Ceramic tile with multi-layer three-dimensional effect and preparation process of ceramic tile

By combining screen printing and digital inkjet processes on ceramic tiles, a multi-layer concave and convex texture is formed, which solves the problem of lack of three-dimensionality in ceramic tiles design, and achieves the three-dimensionality enhancement and production efficiency improvement of ceramic tiles.

CN118955181AActive Publication Date: 2024-11-15GUANGXI JIANYI CERAMICS CO LTD +2

Patent Information

Application Number
CN202411022119.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The existing ceramic tiles lack three-dimensional sense in the design patterns, and the concave and convex texture is single, which cannot fully reproduce the visual and tactile three-dimensional effect of the stone. In addition, the mold replacement takes a long time, low production capacity and high cost during the production process.

Method used

Using a combination of screen printing and digital inkjet, a convex glaze layer, a replica ink layer, a replica glaze layer and a pattern layer are applied in turn, and a bright ink and a positioned dry particle layer is combined to form a multi-layer concave and convex texture. Specific glaze formulas and dry grains are rich and varied, enhancing the three-dimensionality and decorative effect of ceramic tiles.

Benefits of technology

The multi-layer three-dimensional effect on the surface of ceramic tile is achieved, the height difference between the groove texture and the raised texture is obvious, the touch is thick and lubricated, and the decorative effect is rich and varied, which avoids the difficulty of mold replacement and high cost problems, and improves production efficiency and Product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955181A_ABST
    Figure CN118955181A_ABST
Patent Text Reader

Abstract

The invention discloses a ceramic tile with a multi-layer three-dimensional effect. The ceramic tile comprises a ceramic tile blank body, a ground glaze layer, a convex glaze layer, a re-engraved ink layer, a re-engraved surface glaze layer, a pattern layer, a bright ink layer, a positioning dry particle layer and a protective glaze layer which are sequentially stacked, the distribution paths of the convex glaze layer, the re-carved ink layer and the positioning dry particle layer are matched with a design pattern; the convex glaze layer is printed on the ground glaze layer through a silk screen, and the mesh number of a screen printing plate is 30-80. According to the scheme, the convex glaze layer is firstly printed in front of the pattern layer in a silk-screen printing mode, the plane layer with the convex patches or strip-shaped textures is well formed on the surface of the green brick, and then the color patterns are borne, so that the color pattern layer has a three-dimensional effect, and the textures are clearer; and a digital ink-jet printer is used for printing re-engraved ink and re-engraved cover glaze to form groove textures, so that a three-layer concave-convex texture three-dimensional effect is formed on the surface of the green brick, and positioning dry particle layers with different functions are formed in cooperation with double positioning dry particles, so that the decoration effect is further enriched.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building ceramics, and in particular to a multi-layered three-dimensional effect ceramic tile and a preparation process thereof. Background Art

[0002] The development of ceramic decoration technology is oriented towards diversification and continuous innovation. Through equipment improvement, special materials and process combination, the decorative effects of ceramic tiles produced are endless. In order to enhance the three-dimensional effect of ceramic tiles, it can be achieved through a variety of ways:

[0003] 1. Carving concave and convex steel molds. The concave and convex textured bricks are pressed out by steel molds to achieve a three-dimensional effect. However, the production cycle of steel molds is long. During the pressing process, demoulding is difficult. The edges and corners of the concave and convex mold bricks are easily worn and collided when sweeping and cleaning. During production, the molds are bulky and it takes a long time to replace the molds. Changing the molds on the production line will cause empty kilns, reduce production capacity, affect product quality, and have high costs.

[0004] 2. Use sinking ink. This method uses special functional ink and a digital inkjet machine to spray the sinking ink with etching effect on the surface of the brick. On this basis, a layer of transparent glaze is applied. Due to the corrosive effect of the sinking ink, during the firing process, the sinking ink position will chemically react with the transparent glaze and corrode the transparent glaze layer, thereby forming a pit effect. However, at the same time, due to the residual vanadium pentoxide in the sinking ink, the color of the pit position will turn green, affecting the aesthetic effect.

[0005] 3. Printing raised effect glaze. After printing the color pattern, use a silk screen, roller printing machine or digital inkjet machine to print the raised effect glaze at a specific pattern position. Since this process covers the color pattern, the raised effect glaze has poor transparency and the pattern is not clear enough. In addition, the printing aperture of the silk screen, roller and digital inkjet machine is small, the thickness of the printed raised effect glaze layer is thin, the bulge is not obvious, the decorative effect of the raised glaze layer is monotonous, and the color patterns are all printed on the same spatial plane, lacking a three-dimensional sense.

[0006] The three-dimensional sense of stone is not only reflected in the three-dimensional sense of touch, but also in the three-dimensional visual effect and the three-dimensional variability of color space. At present, the design patterns in the ceramic industry mostly remain on the same horizontal plane design display. Only a few companies have superimposed the tactile concave and convex three-dimensional effect on the basis of the horizontal plane design pattern, and there is no multi-dimensional three-dimensional change in the color of the pattern space, which makes the surface of the ceramic tile stiff, and there is a big gap with the surface effect of natural marble, lacking the spirituality of stone. In order to make the surface of the ceramic tile more three-dimensional, more realistic stone in terms of vision, light perception, touch, and texture level, and able to be used for a long time, the present invention provides a ceramic tile with multi-level three-dimensional effect and its preparation process. Summary of the invention

[0007] The main purpose of the present invention is to provide a multi-layered three-dimensional effect ceramic tile, the design pattern layer is three-dimensional, the glaze surface has a concave and convex texture, and the texture height difference is obvious, the touch is thick and smooth, the three-dimensional effect is strong, and the decorative effect is rich and varied.

[0008] To achieve the above-mentioned purpose, the present invention proposes a multi-layered three-dimensional effect ceramic tile, comprising a ceramic tile body, a base glaze layer, a convex glaze layer, a replica ink layer, a replica surface glaze layer, a pattern layer and a protective glaze layer stacked in sequence; the distribution paths of the convex glaze layer and the replica ink layer match the design pattern; the convex glaze layer is screen-printed onto the base glaze layer, and the screen mesh number is 30 to 80 meshes.

[0009] The present invention adopts the screen printing method to print the convex glaze layer before the pattern layer, so as to form a plane layer of raised patches or strip textures on the surface of the brick, and then carry the color pattern, so that the color pattern layer has a three-dimensional effect and the texture is clearer; on the other hand, the digital inkjet machine is used to print the replica ink to form a groove texture with the replica glaze, so that the three-level concave-convex texture three-dimensional effect is formed on the surface of the brick without using a concave-convex steel mold.

[0010] Preferably, the raw materials for preparing the convex glaze layer include convex effect glaze, printing paste and printing oil; the raw material components of the convex effect glaze include, by weight: 15-25 parts of potassium feldspar, 8-16 parts of nepheline, 8-16 parts of kaolin, 8-14 parts of coal gangue, 4-12 parts of aluminum oxide, 8-14 parts of fused quartz, 6-18 parts of spinel, 2-6 parts of zinc oxide and 4-16 parts of zirconium silicate.

[0011] The raised effect glaze with the above components has a higher initial melting point and high temperature viscosity. It is not easy to melt and soften prematurely during the firing process, resulting in the collapse of the edge of the raised effect glaze. The printed raised effect glaze can maintain its original shape without deformation, and the raised performance is firm and the three-dimensional effect is strong.

[0012] Preferably, a glossy ink layer and a positioning dry particle layer are sequentially arranged between the pattern layer and the protective glaze layer, and the distribution paths of the glossy ink layer and the positioning dry particle layer match the design pattern.

[0013] According to the design requirements, the different gray values ​​of the glossy ink are adjusted and printed at the corresponding color pattern positions to control the grayscale changes of the different glossy inks. After firing, the glaze layer surface is integrated with a gradual gloss change effect. Double or multiple positioning dry particles are applied to the pattern layer according to the pattern design to form positioning dry particle layers with different functions on the pattern layer to further enrich the decorative effect.

[0014] Preferably, the raw materials for preparing the positioned dry particle layer include one or more of skin dry particles and functional dry particles, and the functional dry particles include one or more of colored dry particles, ice crystal dry particles, metal dry particles, bright dry particles, cracked dry particles and polycrystalline dry particles.

[0015] To position the dry particle layer, transparent skin dry particles can be used alone to create a transparent raised effect, or they can be used in combination with a variety of functional dry particles to create a transparent raised effect with suspended colored dry particles or suspended ice crystal dry particles, etc., which has rich and varied layers and a strong three-dimensional decorative effect.

[0016] Preferably, the raw material components of the skin dry particles include, by weight: 12 to 22 parts of lithium feldspar, 10 to 18 parts of albite, 3 to 9 parts of kaolin, 6 to 16 parts of dolomite, 8 to 20 parts of strontium carbonate, 8 to 16 parts of magnesium nitride, 4 to 10 parts of diamond, 6 to 14 parts of zinc oxide and 6 to 12 parts of fluorite.

[0017] The raw material components of the above-mentioned skin dry particles are mixed evenly in proportion and then put into a frit furnace for calcination. The calcination curve is that the temperature is raised to 700℃ for 30-45min, 700-1100℃ for 50-60min, 1100-1450℃ for 60-90min, and 1450℃ for 20-30min; the frit slurry is obtained, and the frit slurry is directly put into clean water for water quenching and cooling to obtain a matte transparent frit, the frit is crushed and dried, and passed through a double-layer vibration sieve of 100 mesh and 200 mesh. The middle part, i.e., 100-200 mesh particles, is taken to obtain the above-mentioned skin dry particles. The raw material components and preparation method of the colored dry particles are basically the same as those of the skin dry particles. The difference is that the colored dry particles are dry-mixed with inorganic pigments of different colors on the basis of the raw material components of the skin dry particles. After being mixed evenly, the same firing system is used for high-temperature calcination, and then the colored dry particles are water-quenched, cooled, crushed, and passed through a double-layer vibration sieve to obtain colored dry particles. By adjusting the amount of magnesium nitride in the skin dry particles, the dry particles can feel smoother after firing; by adjusting the proportion of zinc oxide, the transparency and color of the dry particles after firing can be enhanced, making the positioned dry particle layer more transparent and the pattern texture more vivid.

[0018] Preferably, the raw materials for preparing the base glaze layer include, by weight: 16-24 parts of potassium feldspar, 10-20 parts of sodium feldspar, 5-15 parts of kaolin, 14-22 parts of quartz, 4-8 parts of aluminum oxide, 6-10 parts of calcined clay, 4-10 parts of burned talc and 12-20 parts of zirconium silicate. The raw materials for the base glaze layer are put into a ball mill for grinding in proportion until the fineness is controlled to be 0.3-0.6% on a 325-mesh sieve, and the slurry is discharged through a 200-mesh vibrating sieve. The base glaze material used in this scheme adjusts the amount of zirconium silicate added to make the fired base glaze have better whiteness, cover the surface of the green body, enhance the overall whiteness of the ceramic tile glaze, and facilitate the color development of the subsequent pattern layer.

[0019] Preferably, the raw materials for preparing the replica glaze layer include, by weight: 18 to 26 parts of potassium feldspar, 10 to 20 parts of sodium feldspar, 5 to 15 parts of air knife clay, 10 to 18 parts of fused quartz, 3 to 7 parts of aluminum oxide, 4 to 10 parts of calcined clay, 4 to 8 parts of talc, 3 to 7 parts of zinc oxide and 12 to 20 parts of zirconium silicate.

[0020] The use of fused quartz to replace conventional quartz raw materials in the replica glaze formula can solve the problem of glaze pores absorbing dirt. At the same time, during the firing process, the fused quartz produces a high viscosity of the glass phase, which reduces the fluidity of the glaze, thereby making the three-dimensional effect of the replica groove better. Zinc oxide is added to the formula to further enhance the color and brightness of the ceramic tile glaze pattern layer.

[0021] In addition, the present invention also provides a preparation process of the above-mentioned multi-layered three-dimensional effect ceramic tile, comprising the following steps:

[0022] S1, pressing the ceramic powder into a shape, and after drying, forming a ceramic tile body;

[0023] S2, applying a base glaze on the ceramic tile body to form a base glaze layer;

[0024] S3, printing convex glaze on the base glaze layer using a screen printing machine according to the design pattern to form a convex glaze layer;

[0025] S4, according to the design pattern, performing inkjet printing on the base glaze layer to apply replica ink to form a replica ink layer;

[0026] S5, applying a replica glaze on the surface of the ceramic tile body composited with the convex glaze layer and the replica ink layer to form a replica glaze layer;

[0027] S6, printing color ink on the replica glaze layer according to the design pattern texture to form a pattern layer;

[0028] S7, applying a protective glaze on the surface of the body on which the pattern layer is formed, to form a protective glaze layer;

[0029] S8, after drying, firing in a kiln to obtain the multi-layered three-dimensional effect ceramic tile.

[0030] Preferably, after step S6, the following steps are further included:

[0031] S7-1, printing glossy ink on the pattern layer according to the design pattern to form a glossy ink layer;

[0032] S7-2, applying positioning glue and dry particles on the surface of the blank forming the glossy ink layer according to the design pattern to form a positioning dry particle layer;

[0033] S7-3, applying a protective glaze on the surface of the green body after the above treatment to form a protective glaze layer;

[0034] S8, after drying, firing in a kiln to obtain the multi-layered three-dimensional effect ceramic tile.

[0035] Preferably, in the above preparation process, the drying temperature in step S1 is 150-230° C., and the drying cycle is 60-80 min.

[0036] Preferably, in the above preparation process, in step S2, the specific gravity of the base glaze is 1.82-1.88 g / mL, the flow rate is 16-25 s, and the glaze amount is 400-600 g / m 2 .

[0037] Preferably, in the above preparation process, the mesh number of the screen in step S3 is 30 meshes, and the photosensitive glue is thickened on the screen cloth 3 to 4 times. The hardened photosensitive glue three-dimensionally supports the height of the screen, and the thickness of the printed convex glaze layer can be significantly improved.

[0038] Preferably, in the above preparation process, the grayscale of the replica ink in step S4 is 60-90%, and the width of the replica ink design pattern is 1-10 mm.

[0039] Preferably, in the above preparation process, the specific gravity of the replica glaze in step S5 is 1.45-1.50 g / mL, the flow rate is 11-15 s, and the glaze amount is 240-450 g / m 2 .

[0040] Preferably, in the above preparation process, the grayscale value of the bright ink in step S7-1 is 20-80%.

[0041] Preferably, in the above preparation process, the positioning dry particle layer is applied by digital printing using a dry particle digital printer.

[0042] Preferably, in the above preparation process, the specific gravity of the protective glaze is 1.35-1.45 g / mL, the flow rate is 11-16 s, and the glaze amount is 250-400 g / m 2 .

[0043] Preferably, in the above preparation process, the drying and firing steps in step S8 specifically include: drying at 100-180°C for 10-20min, first drying at a low temperature to reduce the moisture content of the bricks, to prevent the bricks from rapidly heating up during firing in the high temperature environment of the firing kiln, and to prevent the bricks from bursting due to untimely evaporation of moisture; at the same time, it can also make the glue, protective glaze and dry particles more firmly bonded, and the dry particles will not fall off in subsequent processes, and then fired in a roller kiln at 1200-1250°C, with a firing cycle of 70-90min, and keeping warm in the high temperature zone for 10-15min.

[0044] Compared with the existing technology in the industry, the present invention first applies a raised effect glaze on the base glaze by screen printing to form a raised glaze layer, and then inkjet prints the pattern layer to make the pattern form a three-dimensional effect, and then cooperates with the groove texture formed by the replica ink and the replica surface glaze, and the groove depth is 0.2-0.6mm; at the same time, by adjusting the formula of the raised effect glaze, the raised texture effect is more three-dimensional, the shape remains unchanged before and after firing, the performance is more solid, the three-dimensional sense is strong, and the raised height can reach 0.4-1.2mm; combined with the dry particle digital printer DDG digital application double positioning dry particles, composite transparent dry particles and functional dry particles, multiple raised effects of different heights and shapes are formed above the pattern layer, which feel smooth and heavy, and the raised height can reach 0.8-2.0mm, further enhancing the three-dimensional effect of the tile surface. The ceramic tile glaze has three levels of concave and convex texture three-dimensional effect, so that the height difference between the ceramic tile groove texture and the raised texture can reach 1.0-2.5mm, and the three-dimensional effect is clearly visible. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying any creative work.

[0046] Figure 1 It is a schematic diagram of the cross-sectional hierarchical structure of Example 4 of the present invention;

[0047] Figure 2 , Figure 3 They are respectively physical pictures of embodiments 3 and 4 of the present invention.

[0048] Attached Figure 1 Middle: 1-ceramic tile body; 2-bottom glaze layer; 3-convex glaze layer; 4-replica ink layer; 5-replica surface glaze layer; 6-pattern layer; 7-gloss ink layer; 8-positioning dry particle layer; 9-protective glaze layer.

[0049] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0050] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement.

[0051] A preparation process of a multi-layer three-dimensional effect ceramic tile comprises the following steps:

[0052] S1. Press the ceramic powder into a shape and send it into a drying kiln for drying to form a ceramic tile body; preferably, the drying temperature is 150-230° C. and the drying cycle is 60-80 min.

[0053] S2. Applying a base glaze on the ceramic tile body to form a base glaze layer; preferably, the base glaze has a specific gravity of 1.82-1.88 g / mL, a flow rate of 16-25 s, and a glaze application amount of 400-600 g / m 2 .

[0054] S3, printing convex glaze on the base glaze layer by a screen printing machine according to the design pattern to form a convex glaze layer;

[0055] S4, according to the design pattern, inkjet printing is performed on the base glaze layer to apply replica ink to form a replica ink layer;

[0056] S5, applying a replica glaze on the surface of the ceramic tile body composited with the convex glaze layer and the replica ink layer to form a replica glaze layer; preferably, the replica glaze has a specific gravity of 1.45-1.50 g / mL, a flow rate of 11-15 s, and a glaze amount of 240-450 g / m 2 .

[0057] S6. Printing color ink on the replica glaze layer according to the design pattern using a digital inkjet machine to form a pattern layer;

[0058] S7-1, printing glossy ink on the pattern layer according to the design pattern to form a glossy ink layer;

[0059] S7-2, according to the design pattern, applying positioning glue and dry particles on the surface of the blank body where the glossy ink layer is formed, to form a positioning dry particle layer;

[0060] S7-3, applying protective glaze on the surface of the green body after the above treatment to form a protective glaze layer; preferably, the specific gravity of the protective glaze is 1.35-1.45 g / mL, the flow rate is 11-16 s, and the glaze amount is 250-400 g / m 2 .

[0061] S8, after drying, firing in a kiln to obtain the multi-layered three-dimensional effect ceramic tile; the drying and firing steps specifically include: drying at 100-180°C for 10-20 minutes, firing in a roller kiln at 1200-1250°C, the firing cycle is 70-90 minutes, and keeping warm in the high temperature zone for 10-15 minutes.

[0062] The multi-layered three-dimensional effect ceramic tiles are softly polished and edge-grinded using a polishing machine. The low light module, rubber brush module and sponge polishing module are arranged and combined to achieve a soft light effect through polishing, and the product is packaged to complete production.

[0063] Preferably, the raw materials for preparing the bottom glaze layer include, by weight: 16-24 parts of potassium feldspar, 10-20 parts of sodium feldspar, 5-15 parts of kaolin, 14-22 parts of quartz, 4-8 parts of aluminum oxide, 6-10 parts of calcined clay, 4-10 parts of calcined talc and 12-20 parts of zirconium silicate; each raw material is put into a ball mill for grinding according to proportion, until the fineness is controlled to be 0.3-0.6% of the residue on a 325-mesh sieve, and the slurry is discharged through a 200-mesh vibrating sieve. The zirconium silicate in the formula has a good opacifying effect during the firing process, covers the surface of the green body, can enhance the whiteness of the ceramic tile glaze, and makes the subsequent pattern layer better in color.

[0064] Preferably, the raw materials for preparing the convex glaze layer, measured by weight, include 100 parts of raised effect glaze, 60 parts of printing paste and 25 parts of printing oil, which are fed into a ball mill in proportion, ball-milled evenly, and discharged after the fineness is qualified, and passed through a 200-mesh vibrating screen; Preferably, the raw material components of the raised effect glaze, measured by weight, include: 15-25 parts of potassium feldspar, 8-16 parts of nepheline, 8-16 parts of kaolin, 8-14 parts of coal gangue, 4-12 parts of aluminum oxide, 8-14 parts of fused quartz, 6-18 parts of spinel, 2-6 parts of zinc oxide and 4-16 parts of zirconium silicate; Preferably, the mesh number of the silk screen is 30-80 mesh, and the photosensitive glue is thickened on the mesh 3-4 times.

[0065] Preferably, the grayscale of the replica ink is 60-90%, and the width of the replica ink design is 1-10 mm. As the grayscale of the replica ink increases and the design line pattern becomes wider, the replica groove effect becomes more obvious.

[0066] Preferably, the raw materials for preparing the replica glaze layer include, by weight: 18 to 26 parts of potassium feldspar, 10 to 20 parts of sodium feldspar, 5 to 15 parts of air knife clay, 10 to 18 parts of fused quartz, 3 to 7 parts of aluminum oxide, 4 to 10 parts of calcined clay, 4 to 8 parts of talc, 3 to 7 parts of zinc oxide and 12 to 20 parts of zirconium silicate.

[0067] Through a digital inkjet machine, the replica glaze functional ink is printed on the surface of the brick blank, and on this basis, a layer of replica glaze is sprayed with a reciprocating glaze spray cabinet. With the help of the replica ink and the glaze etching effect during the firing process, and the repulsion of the oily ink and the water-based glaze, a pit texture peeling effect is formed on the surface of the ceramic tile. Due to the thin glaze layer, the depth of the pit peeled off the glaze layer is limited, and when the area of ​​the connected part of the functional ink pattern is large or the strip design pattern is wide, glaze beads often appear in the groove, forming similar glaze accumulation defects, affecting the appearance. Therefore, it is necessary to adjust the replica glaze formula, use fused quartz to replace conventional quartz raw materials, and during the firing process, the glass phase viscosity is large, which reduces the fluidity of the glaze. At the same time, the width of the replica ink design drawing is controlled to be 1-10mm to avoid the replica groove being not obvious due to the small width, and the glaze beads being easy to be generated due to the large width. The replica glaze formula adopted in this scheme can also solve the problem of glaze pores absorbing dirt, and improve the color and brightness of the glaze pattern as a whole.

[0068] Preferably, the grayscale value of the glossy ink is 20-80%. The higher the grayscale value, the brighter the position where the glossy ink is printed will be after firing.

[0069] Preferably, the raw materials for preparing the positioned dry particle layer include one or more of skin dry particles and functional dry particles, and the functional dry particles include one or more of colored dry particles, ice crystal dry particles, metal dry particles, bright dry particles, cracked dry particles and polycrystalline dry particles.

[0070] Preferably, the raw material components of the skin dry particles include, by weight: 12 to 22 parts of lithium feldspar, 10 to 18 parts of albite, 3 to 9 parts of kaolin, 6 to 16 parts of dolomite, 8 to 20 parts of strontium carbonate, 8 to 16 parts of magnesium nitride, 4 to 10 parts of diamond, 6 to 14 parts of zinc oxide and 6 to 12 parts of fluorite. The raw material components of the above-mentioned skin dry particles are mixed evenly in proportion and then placed in a frit furnace for calcination. The calcination curve is that the temperature rises to 700℃ for 30-45min, 700-1100℃ for 50-60min, 1100-1450℃ for 60-90min, and 1450℃ for 20-30min; the frit slurry is obtained, and the frit slurry is directly placed in clean water for water quenching to obtain a matte transparent frit, the frit is crushed and dried, and passed through a double-layer vibration sieve of 100 mesh and 200 mesh. The middle part, i.e., 100-200 mesh particles, is taken to obtain the above-mentioned skin dry particles. In this scheme, the positioning dry particle layer is applied by Sacmi dry particle digital printer DDG digital printing. The first and third channels are glue functional inks. The gray value of the glue design pattern is 55-100%, which plays a bonding role between the brick and the dry particles; the second and fourth channels are used to apply different types of dry particles respectively for the positioning dry particles. Among them, the dry particles in the second and fourth channels are applied to the surface of the brick in synchronization with the glue in the first and third channels according to the same design drawing. The dry particles in the second and fourth channels do not overlap and are not inlaid with each other. If necessary, the second and fourth channels can also selectively locate the dry particles in the same position to overlap and superimpose multiple three-dimensional effects. The gray value of the design drawing for locating the thickness of the dry particle layer is 40-100%. The larger the gray value of the glue and dry particle design drawing, the more obvious the convex effect of the applied and located dry particle layer, and the better the sense of thickness to touch.

[0071] It should be noted that in conventional processes, in order to achieve a three-dimensional effect on the surface of the tile, a glaze with a raised effect is usually applied to the pattern layer. However, in order not to affect the color and texture of the pattern, the raised effect glaze layer cannot be too thick, but too thin will result in an unclear raised effect. In this scheme, a raised effect glaze is directly applied on the base glaze layer, and then the pattern layer is printed. This can not only make the pattern more three-dimensional, but also solve the problem that the color of the pattern is poorly transparent under the raised effect glaze layer and the pattern is unclear. The formula of the raised effect glaze can also reduce restrictions, and there is no need to consider the transparency of the raised effect glaze. Some commonly used processes such as roller printing or digital inkjet printing have small printing apertures for raised effect glazes, low glaze viscosity, and easy flow and diffusion. The raised glaze layer formed is thin, and the raised effect is not obvious. The dry spreading process using positioning glue ink plus dry powder glaze requires the recovery of excess dry powder glaze after applying the dry powder glaze, and the process flow is complicated. In this solution, the raised effect glaze is applied by screen printing, and the raised effect glaze is printed only in the required position. Not only is the process simple, but a raised glaze layer with stronger three-dimensional effect and more stable performance can be obtained. In particular, by reducing the mesh count of the screen and increasing the number of thickening times of the photosensitive resin, the thickness of the raised effect glaze layer can be significantly increased, and a raised glaze layer with a more three-dimensional effect can be obtained.

[0072] In this scheme, by regulating the compounding of kaolin, coal gangue, fused quartz and spinel components in the raised effect glaze formula, the plasticity is improved, the glaze temperature, initial melting point and high-temperature viscosity are increased, the glaze is prevented from melting and softening prematurely during the firing process, and the collapse of the raised edges is reduced, so that the glaze can maintain its original shape without deformation, the performance is stable, and the three-dimensional effect is strong after firing.

[0073] In this solution, a three-level concave-convex texture effect is designed directly through the distribution of glazes through composite screen-printed convex glaze layer, replica ink layer and replica surface glaze layer, eliminating the use of digital steel molds, avoiding the difficulty of mold changing, reducing the empty kiln rate, and improving production and quality.

[0074] It should be noted that this solution adopts a four-channel digital printing system of a dry particle digital printer. The glue and dry particles are arranged at intervals, and the glue can be positioned and printed separately. Two dry particles with different effects are applied. Compared with the dry material distribution system, the distance between the glue and the dry particle equipment is small, which shortens the penetration time of the glue and the brick. Therefore, the amount of glue can be reduced, and the application of dry particles generates less dust and has precise positioning. Different textures can correspond to the application of dry particles of different colors or functions. There is no cross-contamination between the two dry particles. At the same time, it solves the impurity defects caused by the recycling of dry particles in the dry material distribution system and simplifies the process flow.

[0075] In this solution, a four-channel dry particle digital printer is used as an example. It is not limited to four channels, and six channels, eight channels, etc. can also be used to produce more combined suspended functional particles with rich and varied raised effects. The two positioning dry particles printed by the four-channel DDG can be transparent skin dry particles as a carrier and one or more of a variety of color dry particles such as yellow dry particles, black dry particles, dark blue dry particles, coffee dry particles or white dry particles, etc., mixed evenly and accurately printed at the positioning glue position, or two different effect dry particles. The second and fourth channels of the dry particle digital printer DDG respectively mix one or more of the functional dry particles such as color dry particles, ice crystal dry particles, metal dry particles, bright dry particles, cracked dry particles or polycrystalline dry particles with skin dry particles, and print them accurately at the glue position, with less dry particle loss and mutual interaction. There is no cross-influence, which solves the problem of the previous dry-method spreading system having only a single effect of positioning transparent dry particles, and enriches the diversity of decorative effects of raised positioning dry particles. Through the DDG four-channel twice application of positioning glue dry particles, you can see two or more decorative effects such as colored particles with suspension properties, ice crystal effects, metal effects, crack effects or polycrystalline effects suspended in the surface layer, middle layer and lower layer of transparent skin dry particles, with rich and varied layers, strong three-dimensional sense, smooth and heavy touch, which can improve the different convex and concave touch and visual convex effects on the surface of ceramic tiles.

[0076] The dry particle formula adopted in this scheme is compounded with magnesium nitride and zinc oxide, so that the touch is smoother after firing, the transparency and color are better, the raised positioning dry particle layer is more transparent, and the pattern texture is bright.

[0077] The present invention is further described below by enumerating examples. It should be understood that the following examples are only used to illustrate the present invention, but not to limit the present invention. In the absence of special instructions, the parts are all parts by weight.

[0078] The present invention can use any conventional ceramic tile powder on the market to make ceramic tile blanks. A group of blanks are provided here for the preparation of ceramic tile blanks in the following embodiments. The chemical composition of the blank powder includes, by mass percentage: SiO2 65.83%, Al2O3 20.74%, Fe2O3 0.52%, TiO2 0.13%, CaO 0.48%, MgO 0.95%, K2O3.86%, Na2O 2.68% and loss on ignition 4.81%.

[0079] Embodiment 1-2

[0080] A preparation process of a multi-layer three-dimensional effect ceramic tile comprises the following steps:

[0081] S1. Press the ceramic powder into a 900×1800mm green body using a Henglitai YP8890 hydraulic press 6800T, and send it into a kiln for drying to form a ceramic tile green body; the drying temperature is 180°C and the drying cycle is 75 minutes.

[0082] S2. Apply base glaze on the ceramic tile body to form a base glaze layer; the base glaze specific gravity is 1.86g / mL, the flow rate is 19s, and the glaze amount is 500g / m 2 The raw material formula of the base glaze is shown in Table 1.

[0083] S3. According to the design pattern, a screen printing machine is used to print convex glaze on the base glaze layer to form a convex glaze layer; the raw materials for preparing the convex glaze layer include 100 parts of convex effect glaze, 60 parts of printing paste and 25 parts of printing oil by weight; the screen mesh is 60 mesh, and the photosensitive glue is thickened 3 times. The raw material formula of the convex effect glaze is shown in Table 2.

[0084] S4. According to the design pattern, inkjet printing is performed on the base glaze layer to apply replica ink to form a replica ink layer; the replica ink grayscale is 60%, and the replica ink width is 3 mm;

[0085] S5. Apply a replica glaze on the surface of the ceramic tile body composited with the convex glaze layer and the replica ink layer to form a replica glaze layer; the replica glaze has a specific gravity of 1.45 g / mL, a flow rate of 11 s, and a glaze amount of 300 g / m 2 The raw material formula of the replica glaze is shown in Table 3.

[0086] S6. Printing color ink on the replica glaze layer according to the design pattern to form a pattern layer; using a digital inkjet machine for inkjet printing.

[0087] S7. Apply protective glaze on the surface of the body with the pattern layer to form a protective glaze layer; use a Xinjingtai reciprocating glaze spray cabinet to spray the protective glaze. The protective glaze in this embodiment is made of a variety of chemical raw materials from Lianxing Company, including 50 parts of suspending agent, 30 parts of H188015 dry particles, 10 parts of GY381025 dry particles, and 10 parts of B09 transparent glaze slurry by weight. The specific gravity of the protective glaze is 1.37g / mL, the flow rate is 13s, and the glaze amount is 320g / m 2 .

[0088] S8. After drying at 120°C for 15 minutes, the product is sent to a kiln and fired in a roller kiln at 1220°C with a firing cycle of 80 minutes. The product is kept warm in a high temperature zone for 12 minutes to obtain the multi-layered three-dimensional effect ceramic tile.

[0089] Embodiment 3-4

[0090] A preparation process of a multi-layer three-dimensional effect ceramic tile comprises the following steps:

[0091] S1. Press the ceramic powder into a 900×1800mm green body using a Henglitai YP8890 hydraulic press 6800T, and send it into a drying kiln for drying to form a ceramic tile green body; the drying temperature is 180°C and the drying cycle is 75 minutes.

[0092] S2. Apply base glaze on the ceramic tile body to form a base glaze layer; the base glaze specific gravity is 1.86g / mL, the flow rate is 19s, and the glaze amount is 500g / m 2 The raw material formula of the base glaze is shown in Table 1.

[0093] S3. According to the design pattern, a screen printing machine is used to print convex glaze on the base glaze layer to form a convex glaze layer; the raw materials for preparing the convex glaze layer include 100 parts of convex effect glaze, 60 parts of printing paste and 25 parts of printing oil by weight; the screen mesh is 30 meshes, and the photosensitive glue is thickened 4 times. The raw material formula of the convex effect glaze is shown in Table 2.

[0094] S4. According to the design pattern, inkjet printing is performed on the base glaze layer to apply replica ink to form a replica ink layer; the replica ink grayscale is 90%, and the replica ink width is 8 mm;

[0095] S5. Apply a replica glaze on the surface of the ceramic tile body composited with the convex glaze layer and the replica ink layer to form a replica glaze layer; the replica glaze has a specific gravity of 1.48 g / mL, a flow rate of 12 s, and a glaze amount of 400 g / m 2The raw material formula of the replica glaze is shown in Table 3.

[0096] S6. Printing color ink on the replica glaze layer according to the design pattern to form a pattern layer; using a digital inkjet machine for inkjet printing.

[0097] S7-1. Print glossy ink on the pattern layer according to the design pattern to form a glossy ink layer. In this embodiment, glossy ink model CIK-GL121 of Idaga Company is used, and the gray value of the glossy ink is 45%;

[0098] S7-2. According to the design pattern, the positioning glue and dry particles are applied on the surface of the blank forming the glossy ink layer to form a positioning dry particle layer. In this embodiment, the Sacmi dry particle digital printer DDG four-channel digital printing system is used, and the glue ink of the Itaga company model CIK-AD1109 is selected. The gray value of the glue design is 85%. A variety of dry particles are mixed and used. The ratio of the various dry particles and the raw material components of the dry particles are shown in Tables 3 and 4, where the ratio of the second channel skin dry particles to the color dry particles is 90:10; the ratio of the fourth channel skin dry particles to the functional dry particles is 75:25. The gray value of the positioning dry particle design is 90%.

[0099] S7-3, apply protective glaze on the surface of the green body after the above treatment to form a protective glaze layer; use the Xinjingtai reciprocating glaze spray cabinet to spray the protective glaze. The protective glaze of this embodiment is made of various chemical raw materials from Lianxing Company, including 50 parts of suspending agent, 30 parts of H188015 dry particles, 10 parts of GY381025 dry particles, and 10 parts of B09 transparent glaze slurry by weight. The specific gravity of the protective glaze is 1.43g / mL, the flow rate is 14s, and the glaze amount is 360g / m 2 .

[0100] S8. After drying at 150°C for 15 minutes, the product is sent to a kiln and fired in a roller kiln at 1220°C with a firing cycle of 80 minutes. The product is kept warm in a high temperature zone for 14 minutes to obtain the multi-layered three-dimensional effect ceramic tile.

[0101] Comparative Example 1

[0102] This comparative example adopts the same raw material formula and preparation process as Example 1, except that in step S3, the convex glaze layer is prepared by roller printing process.

[0103] Comparative Example 2

[0104] This comparative example adopts the same raw material formula and preparation process as Example 1, except that in step S3, the convex glaze layer is prepared by inkjet printing process.

[0105] Comparative Example 3

[0106] This comparative example adopts the same raw material formula and preparation process as Example 1, except that in step S3, the screen mesh number is 100 meshes and the photosensitive adhesive is thickened once.

[0107] Comparative Examples 4-5

[0108] This comparative example adopts the same raw material formula and preparation process as Example 1, except that the raw material formula of the raised effect glaze is adjusted, as shown in Table 2.

[0109] Comparative Example 6

[0110] This comparative example adopts the same raw material formula and preparation process as Example 3, except that the raw material formula of the skin dry particles is adjusted, as shown in Table 3.

[0111] Comparative Examples 7 to 8

[0112] This comparative example adopts the same raw material formula and preparation process as Example 4, except that the gray value comparison of the double-positioning glue dry particle design diagram is adjusted, as shown in Table 4.

[0113] Table 1 Raw material formula of base glaze (parts)

[0114] Example 1 Example 2 Example 3 Example 4 Potassium feldspar 22 22 20 20 Sodium feldspar 15 15 15 15 Kaolin 10 10 10 10 quartz 18 18 18 17 Alumina 6 6 6 6 Calcined clay 8 6 8 8 Burnt Talc 9 7 7 6 Zirconium silicate 12 16 16 18

[0115] Table 2 Raw material formula of convex effect glaze (parts)

[0116] Example 1 Example 2 Example 3 Example 4 Comparative Example 4 Comparative Example 5 Potassium feldspar 24 20 20 18 28 30 Nepheline 14 14 10 10 20 20 Kaolin 10 10 12 12 4 11 Coal Gangue 10 11 11 13 10 5 Alumina 8 8 8 6 10 8 Fused Silica 11 11 13 13 11 3 Spinel 10 12 12 14 4 10 Zinc Oxide 3 4 4 4 3 3 Zirconium silicate 10 10 10 10 10 10

[0117] Table 3 Skin dry granule raw material formula (portions)

[0118]

[0119]

[0120] Table 4 Gray value of double positioning glue dry particle design drawing (%)

[0121] Example 3 Example 4 Comparative Example 7 Comparative Example 8 Positioning glue grayscale (%) 80 100 20 80 Positioning dry particle grayscale (%) 75 100 80 30

[0122] Note: The positioning dry particles are prepared by mixing skin dry particles with color dry particles or skin dry particles with functional dry particles, wherein the functional dry particles can be a mixture of one or more of ice crystal dry particles, metal dry particles, bright dry particles, cracked dry particles, polycrystalline dry particles, etc. The functional dry particles can be purchased in a known manner.

[0123] The height difference of the concave-convex texture, the color saturation of the glaze and the tactile feel of the glaze of Examples 1 to 4 and Comparative Examples 1 to 8 were tested. Among them, the test method for the height difference of the concave-convex texture is: the thickness of the ceramic tile from the bottom of the ceramic tile to the highest point of the surface protrusion is measured with a vernier caliper, which is h1, and the thickness of the ceramic tile from the bottom of the ceramic tile to the position of the surface groove is h2, and the height difference of the concave-convex texture is ΔH=h1-h2. The test method for the color saturation of the glaze surface is: the saturation of the color on the surface of the ceramic tile is tested with a colorimeter, and a 100 grayscale design drawing is printed. After the firing is completed, the saturation of the color on the surface of the ceramic tile is measured. The higher the value is ≥90%, the darker the color and the better the color; the saturation is 80-90%, the color is good; the lower the saturation value is <80%, the worse the color. The test method of tactile lubricity is based on the national standard GB / T 4100-2015 Appendix M "Determination of Friction Coefficient" using the static friction coefficient for testing. The lower the static friction coefficient, the smoother the touch and the better the feel. The higher the static friction coefficient, the rougher the surface and the worse the feel. The test results are shown in Table 5:

[0124] Table 5 Glaze effect test results

[0125]

[0126]

[0127] like Figure 1 As shown, the multi-layered three-dimensional effect ceramic tile prepared by the present invention includes, from bottom to top, a ceramic tile body 1, a bottom glaze layer 2, a convex glaze layer 3, a replica ink layer 4, a replica surface glaze layer 5, a pattern layer 6, a glossy ink layer 7, a positioning dry particle layer 8, and a protective glaze layer 9. It can be seen that the convex glaze layer 3 printed by screen printing is below the pattern layer 6, so that the pattern layer has a three-dimensional effect; the composite effect of the replica ink and the replica surface glaze forms a groove texture; the positioning dry particle layer 8 is above the pattern layer 6, so that the ceramic tile of the present invention has a variety of different convex effects. Among them, the distribution paths of the replica ink layer 4, the glossy ink layer 7, and the positioning dry particle layer 8 match the design pattern. Figure 2 , Figure 3 These are the actual pictures of Example 3 and Example 4 respectively. It can be seen that the surface of the ceramic tile has obvious and diverse concave-convex textures, good three-dimensional effect, and high color saturation.

[0128] From the test results, it can be seen that Example 1 and Example 2 use screen printing raised effect glaze to form a raised glaze layer, and the raised height can reach 1.6mm, which greatly exceeds the raised height formed by roller printing in Comparative Example 1 and the raised height formed by inkjet printing in Comparative Example 2. The color saturation of the glaze surface is 83-85%, and the pattern color rendering effect is good. Example 3 and Example 4 use DDG digital printing to position dry particles to form a positioning dry particle layer, which significantly increases the raised height, and the height difference of the concave-convex texture can reach 2.5mm, making the concave-convex texture more three-dimensional, while significantly increasing the color saturation of the glaze surface, making the pattern decoration effect better. The tile surface friction coefficient of Examples 1 to 4 is low and the touch is smooth.

[0129] The height difference of the concave-convex texture of comparative example 3 is 0.7, which is significantly lower than that of embodiment 1. The screen mesh number of the screen printing of comparative example 3 is large, and the number of thickening times of the photosensitive resin is relatively reduced, so that the height difference of the concave-convex texture after firing is small, and the three-dimensional effect is not obvious.

[0130] The height difference of the concave-convex texture of comparative example 4 is only 0.7 mm, which is lower than that of embodiment 1. Since the high-temperature viscosity is significantly reduced after the kaolin and spinel components in the raised glaze are relatively reduced, the firing hardness is reduced, and the glaze has high fluidity, so the height of the raised protrusion after firing is also relatively low, and the color saturation of the glaze surface is 76%, indicating that during the firing process, the edges of the raised protrusions melt and collapse and spread to the surroundings, thereby blurring the pattern texture and causing poor pattern effect.

[0131] The height difference of the concave-convex texture of comparative example 5 is only 0.9 mm, which is lower than that of the concave-convex texture of example 1. Since the gangue and fused quartz components in the raised glaze are relatively reduced, the glaze temperature and high-temperature viscosity are reduced during firing, the leveling property is too large, and the glaze is severely dispersed after high-temperature melting, so the raised effect is not obvious, and the pattern texture is not clear, and the color saturation of the glaze surface is also reduced to 78%.

[0132] In the skin dry particle formula of Comparative Example 6, the magnesium nitride and zinc oxide components are relatively reduced, and the friction coefficient of the ceramic tile surface after firing is 0.75, and the hand feel is relatively rough.

[0133] The printing grayscale value of the positioning glue in Comparative Example 7 is 20%, and the printing grayscale value of the positioning dry particles in Comparative Example 8 is 30%. The height differences of the concave and convex textures after firing are 1.5 mm and 1.7 mm, respectively, which are significantly lower than 2.5 mm in Example 4. The proportion of glue in Comparative Example 7 is small, the bonding strength is insufficient, and most of the positioning dry particles are not fixed, which easily causes edge diffusion and unclear patterns. The color saturation of the glaze is 84%, which is lower than 90%, and the raised texture is also small. Although the proportion of glue in Comparative Example 8 is appropriate, the amount of dry particles applied is insufficient, so the raised texture formed is small and the three-dimensional effect is not obvious.

[0134] In summary, the present invention uses screen printing to print a raised effect glaze before the pattern layer to form a raised glaze layer, so that the pattern layer is three-dimensional, and the concave-convex texture is more obvious, while not affecting the color rendering of the pattern color, and can ensure that the glaze color saturation is high. The groove texture formed by the replica ink and the replica glaze can form a three-dimensional concave-convex texture that can replace the digital steel film. Combined with the dry particle digital printer DDG digital application dual positioning dry particles, compound skin dry particles and functional dry particles, a plurality of raised layers with different heights and shapes and different decorative effects are formed above the pattern layer, which can further enhance the three-dimensional effect of the tile surface and improve the glaze color saturation. By improving and optimizing the technical parameters, the technical solution of Example 4 in this solution is the optimal solution.

[0135] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by the content of the present invention specification, or direct / indirect application in other related technical fields within the concept and extension of the present invention are included in the patent protection scope of the present invention.

Claims

1. A multi-layered three-dimensional effect ceramic tile, characterized in that: It comprises a ceramic tile body, a base glaze layer, a convex glaze layer, a replica ink layer, a replica surface glaze layer, a pattern layer and a protective glaze layer which are stacked in sequence; the distribution paths of the convex glaze layer and the replica ink layer match the design pattern; the convex glaze layer is screen-printed onto the base glaze layer, and the screen mesh number is 30 to 80.

2. A multi-layered three-dimensional effect ceramic tile as claimed in claim 1, characterized in that: The raw materials for preparing the convex glaze layer include convex effect glaze, printing paste and printing oil; the raw material components of the convex effect glaze include, by weight: 15-25 parts of potassium feldspar, 8-16 parts of nepheline, 8-16 parts of kaolin, 8-14 parts of coal gangue, 4-12 parts of aluminum oxide, 8-14 parts of fused quartz, 6-18 parts of spinel, 2-6 parts of zinc oxide and 4-16 parts of zirconium silicate.

3. The multi-layered three-dimensional effect ceramic tile according to claim 1, characterized in that: A glossy ink layer and a positioning dry particle layer are sequentially arranged between the pattern layer and the protective glaze layer, and the distribution paths of the glossy ink layer and the positioning dry particle layer match the design pattern.

4. The multi-layered three-dimensional effect ceramic tile according to claim 3, characterized in that: The raw materials for preparing the positioned dry particle layer include one or more of skin dry particles and functional dry particles, and the functional dry particles include one or more of colored dry particles, ice crystal dry particles, metal dry particles, bright dry particles, cracked dry particles and polycrystalline dry particles.

5. The multi-layered three-dimensional effect ceramic tile according to claim 4, characterized in that: The raw material components of the skin dry particles include, by weight: 12 to 22 parts of lithium feldspar, 10 to 18 parts of albite, 3 to 9 parts of kaolin, 6 to 16 parts of dolomite, 8 to 20 parts of strontium carbonate, 8 to 16 parts of magnesium nitride, 4 to 10 parts of diamond, 6 to 14 parts of zinc oxide and 6 to 12 parts of fluorite.

6. The multi-layered three-dimensional effect ceramic tile according to claim 1, characterized in that: The raw materials for preparing the base glaze layer include, by weight: 16 to 24 parts of potassium feldspar, 10 to 20 parts of sodium feldspar, 5 to 15 parts of kaolin, 14 to 22 parts of quartz, 4 to 8 parts of aluminum oxide, 6 to 10 parts of calcined clay, 4 to 10 parts of calcined talc and 12 to 20 parts of zirconium silicate.

7. The multi-layered three-dimensional effect ceramic tile according to claim 1, characterized in that: The raw materials for preparing the replica glaze layer include, by weight: 18 to 26 parts of potassium feldspar, 10 to 20 parts of sodium feldspar, 5 to 15 parts of air knife clay, 10 to 18 parts of fused quartz, 3 to 7 parts of aluminum oxide, 4 to 10 parts of calcined clay, 4 to 8 parts of calcined talc, 3 to 7 parts of zinc oxide and 12 to 20 parts of zirconium silicate.

8. A process for preparing a multi-layered three-dimensional effect ceramic tile as claimed in claim 1, characterized in that: The steps include: S1, pressing the ceramic blank into shape, and after drying, forming a ceramic tile body; S2, applying a base glaze on the ceramic tile body to form a base glaze layer; S3, printing convex glaze on the base glaze layer using a screen printing machine according to the design pattern to form a convex glaze layer; S4, according to the design pattern, performing inkjet printing on the base glaze layer to apply replica ink to form a replica ink layer; S5, applying a replica glaze on the surface of the ceramic tile body composited with the convex glaze layer and the replica ink layer to form a replica glaze layer; S6, printing color ink according to the design pattern on the replica glaze layer to form a pattern layer; S7, applying a protective glaze on the surface of the body on which the pattern layer is formed, to form a protective glaze layer; S8, after drying, firing in a kiln to obtain the multi-layered three-dimensional effect ceramic tile.

9. A preparation process according to claim 8, characterized in that: After step S6, the following steps are also included: S7-1, printing glossy ink on the pattern layer according to the design pattern to form a glossy ink layer; S7-2, applying positioning glue and dry particles on the surface of the blank forming the glossy ink layer according to the design pattern to form a positioning dry particle layer; S7-3, applying a protective glaze on the surface of the green body after the above treatment to form a protective glaze layer; S8, after drying, firing in a kiln to obtain the multi-layered three-dimensional effect ceramic tile.

10. A preparation process according to claim 9, characterized in that: The positioning dry particle layer is applied by digital printing using a dry particle digital printer.

Citation Information

Patent Citations

  • Glazed tile with wallpaper or bark-shaped surface and concave and convex effect and preparation method

    CN103880474A

  • Multi-dimension decorative wood-grained ceramic tile with original edges and production method of multi-dimension decorative wood-grained ceramic tile with original edges

    CN110372416A

  • Colorful marble tile with 3D digital mold effect and preparation method of colorful marble tile

    CN118145975A

  • The protruding grains - fuse forming method

    JP1989003088A

  • Production of transparent semi-spherical spinel sintered product

    JP1993043359A

Cited By

  • Ceramic tile with concave-convex textures and preparation method thereof

    CN119330754A

  • Preparation method of polished tile with local inlaid pattern effect

    CN119610341A

  • Preparation method of high-performance antiskid ceramic tile

    CN120157517A

  • Silky ceramic tile with multi-layer stone texture and preparation method thereof

    CN120483775A