Rare-earth-doped LaAlO3-based wide-temperature-range high-stability negative-temperature-coefficient thermal sensitive ceramic material and thermistor and preparation method thereof
Through the solid phase reaction and process steps of rare earth doped lanthanum aluminate-based material, the problem of insufficient electrical properties and temperature resistance of NTC materials in high temperature zones is solved, and high stability and excellent electrical properties in wide temperature zones are achieved. In a high temperature environment of 500℃ to 1500℃.
Patent Information
- Application Number
- CN202411011521.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The existing materials with negative temperature coefficient in high temperature zones have limitations in electrical properties and temperature resistance, resulting in resistance drift, extended response time and insufficient temperature resistance when used in high temperature environments, which limits its application range and preparation process There are challenges such as microstructure control and uniform distribution of doped elements.
Using rare earth doped lanthanum aluminate (LaAlO3)-based material, made by solid phase reaction of lanthanum trioxide, aluminum trioxide, europium trioxide, digadolinium trioxide or diholmium trioxide, combined with ball milling and drying , calcination and isostatic pressing steps to prepare a wide temperature zone NTC ceramic material with high stability and excellent electrical properties.
High electrical performance and stability in the range of 500℃~1500℃, the resistance drift rate is less than 8% after aging at 1000℃ for 500 hours, and the lattice deformation and structural transformation of the material are enhanced by doping rare earth elements. , improves conductivity and high temperature stability.
Smart Images

Figure CN118955114A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrical materials, and specifically relates to a rare earth doped lanthanum aluminate (LaAlO3) based wide temperature range high stability negative temperature coefficient thermistor and a thermistor and a preparation method thereof. Background Art
[0002] With the rapid development of electronic technology, especially in the application of high temperature environment such as aerospace, automobile engine management, industrial furnace control, power system, the demand for high temperature negative temperature coefficient (NTC) materials is growing. The characteristics of this kind of material are that it maintains good electrical stability in high temperature environment, and its resistance value decreases with the increase of temperature. Therefore, they are widely used in temperature sensors, thermistors, overheat protection and temperature control.
[0003] However, existing high temperature zone NTC materials have certain limitations in terms of electrical performance and temperature resistance. On the one hand, many high temperature zone NTC materials will have unstable electrical performance during long-term high temperature use, such as drift of resistance value, prolonged response time and other problems, which will lead to a decrease in the accuracy of temperature control, thereby affecting the stability and reliability of the entire system. On the other hand, existing high temperature zone NTC materials often have poor temperature resistance and cannot work for a long time at extremely high temperatures, which limits their application range in high temperature environments.
[0004] In addition, the existing preparation process of NTC materials in the high temperature zone also has certain challenges. For example, the microstructure control of the material, the uniform distribution of doping elements, the optimization of the sintering process, etc., all of which will affect the electrical properties and stability of the final material. Therefore, the development of a new type of NTC material with excellent electrical properties and stability at high temperatures, as well as its efficient and controllable preparation method, has become an important research direction in the fields of materials science and electronic technology. Summary of the invention
[0005] The purpose of the present invention is to provide a rare earth doped lanthanum aluminate based negative temperature coefficient thermistor ceramic material with wide temperature range and high stability, which has good electrical properties and stability at high temperatures.
[0006] To achieve this purpose, the present invention adopts the following technical solution:
[0007] A rare earth doped LaAlO3 based wide temperature range high stability negative temperature coefficient thermistor ceramic material, the thermistor ceramic material is made of lanthanum trioxide, aluminum trioxide and europium trioxide, gadolinium trioxide, holmium trioxide or thulium trioxide by solid phase reaction according to weight percentage, and its chemical composition is La 0.9 X0.1 AlO3, wherein X = Eu, Gd, Ho or Tm.
[0008] The electrical performance parameters of the thermosensitive ceramic material are as follows: 700 / 1000k =213.39K~13564.1K,ρ 1000k =12.9×10 3 Ω·cm~13.3×10 5 Ω·cm, the applicable temperature range is 500℃~1500℃; after aging at high temperature of 1000℃ for 500 hours, the resistance drift rate ΔR / R0(%) is less than 8%.
[0009] The present invention further provides a method for preparing a rare earth-doped LaAlO3-based wide temperature range high stability negative temperature coefficient thermistor ceramic material, comprising the following steps:
[0010] a. Weigh the raw materials of lanthanum trioxide, aluminum trioxide and one of europium trioxide, gadolinium trioxide, holmium trioxide and thulium trioxide, respectively, mix them, ball-mill and dry them to obtain powders;
[0011] b. Heat the powder to 150-250℃, keep it at 150-250℃ for 0.5-1.5h, then heat it to 1200-1400℃, calcine it at 1200-1400℃ for 8-11h, with a heating rate of 1-3℃ / min; then cool it at a cooling rate of 1-3℃ / min to obtain La 0.9 X 0.1 AlO3 powder;
[0012] c.La 0.9 X 0.1 The AlO3 powder is subjected to secondary ball milling and drying to obtain rare earth doped LaAlO3 based wide temperature range high stability negative temperature coefficient thermistor ceramic material powder.
[0013] Preferably, in step a and step c, the grinding medium used in ball milling is agate balls, and the ball milling medium is ethanol.
[0014] Preferably, in step a, the ball mill rotates clockwise at 300 rpm for 40 minutes, stops for 20 minutes, and then rotates counterclockwise at 300 rpm for 40 minutes, and repeats this process for 8 hours.
[0015] Preferably, in step a and step c, the drying temperature is 90°C.
[0016] Preferably, in step c, the ball milling time is 5-7 hours.
[0017] The present invention further provides a method for preparing a thermistor using the rare earth doped LaAlO3-based wide temperature range high stability negative temperature coefficient thermistor ceramic material, the method comprising the following steps:
[0018] The powder of rare earth doped LaAlO3 based wide temperature range high stability negative temperature coefficient thermistor ceramic material is pressed into a circular sheet, and cold isostatically pressed for 170-190s; then kept at 1550-1650℃ for 18-22h to obtain a circular sheet-shaped wide temperature range high stability thermistor ceramic material; finally, platinum slurry electrodes are coated on both sides of the circular sheet-shaped wide temperature range high stability thermistor ceramic material, annealed and cooled to room temperature to obtain a wide temperature range high stability negative temperature coefficient thermistor.
[0019] Preferably, the cold isostatic pressing pressure is 250-350 MPa.
[0020] According to a preferred embodiment of the present invention, the present invention adopts a rare earth element doping method to prepare La 0.9 X 0.1 AlO3 (X = Eu, Gd, Ho, Tm) thermistor ceramic material and further prepared LaAlO3 ceramic resistor, the preparation method includes:
[0021] a. First, accurately weigh high-purity lanthanum oxide, aluminum oxide, europium oxide, gadolinium oxide, holmium oxide and thulium oxide to ensure that they are mixed according to the stoichiometric ratio.
[0022] b. Next, the powders were placed in a ball mill, using agate balls as grinding media and ethanol as a dispersant. The ball mill was first rotated clockwise at 300 revolutions per minute for 40 minutes, then paused for 20 minutes, and then rotated counterclockwise for 40 minutes. This cycle was repeated for a total of 8 hours.
[0023] c. After ball milling, place the mixed powder in a drying oven and dry it at 90°C. Then, heat the dried powder to 200°C and keep it at this temperature for 1 hour. Then, continue to heat it to 1300°C and calcine it at this temperature for 10 hours, with the heating rate set at 2°C per minute. After calcination, cool the powder at the same rate of 2°C per minute.
[0024] d. The calcined and cooled powder was put into the ball mill again, ground for 6 hours, and then dried. The powder was squeezed into a circular sheet with a diameter of 10 mm and a thickness of 2 mm using a pressure of 20 MPa, and then maintained at an isostatic pressure of 300 MPa for 180 seconds.
[0025] e. Finally, the extruded circular sheet is kept at a temperature of 1600°C for 20 hours, and the heating and cooling rate is also kept at 2°C per minute. After these steps, the final ceramic sample is prepared.
[0026] The present invention compresses the powder into tablets for sintering and densification, and coats the platinum slurry electrode for more accurate testing.
[0027] Compared with the prior art, the rare earth doped high temperature zone NTC material of the present invention has the following advantages:
[0028] 1. Through the addition of rare earth elements, LaAlO3-based ceramics will undergo lattice deformation and structural transformation in a specific high temperature range, which directly leads to the enhancement of the electrical properties and stability of the material.
[0029] 2. The complex impedance measurement results show that La 0.9 X 0.1 The resistive behavior of AlO3 is mainly controlled by the grain size and the characteristics of the grain boundaries, showing excellent electrical stability.
[0030] 3. Photoluminescence (PL) analysis revealed that the introduction of rare earth elements enhanced the charge transfer process between rare earth ions and oxygen ions. In particular, the doping of europium (Eu) significantly improved the optical properties of the material, providing valuable insights into the luminescence properties of the material and its potential application in optical temperature sensing.
[0031] 4. The high temperature tolerance test results show that in a low temperature environment, electron transition becomes difficult due to the higher activation energy, while in a high temperature environment, electron transition becomes easier and the activation energy is reduced, thereby enhancing the conductivity and high temperature stability of the material.
[0032] 5. Density functional theory (DFT) calculation analysis shows that the doping of rare earth elements effectively reduces the band gap width of the material and increases the number of carriers, thereby improving the conductivity and optimizing the NTC characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The XRD diagram of the present invention shows that the diffraction peaks of different elements all match the LaAlO3 structure very well, indicating that all elements are well doped into LaAlO3;
[0034] Figure 2 For the present invention La 0.9 X 0.1 B of AlO3 thermal sensitive ceramic materials and LaAlO3 700 / 1000k Value and 1000K relationship diagram;
[0035] Figure 3 For the present invention La 0.9 X 0.1 Aging relationship diagram of AlO3 thermistor ceramic material and LaAlO3 material. DETAILED DESCRIPTION
[0036] The technical solution of the present invention is described in detail below with reference to the accompanying drawings and embodiments.
[0037] Example 1
[0038] A method for preparing a rare earth doped lanthanum aluminate based wide temperature range high stability negative temperature coefficient thermistor and a thermistor, the preparation method comprising the following steps:
[0039] a. According to La 0.9 Eu 0.1 The weight percentage is calculated according to the stoichiometric ratio of AlO3, and 68.08% of lanthanum trioxide, 23.74% of aluminum trioxide, and 8.17% of europium trioxide are weighed and mixed according to the weight percentage;
[0040] b. Place the powder prepared in step a into a ball mill, using agate balls as grinding media and ethanol as a dispersant. The ball mill first rotates clockwise at 300 revolutions per minute for 40 minutes, then pauses for 20 minutes, and then rotates counterclockwise for 40 minutes. This cycle is repeated for a total of 8 hours. After ball milling, place the obtained mixed powder in a drying oven and dry it at 90°C. Subsequently, heat the dried powder to 200°C and maintain it at this temperature for 1 hour. After that, continue to heat to 1300°C and calcine at this temperature for 10 hours, with the heating rate set to 2°C per minute. After calcination is completed, cool the powder at the same rate of 2°C per minute to obtain La. 0.9 Eu 0.1 AlO3 powder.
[0041] c. Resuspend the La obtained in step b 0.9 Eu 0.1 The AlO3 powder is put into the ball mill again, ground for 6 hours, and then dried to obtain a rare earth doped lanthanum aluminate based wide temperature range high stability negative temperature coefficient thermistor ceramic material.
[0042] d. Use a pressure of 20 MPa to squeeze the powder into a circular sheet with a diameter of 10 mm and a thickness of 2 mm, and then keep it under an isostatic pressure of 300 MPa for 180 seconds. Finally, keep the extruded circular sheet at a temperature of 1600°C for 20 hours, and the heating and cooling speed is also maintained at 2°C per minute to obtain a high-temperature thermistor ceramic resistor.
[0043] Example 2
[0044] A method for preparing a rare earth doped lanthanum aluminate based wide temperature range high stability negative temperature coefficient thermistor and a thermistor, the preparation method comprising the following steps:
[0045] a. According to La 0.9 G 0.1The weight percentage is calculated based on the stoichiometric ratio of AlO3, and 67.91% of lanthanum trioxide, 23.68% of aluminum trioxide, and 8.41% of gadolinium trioxide are weighed and mixed according to the weight percentage;
[0046] b. Place the powder prepared in step a into a ball mill, using agate balls as grinding media and ethanol as a dispersant. The ball mill first rotates clockwise at 300 revolutions per minute for 40 minutes, then pauses for 20 minutes, and then rotates counterclockwise for 40 minutes. This cycle is repeated for a total of 8 hours. After ball milling, place the mixed powder obtained in step b into a drying oven and dry it at 90°C. Subsequently, heat the dried powder to 200°C and maintain it at this temperature for 1 hour. After that, continue to heat to 1300°C and calcine at this temperature for 10 hours, with the heating rate set to 2°C per minute. After calcination is completed, cool the powder at the same rate of 2°C per minute. That is, La is obtained. 0.9 G 0.1 AlO3 powder.
[0047] c. Resuspend the La obtained in step b 0.9 G 0.1 The AlO3 powder is put into the ball mill again, ground for 6 hours, and then dried to obtain a rare earth doped lanthanum aluminate based wide temperature range high stability negative temperature coefficient thermistor ceramic material.
[0048] d. Use a pressure of 20 MPa to squeeze the powder into a circular sheet with a diameter of 10 mm and a thickness of 2 mm, and then keep it under an isostatic pressure of 300 MPa for 180 seconds. Finally, keep the extruded circular sheet at a temperature of 1600°C for 20 hours, and the heating and cooling speed is also maintained at 2°C per minute to obtain a high-temperature thermistor ceramic material.
[0049] Example 3
[0050] A method for preparing a rare earth doped lanthanum aluminate based wide temperature range high stability negative temperature coefficient thermistor and a thermistor, the preparation method comprising the following steps:
[0051] a. According to La 0.9 Ho 0.1 The weight percentage is calculated based on the stoichiometric ratio of AlO3, and 67.67% of lanthanum trioxide, 23.59% of aluminum trioxide, and 8.72% of holmium trioxide are weighed and mixed according to the weight percentage;
[0052] b. Place the powder prepared in step a into a ball mill, using agate balls as grinding media and ethanol as a dispersant. The ball mill first rotates clockwise at 300 revolutions per minute for 40 minutes, then pauses for 20 minutes, and then rotates counterclockwise for 40 minutes. This cycle is repeated for a total of 8 hours. After ball milling, place the mixed powder obtained in step b into a drying oven and dry it at 90°C. Subsequently, heat the dried powder to 200°C and maintain it at this temperature for 1 hour. After that, continue to heat to 1300°C and calcine at this temperature for 10 hours, with the heating rate set to 2°C per minute. After calcination is completed, cool the powder at the same rate of 2°C per minute. That is, La is obtained. 0.9 Ho 0.1 AlO3 powder.
[0053] c. Resuspend the La obtained in step b 0.9 Ho 0.1 The AlO3 powder is put into the ball mill again, ground for 6 hours, and then dried to obtain a rare earth doped lanthanum aluminate based wide temperature range high stability negative temperature coefficient thermistor ceramic material.
[0054] d. Use a pressure of 20 MPa to squeeze the powder into a circular sheet with a diameter of 10 mm and a thickness of 2 mm, and then keep it under an isostatic pressure of 300 MPa for 180 seconds. Finally, keep the extruded circular sheet at a temperature of 1600°C for 20 hours, and the heating and cooling speed is also maintained at 2°C per minute to obtain a high-temperature thermistor ceramic material.
[0055] Example 4
[0056] A method for preparing a rare earth doped lanthanum aluminate based wide temperature range high stability negative temperature coefficient thermistor and a thermistor, the preparation method comprising the following steps:
[0057] a. According to La 0.9 Tm 0.1 The weight percentage is calculated based on the stoichiometric ratio of AlO3, and 67.54% of lanthanum trioxide, 23.55% of aluminum trioxide, and 8.89% of thulium trioxide are weighed and mixed according to the weight percentage;
[0058] b. Place the powder prepared in step a into a ball mill, using agate balls as grinding media and ethanol as a dispersant. The ball mill first rotates clockwise at 300 revolutions per minute for 40 minutes, then pauses for 20 minutes, and then rotates counterclockwise for 40 minutes. This cycle is repeated for a total of 8 hours. After ball milling, place the mixed powder obtained in step b into a drying oven and dry it at 90°C. Subsequently, heat the dried powder to 200°C and maintain it at this temperature for 1 hour. After that, continue to heat to 1300°C and calcine at this temperature for 10 hours, with the heating rate set to 2°C per minute. After calcination is completed, cool the powder at the same rate of 2°C per minute. That is, La is obtained. 0.9 Tm 0.1 AlO3 powder.
[0059] c. Resuspend the La obtained in step b 0.9 Tm 0.1 The AlO3 powder is put into the ball mill again, ground for 6 hours, and then dried to obtain a rare earth doped lanthanum aluminate based wide temperature range high stability negative temperature coefficient thermistor ceramic material.
[0060] d. Use a pressure of 20 MPa to squeeze the powder into a circular sheet with a diameter of 10 mm and a thickness of 2 mm, and then keep it under an isostatic pressure of 300 MPa for 180 seconds. Finally, keep the extruded circular sheet at a temperature of 1600°C for 20 hours, and the heating and cooling speed is also maintained at 2°C per minute to obtain a high-temperature thermistor ceramic material.
[0061] Comparative Example 1
[0062] A method for preparing a lanthanum aluminate thermistor and a thermistor, the method comprising the following steps:
[0063] a. Calculate the weight percentage according to the stoichiometric ratio of LaAlO3, and weigh 76.03% of lanthanum trioxide and 23.86% of aluminum trioxide according to the weight percentage and mix them;
[0064] b. Put the powder prepared in step a into a ball mill, use agate balls as grinding media and ethanol as dispersant. The ball mill first rotates clockwise at 300 revolutions per minute for 40 minutes, then pauses for 20 minutes, and then rotates counterclockwise for 40 minutes. This cycle is repeated for a total of 8 hours. After ball milling, the mixed powder obtained in step b is placed in a drying oven and dried at 90°C. Subsequently, the dried powder is heated to 200°C and maintained at this temperature for 1 hour. After that, continue to heat to 1300°C and calcine at this temperature for 10 hours, with the heating rate set to 2°C per minute. After calcination is completed, the powder is also cooled at a rate of 2°C per minute. That is, LaAlO3 powder is obtained.
[0065] c. Put the powder obtained in step b into the ball mill again, grind for 6 hours, and then dry it. Use a pressure of 20MPa to squeeze the powder into a circular sheet with a diameter of 10 mm and a thickness of 2 mm, and then keep it under an isostatic pressure of 300MPa for 180 seconds. Finally, keep the extruded circular sheet at a temperature of 1600°C for 20 hours, and the heating and cooling speed is also maintained at 2°C per minute to obtain a high-temperature thermistor ceramic material.
[0066] In summary, the present invention relates to a rare earth doped LaAlO3 based NTC material with wide temperature range and high stability, specifically La 0.9 X 0.1 AlO3, X = (Eu, Gd, Ho, Tm) is prepared by a solid phase reaction method. The preparation process includes the following steps: first, accurately weighing the raw materials according to the weight percentage; second, mixing the raw materials, grinding, pre-sintering, secondary grinding, tableting, isostatic pressing, sintering, platinum slurry coating, annealing, and welding the leads.
[0067] Figure 1 The XRD diagram of the present invention shows that the diffraction peaks of different elements all match the LaAlO3 structure very well, indicating that all elements are well doped into LaAlO3; Figure 2 For the present invention La 0.9 X 0.1 B of AlO3 thermal sensitive ceramic materials and LaAlO3 700 / 1000k Value and 1000K relationship diagram; Figure 3 For the present invention La 0.9 X 0.1 Aging relationship diagram of AlO3 thermistor ceramic material and LaAlO3 material. Figure 1-Figure 3 It can be seen that the NTC thermistor material has a wide temperature application range (500℃-1500℃) and exhibits excellent aging stability. After 500 hours of aging test at high temperature of 1000℃, La 0.9 X 0.1 The resistance drift rate of the samples of AlO3, X = (Eu, Gd, Ho, Tm) is less than 8%, and the electrical performance parameters of the NTC ceramics are as follows: 700 / 1000k =213.39K~13564.1K,ρ 1000k =12.9×10 3 Ω·cm~13.3×10 5 Ω·cm, showing its long service life. In addition, the powder particles provided by the invention have good dispersibility, are not easy to agglomerate, and have high material strength.
[0068] The process parameters (such as temperature, time, etc.) of the present invention can realize the method by taking upper and lower limits and interval values, and the embodiments are not listed one by one here.
[0069] Any contents not described in detail in the present invention can be based on the conventional technical knowledge in the art.
[0070] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the embodiments, it should be understood by those skilled in the art that any modification or equivalent replacement of the technical solutions of the present invention does not depart from the spirit and scope of the technical solutions of the present invention and should be included in the scope of the claims of the present invention.
Claims
1. A rare earth doped LaAlO3 based wide temperature range high stability negative temperature coefficient thermistor ceramic material, characterized in that: The thermal sensitive ceramic material is made of lanthanum trioxide, aluminum trioxide, europium trioxide, gadolinium trioxide, holmium trioxide or thulium trioxide by solid phase reaction according to weight percentage, and its chemical composition is La 0.9 X 0.1 AlO3, wherein X = Eu, Gd, Ho or Tm.
2. The rare earth doped LaAlO3 based wide temperature range high stability negative temperature coefficient thermistor ceramic material according to claim 1, characterized in that: The electrical performance parameters of the thermosensitive ceramic material are as follows: 700 / 1000k =213.39K~13564.1K,ρ 1000k =12.9×10 3 Ω·cm~13.3×10 5 Ω·cm, the applicable temperature range is 500℃~1500℃; after aging at high temperature of 1000℃ for 500 hours, the resistance drift rate ΔR / R0(%) is less than 8%.
3. A method for preparing a rare earth doped LaAlO3-based wide temperature range high stability negative temperature coefficient thermistor ceramic material, comprising the following steps: a. Weigh the raw materials of lanthanum trioxide, aluminum trioxide and one of europium trioxide, gadolinium trioxide, holmium trioxide and thulium trioxide, respectively, mix them, ball-mill and dry them to obtain powders; b. Heat the powder to 150-250℃, keep it at 150-250℃ for 0.5-1.5h, then heat it to 1200-1400℃, calcine it at 1200-1400℃ for 8-11h, with a heating rate of 1-3℃ / min; then cool it at a cooling rate of 1-3℃ / min to obtain La 0.9 X 0.1 AlO3 powder, X=Eu, Gd, Ho or Tm; c.La 0.9 X 0.1 The AlO3 powder is subjected to secondary ball milling and drying to obtain rare earth doped LaAlO3 based wide temperature range high stability negative temperature coefficient thermistor ceramic material powder.
4. The preparation method according to claim 3, characterized in that: In step a and step c, the grinding medium used in ball milling is agate balls, and the ball milling medium is ethanol.
5. The preparation method according to claim 3, characterized in that: In step a, the ball mill rotates clockwise at 300 rpm for 40 minutes, stops for 20 minutes, and then rotates counterclockwise at 300 rpm for 40 minutes, and repeats this process for 8 hours.
6. The preparation method according to claim 3, characterized in that: In step a and step c, the drying temperature is 90°C.
7. The preparation method according to claim 3, characterized in that: In step c, the ball milling time is 5-7 hours.
8. A method for preparing a thermistor using the rare earth doped LaAlO3-based wide temperature range high stability negative temperature coefficient thermistor ceramic material according to claim 1 or 2, the method comprising the following steps: The powder of rare earth doped LaAlO3 based wide temperature range high stability negative temperature coefficient thermistor ceramic material is pressed into a circular sheet and cold isostatically pressed for 170-190s; then the sheet is kept at 1550-1650°C for 18-22h to obtain a circular sheet-shaped wide temperature range high stability thermistor ceramic material; finally, platinum slurry electrodes are coated on both sides of the circular sheet-shaped wide temperature range high stability thermistor ceramic material, annealed and cooled to room temperature to obtain a wide temperature range high stability negative temperature coefficient thermistor.
9. The method according to claim 8, characterized in that The cold isostatic pressing pressure is 250-350 MPa.
Citation Information
Patent Citations
Preparation method of Ce-doped LaAlO3 flickering ceramic material
CN102701723A
Thermal sensitive ceramic material with negative temperature coefficient in medium-high temperature region and preparation method of thermal sensitive ceramic material
CN117923898A
Wide-temperature-range negative-temperature-coefficient thermal sensitive ceramic material and preparation method thereof
CN118239777A
METHOD FOR PRODUCING LaAlO3 CERAMIC
JP2012218973A