the method is simple in process, easy to operate, and the material structure is stable and reliable.

[0028] The positive electrode material of lithium-ion battery with different layered structures prepared by the method of the present invention has excellent cycle performance. Under the conditions of 3.0-4.7V and 0.2C, the capacity retention rate of the material is still as high as more than 92% after 40 cycles, and can be widely used in the electronic products and power vehicle markets. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic structural diagram of an ultrasonic reactor device used in a method for preparing O3, O2 and T2 type lithium battery positive electrode materials by ultrasonic-assisted liquid phase ion exchange provided by the present invention;

[0030] In the figure, 1 is a stirring controller; 2 is an ultrasonic controller; 3 is an ultrasonic generator; 4 is a stirring paddle; 5 is a stirring motor; 6 is a reactor body; 7 is a jacket; and 8 is a feed port.

[0031] Figure 2 The first charge-discharge curve of the T2-type layered cathode material prepared in Example 1 of the present invention at a rate of 0.2C;

[0032] Figure 3 This is the X-ray diffraction spectrum of the T2-type layered positive electrode material prepared in Example 1 of the present invention;

[0033] Figure 4 This is a comparison chart of the X-ray diffraction spectra of the T2-type layered positive electrode material prepared in Example 1 of the present invention and the material obtained under the same conditions without ultrasonic assistance;

[0034] Figure 5 This is the X-ray diffraction spectrum of the O2-type layered positive electrode material prepared in Example 2 of the present invention;

[0035] Figure 6 The first charge-discharge curve of the O2-type layered cathode material prepared in Example 2 of the present invention at a 1C rate;

[0036] Figure 7 This is the X-ray diffraction spectrum of the O3-type layered positive electrode material prepared in Example 3 of the present invention;

[0037] Figure 8 The first charge-discharge curve of the O3-type layered cathode material prepared in Example 3 of the present invention at a 1C rate;

[0038] Fig. 9 The first charge-discharge curve of the O2-type layered cathode material prepared in Example 4 of the present invention at a rate of 0.1C;

[0039] Fig.10 The cycle performance of the O2 / O3 composite layered cathode material prepared in Example 5 of the present invention;

[0040] Fig.11 This is the X-ray diffraction spectrum of the O3-type layered positive electrode material prepared in Example 6 of the present invention;

[0041] Fig.12 This is a scanning electron microscope image of the O3 type layered positive electrode material prepared in Example 7 of the present invention. DETAILED DESCRIPTION

[0042] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0043] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0044] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0045] See also Figure 1, is a schematic diagram of the structure of an ultrasonic reactor device used in the method for preparing O3, O2 and T2 type lithium battery positive electrode materials by ultrasonic-assisted liquid phase ion exchange described in the following embodiments of the present invention. The reaction device is designed by combining the existing ultrasonic generator and stirring tank on the market.

[0046] Example 1

[0047] The positive electrode material prepared in this embodiment is LiCoO2.

[0048] A method for preparing a positive electrode material for a T2 structure lithium-ion battery comprises the following steps:

[0049] Step 1. High temperature calcination:

[0050] According to the chemical formula NaCoO2, the molar ratio of sodium to cobalt is 1.0:1.0. The corresponding Na2CO3 and Co2O3 are weighed respectively, mixed evenly in a ball mill, and then placed in a muffle furnace. The temperature is increased to 500°C at a heating rate of 5°C / min in an air atmosphere, pre-burned for 6h, and then increased to 800°C at a heating rate of 10°C / min, calcined for 18h, and naturally cooled to room temperature to obtain P2 type sodium ion battery layered oxide NaCoO2;

[0051] Step 2. Ion exchange:

[0052] The P2 type sodium ion battery layered oxide NaCoO2 obtained in step 1 is immersed in a 0.5 mol / L LiOH·H2O aqueous solution, the ratio of the sodium ion layered oxide to the LiOH·H2O solution is 1:5 mg / μL, and added into an ultrasonic reactor. At a reaction temperature of 90°C, liquid phase ion exchange treatment is carried out with the aid of ultrasound at a frequency of 15 kHz for 0.5 h, followed by centrifugation and washing with ethanol for 3 times. The product obtained by drying and collecting is the T2 type lithium ion battery positive electrode layered oxide LiCoO2.

[0053] The charging and discharging performance test process of the positive electrode material prepared in this embodiment is as follows:

[0054] A certain amount of the positive electrode material prepared in this embodiment, acetylene black, and binder polyvinylidene fluoride (PVDF) were weighed in a mass ratio of 8:1:1, added to N-methylpyrrolidone (NMP) to form a slurry, the content of NMP was 30 times that of PVDF, and evenly coated on an aluminum foil. The mixture was vacuum dried at 80° C. for 12 hours, and then cut into pole pieces with a diameter of 12 mm using a mold; a metal lithium sheet was used as a negative electrode, a Celgard 2400 commercial polypropylene film was used as a separator, and an electrolyte was LP30. The mixture was assembled into a button cell of model CR2032 in a glove box filled with inert gas.

[0055] The T2-type lithium ion layered oxide elements prepared in this embodiment are evenly distributed in the grains, and the particle size is about 5 μm. The XRD pattern of LiCoO2 prepared in this embodiment is shown in FIG. Figure 2 From the XRD graph, it can be seen that all diffraction peaks belong to the T2 type layered structure. Under the same conditions in this embodiment, the XRD comparison graphs of the materials prepared with and without ultrasonic assistance are shown in FIG. Figure 3 It can be seen that the diffraction peaks of the material prepared without ultrasonic assistance belong to the mixed phase structure of P2 and T2, and the ion exchange is incomplete.

[0056] Charge and discharge performance test: The T2 phase layered cathode material LiCoO2 prepared in this example was tested at a voltage range of 3.0-4.65 V and 0.2 C. The first charge and discharge capacities were 171.4 mAh / g and 219.4 mAh / g, respectively. Figure 4 shown.

[0057] Example 2

[0058] The positive electrode material prepared in this embodiment is LiCoO2.

[0059] A method for preparing an O2 structure lithium-ion battery positive electrode material comprises the following steps:

[0060] Step 1. High temperature calcination:

[0061] According to the chemical formula NaCoO2, the molar ratio of sodium to cobalt is 1.0:1.0. The corresponding Na2CO3 and Co2O3 are weighed respectively, mixed evenly in a ball mill, and then placed in a muffle furnace. The temperature is increased to 500°C at a heating rate of 5°C / min in an air atmosphere, pre-burned for 6h, and then increased to 800°C at a heating rate of 10°C / min, calcined for 18h, and naturally cooled to room temperature to obtain P2 type sodium ion battery layered oxide NaCoO2;

[0062] Step 2. Ion exchange:

[0063] The P2 type sodium ion battery layered oxide NaCoO2 obtained in step 1 is immersed in a 0.5 mol / L LiOH·H2O aqueous solution, the ratio of the sodium ion layered oxide to the LiOH·H2O solution is 1:5 mg / μL, and then added into an ultrasonic reactor. At a reaction temperature of 90°C, liquid phase ion exchange treatment is carried out with the aid of ultrasound at a frequency of 75 kHz for 0.5 h, followed by centrifugation and washing with ethanol for 3 times. The product obtained by drying and collecting is the O2 type lithium ion battery positive electrode layered oxide LiCoO2.

[0064] The O2-type lithium ion layered oxide elements prepared in this embodiment are uniformly distributed in the grains, and the particle size is about 5 μm. The XRD pattern of LiCoO2 prepared in this embodiment is shown in FIG. Figure 5 From the XRD diagram, we can see that all the diffraction peaks belong to the O2-type layered structure with a space group of P6 3mc.

[0065] Charge and discharge performance test: The test method is the same as that of Example 1. The results show that the first charge and discharge capacities of the O2 structure cathode material prepared in this example are 233.7 mAh / g and 223.7 mAh / g at a voltage range of 3.0 to 4.7 V and 1C, respectively. Figure 6 .

[0066] Example 3

[0067] The positive electrode material prepared in this embodiment is LiCoO2.

[0068] A method for preparing an O3 structure lithium-ion battery positive electrode material comprises the following steps:

[0069] Step 1. High temperature calcination:

[0070] According to the chemical formula NaCoO2, the molar ratio of sodium to cobalt is 1.0:1.0. The corresponding Na2CO3 and Co2O3 are weighed respectively, mixed evenly in a ball mill, and then placed in a muffle furnace. The temperature is increased to 500°C at a heating rate of 5°C / min in an air atmosphere, pre-burned for 6h, and then increased to 800°C at a heating rate of 10°C / min, calcined for 18h, and naturally cooled to room temperature to obtain P2 type sodium ion battery layered oxide NaCoO2;

[0071] Step 2. Ion exchange:

[0072] The P2 type sodium ion battery layered oxide NaCoO2 obtained in step 1 is immersed in a 0.5 mol / L LiOH·H2O aqueous solution, the ratio of the sodium ion layered oxide to the LiOH·H2O solution is 1:5 mg / μL, and then added into an ultrasonic reactor. At a reaction temperature of 90°C, liquid phase ion exchange treatment is carried out with the aid of ultrasound at a frequency of 120 kHz for 0.5 h, followed by centrifugation and washing with ethanol for 3 times. The product obtained by drying and collecting is the O3 type lithium ion battery positive electrode layered oxide LiCoO2.

[0073] The O3 type lithium ion layered oxide elements prepared in this embodiment are evenly distributed in the grains, and the particle size is about 5 μm. The XRD pattern of LiCoO2 prepared in this embodiment is shown in FIG. Figure 7 From the XRD diagram, we can see that all the diffraction peaks belong to the O3-type layered structure with a space group of R3m.

[0074] Charge and discharge performance test: The test method is the same as that of Example 1. The results show that the first charge and discharge capacities of the O3 structure positive electrode material prepared in this example are 225.4 mAh / g and 213 mAh / g at a voltage range of 3.0 to 4.7 V and 1C, respectively. Figure 8 .

[0075] Example 4

[0076] The positive electrode material prepared in this embodiment is Li[Li 0.15 Ni 0.25 Mn 0.6 ]O2.

[0077] A method for preparing an O2 structure lithium-ion battery positive electrode material comprises the following steps:

[0078] Step 1. High temperature calcination:

[0079] According to the chemical formula Na[Li 0.15 Ni 0.25 Mn 0.6 ]O2 ingredients, the molar ratio of sodium, lithium, nickel and manganese elements is 1.0:0.15:0.25:0.60, the corresponding Na2CO3, Li2CO3, NiO and MnO are weighed respectively, placed in a ball mill and mixed evenly, and then placed in a muffle furnace, heated to 400℃ at a heating rate of 6℃ / min in an air atmosphere, pre-burned for 6h, and then heated to 700℃ at a heating rate of 10℃ / min, calcined for 15h, and naturally cooled to room temperature to obtain P2 type sodium ion battery layered oxide Na[Li 0.15 Ni 0.25 Mn 0.6 ]O2;

[0080] Step 2. Ion exchange:

[0081] The P2-type layered oxide Na[Li 0.15 Ni 0.25 Mn 0.6 ]O2 was immersed in a 3.0 mol / L LiOH·H2O aqueous solution, the ratio of sodium ion layered oxide to LiOH·H2O aqueous solution was 1:50 mg / μL, added to an ultrasonic reactor, and liquid phase ion exchange treatment was carried out for 4 hours at a reaction temperature of 60°C with the assistance of ultrasound at a frequency of 75 kHz, followed by centrifugation and washing with ethanol for 3 times. The product obtained by drying and collecting is the positive electrode layered oxide Li[Li 0.15 Ni 0.25 Mn 0.6 ]O2.

[0082] The electrochemical performance test of the battery was carried out at a voltage range of 2.0 to 4.8 V and 0.1 C. The results showed that the positive electrode material Li[Li 0.15 Ni 0.25 Mn 0.6 ]O2 has a first charge and discharge capacity of 178 mAh / g and 218 mAh / g at a rate of 0.1C. Fig. 9 shown.

[0083] Example 5

[0084] The positive electrode material prepared in this embodiment is Li 2 / 3 □ 1 / 3 [Co 0.5 Mn 0.5 ]O2. Note: “□” in the formula means a vacancy.

[0085] A method for preparing an O3 / O2 mixed structure lithium ion battery positive electrode material comprises the following steps:

[0086] Step 1. High temperature calcination:

[0087] According to the chemical formula Na 2 / 3 □ 1 / 3 [Co 0.5 Mn 0.5 ]O2 ingredients, the molar ratio of sodium, cobalt and manganese elements is 0.67:0.50:0.50, the corresponding NaOH, CoCO3 and MnCO3 are weighed respectively, placed in a ball mill and mixed evenly, and then placed in a muffle furnace, heated to 450°C at a heating rate of 3°C / min in an air atmosphere, pre-burned for 2h, and then heated to 750°C at a heating rate of 5°C / min, calcined for 5h, and naturally cooled to room temperature to obtain P3 and P2 mixed sodium ion battery layered oxide Na 2 / 3 □ 1 / 3 [Co 0.5 Mn 0.5 ]O2;

[0088] Step 2. Ion exchange:

[0089] The P3 / P2 hybrid sodium ion battery layered oxide Na obtained in step 1 2 / 3 □ 1 / 3 [Co 0.5 Mn 0.5]O2 was immersed in a 5.5mol / L LiCl solution, the solvent was ethanol, the ratio of sodium ion layered oxide to LiCl solution was 1:100mg / μL, and added to an ultrasonic reactor. At a reaction temperature of 120°C, liquid-phase ion exchange treatment was first performed for 2h without ultrasonic assistance, and then for 2h with ultrasonic assistance at a frequency of 90kHz. Then, it was centrifuged and washed with ethanol three times. The product obtained by drying and collecting was a mixed lithium ion layered oxide LiO3 and O2. 2 / 3 □ 1 / 3 [Co 0.5 Mn 0.5 ]O2.

[0090] The O3 / O2 mixed lithium ion layered oxide particles prepared in this embodiment are about 6 μm and have a uniform particle size distribution.

[0091] Charge and discharge performance test: The test method is the same as that of Example 1. The results show that the first discharge capacity of the O3 / O2 mixed lithium ion layered positive electrode material prepared in this example is 198 mAh / g at 2.0-4.8 V and 0.1 C. After 25 cycles, the capacity is still 186 mAh / g. Fig.10 .

[0092] Example 6

[0093] The positive electrode material prepared in this embodiment is Li[Li 1 / 3 Mn 2 / 3 ]O2.

[0094] A method for preparing an O3 structure lithium-ion battery positive electrode material comprises the following steps:

[0095] Step 1. High temperature calcination:

[0096] According to the chemical formula Na[Li 1 / 3 Mn 2 / 3 ]O2 ingredients, the molar ratio of sodium, lithium and manganese elements is 1.0:0.33:0.67, the corresponding NaOH, LiOH·H2O and MnCO3 are weighed respectively, placed in a ball mill and mixed evenly, and then placed in a muffle furnace, heated to 600℃ at a heating rate of 3℃ / min in an air atmosphere, pre-burned for 8h, and then heated to 800℃ at a heating rate of 8℃ / min, calcined for 25h, and naturally cooled to room temperature to obtain O3 type sodium ion battery layered oxide Na[Li 1 / 3 Mn 2 / 3 ]O2;

[0097] Step 2. Ion exchange:

[0098] The O3-type sodium ion battery layered oxide Na[Li1 / 3 Mn 2 / 3 ]O2 was immersed in a 7.5mol / L LiNO3 solution, the solvent was ethanol, the ratio of sodium ion layered oxide to LiNO3 solution was 1:150mg / μL, added to an ultrasonic reactor, and liquid phase ion exchange treatment was carried out for 4 hours at a reaction temperature of 120℃ under the assistance of ultrasound at a frequency of 90kHz, followed by centrifugation and washing with ethanol for 3 times. The product obtained by drying and collecting is the positive electrode layered oxide Li[Li 1 / 3 Mn 2 / 3 ]O2.

[0099] The oxide Li[Li 1 / 3 Mn 2 / 3 ]XRD of O2 Fig.11 ,From the figure, we can see that all the diffraction peaks belong to the O3 type layered structure, the space group is C2 / m, and the diffraction peak around 22° is a honeycomb superlattice structure.

[0100] Charge and discharge performance test: The test method is the same as that in Example 1. The results show that the first discharge capacity of the O3-type lithium-ion layered positive electrode material prepared in this example at 0.1C is 205 mAh / g.

[0101] Example 7

[0102] The positive electrode material prepared in this embodiment is Li 0.5 MnO2.

[0103] A method for preparing an O3 structure lithium-ion battery positive electrode material comprises the following steps:

[0104] Step 1. High temperature calcination:

[0105] According to the chemical formula Na 0.5 The molar ratio of sodium and manganese elements is 0.50:1.0. The corresponding Na2CO3 and MnO2 are weighed respectively, placed in a ball mill and mixed evenly, and then placed in a muffle furnace. The temperature is increased to 550℃ at a heating rate of 4℃ / min in an air atmosphere, pre-burned for 4h, and then heated to 900℃ at a heating rate of 4℃ / min, calcined for 5h, and naturally cooled to room temperature to obtain P3 type sodium ion battery layered oxide Na 0.5 MnO2;

[0106] Step 2. Ion exchange:

[0107] The P3 type sodium ion battery layered oxide Na obtained in step 1 0.5MnO2 was immersed in a 10.0 mol / L LiCH3COO aqueous solution, the ratio of sodium ion layered oxide to LiCH3COO aqueous solution was 1:200 mg / μL, added to an ultrasonic reactor, and treated with 120 kHz ultrasonic-assisted liquid phase ion exchange at a reaction temperature of 90°C for 10 h, followed by centrifugation and washing with ethanol three times. The product was dried and collected to obtain the positive electrode layered oxide Li O3 type lithium ion battery. 0.5 MnO2.

[0108] The morphology of the lithium ion layered oxide prepared in this example is shown in Fig.12 ,From the figure, we can see that the particles are mainly hexagonal, evenly distributed, and the particle size is about 2μm.

[0109] Charge and discharge performance test: The test method is the same as that in Example 1. The results show that the first discharge capacity of the O3 structure positive electrode material prepared in this example at 0.1C reaches 195 mAh / g.

[0110] In summary, the method of the present invention first directly prepares sodium-containing oxides by mixing raw materials through a fully dry method, which can improve the tap density of the material and has the advantages of simple and mature process, energy saving, emission reduction, cost reduction and efficiency improvement; secondly, liquid phase ion exchange is adopted to provide an environment with highly controllable temperature, time and ion concentration, good ion diffusion effect, and fast, uniform and sufficient exchange process; finally, ultrasonic wave is used to generate mechanical vibration to assist Li in the liquid environment + / Na + Ion exchange can enhance the efficiency of ion transmission, ensure the uniformity and consistency of the exchange process, reduce temperature and energy consumption, realize controllable ion exchange at a lower temperature, and ensure the effective regulation of the oxygen accumulation mode in the layered structure. Therefore, it is possible to effectively regulate the oxygen accumulation mode in the layered structure. By changing the ultrasonic frequency, ultrasonic auxiliary time and other conditions, not only can thermodynamically stable O3 phase layered oxides be prepared, but also metastable O2 phase layered structures and lithium-poor T2 phase layered structures can be prepared. The prepared oxide particles are all composed of micron-sized particles, with a grain size distribution between 1 and 10 microns, controllable particle size, good consistency, excellent cycle stability, and a wide range of use (4.3 to 4.7V), which can be widely used in the electronic products and power vehicle markets.

[0111] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing O3, O2 and T2 type lithium battery positive electrode materials by ultrasonic assisted liquid phase ion exchange, characterized in that: include: First, sodium-containing layered oxide Na is synthesized by high-temperature calcination. m [Li x Ni y Co z Mn 1-x-y-z ]O2, and then immersed it in a solution containing lithium salt, and carried out liquid phase ion exchange treatment under ultrasonic conditions. The product was filtered, washed and dried to obtain O3, O2 and T2 structure lithium ion battery positive electrode layered oxide material Li m [Li x Ni y Co z Mn 1-x-y-z ]O2; Among them, 0.50≤m≤1.00, 0.00≤x≤0.33; 0.00≤y≤1.00; 0.00≤z≤1.

00.

2. The method for preparing O3, O2 and T2 type lithium battery positive electrode materials by ultrasonic-assisted liquid phase ion exchange according to claim 1, characterized in that: The following steps are involved: 1) According to the chemical formula Na m [Li x Ni y Co z Mn 1-x-y-z ]O2 ratio, take sodium source, lithium source, nickel source, cobalt source and manganese source, mix them evenly, then pre-sinter at 400-600℃ for 2-8h, then calcine at 700-900℃ for 5-25h, and cool naturally to room temperature to obtain P3 and P2 type sodium ion battery layered oxide Na m [Li x Ni y Co z Mn 1-x-y-z ]O2; where 0.50≤m≤1.00, 0.00≤x≤0.33, 0.00≤y≤1.00; 0.00≤z≤1.00; 2) The sodium ion battery layered oxide Na prepared in step 1) m [Li x Ni y Co z Mn 1-x-y-z ]O2 and a lithium salt solution with a concentration of 0.5 to 10 mol / L are treated with liquid phase ion exchange for 0.5 to 10 hours at a reaction temperature of 60 to 180°C with the assistance of ultrasound with a frequency of 15 to 120 kHz, and then centrifuged, washed and dried to collect the resulting products, namely O3, O2 and T2 type lithium battery positive electrode material Li m [Li x Ni y Co z Mn 1-x-y-z ]O2.

3. The method for preparing O3, O2 and T2 type lithium battery positive electrode materials by ultrasonic-assisted liquid phase ion exchange according to claim 2, characterized in that: In step 1), the sodium source is Na2CO3 or NaOH; the lithium source is Li2CO3 or LiOH·H2O; the nickel source is NiO or NiCO3; the cobalt source is Co3O4, Co2O3 or CoCO3; and the manganese source is MnO, MnO2 or MnCO3.

4. The method for preparing O3, O2 and T2 type lithium battery positive electrode materials by ultrasonic-assisted liquid phase ion exchange according to claim 2, characterized in that: In step 1), the sintering system is: starting from room temperature, heating to 400-600° C. at a heating rate of 3-10° C. / min, pre-burning for 2-8 hours, and then calcining at 700-900° C. for 5-25 hours.

5. The method for preparing O3, O2 and T2 type lithium battery positive electrode materials by ultrasonic-assisted liquid phase ion exchange according to claim 2, characterized in that: In step 2), the lithium salt is LiNO3, LiCl, LiOH·H2O or LiCH3COO.

6. The method for preparing O3, O2 and T2 type lithium battery positive electrode materials by ultrasonic-assisted liquid phase ion exchange according to claim 2, characterized in that: In step 2), the solvent of the lithium salt solution is water or ethanol.

7. The method for preparing O3, O2 and T2 type lithium battery positive electrode materials by ultrasonic-assisted liquid phase ion exchange according to claim 6, characterized in that: The sodium ion battery layered oxide Na m [Li x Ni y Co z Mn 1-x-y-z ]The dosage ratio of O2 to lithium salt solution is 1 mg: (5~200) μL.

8. O3, O2 and T2 type lithium battery positive electrode materials prepared by the method according to any one of claims 1 to 7, characterized in that: The prepared O3 type lithium battery positive electrode material has a thermodynamically stable O3 phase layer; the prepared O2 type lithium battery positive electrode material has a metastable O2 phase layer; and the prepared T2 type lithium battery positive electrode material has a lithium-deficient T2 phase layer structure.

9. The O3, O2 and T2 type lithium battery positive electrode material according to claim 8, characterized in that: O3, O2 and T2 lithium battery positive electrode materials are all composed of micron-sized particles, with grain sizes distributed between 1 and 10 microns, and the particle size is controllable.

10. Use of the O3, O2 and T2 type lithium battery positive electrode materials according to claim 8 or 9 in the preparation of lithium ion batteries.

Citation Information

Patent Citations

  • Ternary positive electrode material of lithium ion battery and preparation method of ternary positive electrode material

    CN114436345A

  • T2 type lithium cobalt oxide positive electrode material with space group of Cmca and preparation method of T2 type lithium cobalt oxide positive electrode material

    CN114784269A

  • Single-crystal lithium ion battery positive electrode material with different layered structures as well as preparation method and application of single-crystal lithium ion battery positive electrode material

    CN114956210A

  • Coated positive electrode material for sodium-ion battery and preparation method of coated positive electrode material

    CN117117167A

  • Modified sodium ion battery positive electrode material and preparation method and application thereof

    CN117712325A

Cited By

  • Lithium ion battery positive electrode layered oxide with prism-surface shared layered structure and preparation method and application of lithium ion battery positive electrode layered oxide

    CN119503897A

  • A facet-sharing layered structure lithium-ion battery positive electrode layered oxide and its preparation method and application

    CN119503897B

  • Triangular bipyramid vacancy layered oxide and application thereof in lithium battery

    CN121292533A

  • A triangular bipyramidal vacancy layered oxide and its application in lithium batteries

    CN121292533B

  • O2 type lithium ion layered oxide with coating layer and preparation method of O2 type lithium ion layered oxide

    CN121416459A