Naphthalene-ring-containing bio-based polyamide copolymer material and preparation method thereof
By synthesizing naphthalene ring-containing bio-based polyamide copolymer materials in high-temperature and high-pressure reactors, the problem of insufficient thermal performance and ductility of the material in the prior art is solved, and the high-temperature characteristics and ductility of the material are improved, and it is suitable for a variety of applications Scene.
Patent Information
- Application Number
- CN202410970974.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-15
AI Technical Summary
The lack of high-performance polyamide materials that use naphthalene ring structures and bio-based long carbon chains is copolymerized in the prior art, resulting in insufficient thermal performance and ductility of the material, making it difficult to meet the needs of high-performance products.
By synthesizing naphthalene ring-containing bio-based polyamide copolymerization materials in a high-temperature and autoclave reactor, copolymerization of naphthalene ring structure diacid/diesters with bio-based long carbon chain diamine, combining a variety of catalysts and nucleating agents, the reaction conditions are controlled To form a polyamide material with a wide melting point range.
The high-temperature characteristics and ductility of the material have been improved, with a melting point of more than 300℃ and excellent ductility. It is suitable for a variety of application scenarios, and the efficiency is improved through the coordinated catalysis of economical deionized water and a variety of catalysts.
Smart Images

Figure CN118955891A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer synthesis and relates to a synthesis and modification preparation method of a naphthalene ring-containing bio-based polyamide copolymer material. Background Art
[0002] Polyamide, also known as nylon, is a thermoplastic polymer with repeating structural units of amide groups (-CO-NH-) on its main chain. Polyamide has many excellent properties, such as high crystallinity, high surface hardness, wear resistance, low friction coefficient, self-lubrication, shock absorption and sound absorption. However, different polyamide polymers have different properties, with obvious advantages and disadvantages. Therefore, in order to obtain polyamide materials with better performance, polyamide is usually physically or chemically modified in industry to achieve better use effects. Copolymerization of polyamide is a common chemical modification method. Through molecular structure design, suitable comonomers are selected according to the chemical structure of the target polymer to obtain materials with desired properties. Considering sustainable development, it is more meaningful to use bio-based raw materials as copolymers. For polyamide, the density of amide bonds and the length of alkyl chains in the molecule are crucial to its performance. In general, increasing the density of amide bonds will enhance the intermolecular hydrogen bonding interaction and molecular polarity, resulting in higher water absorption and more perfect crystallization. In addition, longer alkyl chains will increase the flexibility of the molecular chain and enhance the ductility and plasticity of the material.
[0003] In recent years, with the rapid development of electronic appliances, new energy vehicles, LED and other industries, the market demand for the application of polyamide materials to high-performance products has greatly increased, especially high-performance polyamide materials. At present, there is no report on semi-aromatic long carbon chain bio-based copolymer polyamide materials with naphthalene ring monomers added to the molecular chain. Therefore, it is an effective way to obtain polyamide by copolymerizing diacids / diesters of naphthalene ring structure with bio-based long carbon chain diamines / diacids. Among the obtained polyamides, the melting point of naphthalene ring polyamides with ten methylene groups in the main chain can be as high as 313.30℃ or as low as 164,50℃, and the application range of thermal properties is very wide. Under the premise of not affecting the performance, it is of great significance to copolymerize and modify the naphthalene ring-containing polyamide to improve the ductility and plasticity of the material. Summary of the invention
[0004] The purpose of the present invention is to synthesize a novel naphthalene ring-containing bio-based polyamide copolymer material with a wide melting point range.
[0005] Another object of the present invention is to provide a method for preparing the above-mentioned naphthalene ring-containing bio-based polyamide copolymer material. To achieve the above-mentioned object, the present invention adopts the following technical scheme:
[0006] A naphthalene ring-containing bio-based polyamide copolymer material, characterized in that the material comprises the following component raw materials: 100 molar parts of naphthalene ring structure diacid / diester and bio-based long carbon chain dibasic acid, wherein the naphthalene ring structure diacid / diester is 20-90 parts, and the rest is bio-based long carbon chain dibasic acid;
[0007] 100-102 mole parts of a bio-based long carbon chain diamine;
[0008] 0.3-0.5 parts by mass of a catalyst;
[0009] 0.3-0.5 parts by mass of a nucleating agent;
[0010] 50-200 parts by mass of deionized water;
[0011] The naphthalene ring structure diacid / diester is one of 1,3-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid dimethyl ester, 2,6-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid dimethyl ester, 2,6-naphthalene dicarboxylic acid dimethyl ester, 2,7-naphthalene dicarboxylic acid dimethyl ester, and 2,6-naphthalene dicarboxylic acid diethyl ester;
[0012] The bio-based long carbon chain dibasic acid is one of dodecanedioic acid, sebacic acid and tetradecanedioic acid;
[0013] The bio-based long carbon chain diamine is one of decanediamine, dodecanediamine and tetradecanediamine;
[0014] The catalyst is a combination of one or more of sodium hypophosphite, sodium phosphite, potassium hypophosphite, magnesium hypophosphite, calcium hypophosphite or zinc hypophosphite and stannous chloride;
[0015] The nucleating agent is one of calcium carbonate, barium sulfate, silicon dioxide, titanium dioxide and talc.
[0016] The present invention also provides a method for preparing the above-mentioned naphthalene ring-containing bio-based polyamide copolymer material, comprising the following steps:
[0017] Step 1, weighing the naphthalene ring structure diacid / diester, bio-based long carbon chain dibasic acid, bio-based long carbon chain diamine, catalyst, nucleating agent, and deionized water according to the above components into a high temperature and high pressure reactor, sealing the high temperature and high pressure reactor, starting a stirring device, and filling the reactor with inert gas to replace the residual air therein, repeating the gas replacement 5-10 times, and retaining 0.1-0.5MPa of inert gas in the reactor as a protective gas after the replacement is completed;
[0018] Step 2: After the components are mixed, the high temperature and high pressure polymerization reactor is heated to 70-90°C, the stirring rate is 200-300r / min, and the temperature is maintained for 2-3h until the reaction is complete to form a polyamide salt;
[0019] Step 3, after the insulation is completed, the high-temperature and high-pressure polymerization reactor is continued to be heated and stirred. After the pressure in the reactor reaches 1.5-2.5MPa, the solvent system is released to make the reactor in a constant pressure state. After the temperature in the reactor continues to rise to 240-280°C and then maintained for 2-3h, the reactor is depressurized to normal pressure within 1.5-3h, and the stirring speed is reduced to 10-50r / min. At this time, the temperature in the reactor is controlled to be maintained at 240-280°C for 2-3h, and then the temperature is kept unchanged, and the reactor is evacuated to -0.1MPa and maintained for 1h to obtain a polyamide prepolymer;
[0020] Step 4: Grind the polyamide prepolymer obtained in step 3 into a powder of 0.1-1 mm and then perform solid phase polycondensation, evacuate the pressure to -0.1 MPa, set the temperature to 20-30° C. lower than the melting point of the prepolymer, and obtain a polyamide polymer after 8-12 hours.
[0021] The inert gas in step 1 is one of nitrogen, carbon dioxide, argon or helium; preferably, the inert gas is nitrogen.
[0022] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0023] (1) The partial naphthalene ring-containing long carbon chain polyamide described in the present invention has a melting temperature of more than 300°C and has high temperature resistance. It has not yet been industrialized and there are relatively few related research reports. It has high research value and broad research prospects and is expected to be industrialized in the future.
[0024] (2) The melting point of the copolymer of the present invention changes with the change of the content of the long carbon chain aliphatic polyamide. The melting point of the polyamide material can be designed within a certain range according to specific needs. The melting point range is large and the thermal performance application range is wide. The copolymerization of naphthalene ring-containing polyamide and bio-based long carbon chain polyamide reduces the melting temperature of the material, but improves its ductility, thereby obtaining a material with better elongation at break.
[0025] (3) The catalyst used in the present invention is a synergistic catalysis of multiple catalysts, which has higher efficiency; and the polymerization solvent is economical, affordable, green and environmentally friendly deionized water. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the infrared structural characterization of Example 1, Example 5, and Example 9 of the present invention. DETAILED DESCRIPTION
[0027] Embodiment 1 A naphthalene ring-containing bio-based polyamide copolymer material, the preparation method is as follows:
[0028] Step 1, weighing 90 parts of 2,6-naphthalene dicarboxylic acid, 10 parts of dodecanedioic acid, 100 parts of decanediamine by mole fraction, 0.2 parts of sodium hypophosphite and 0.1 parts of stannous chloride by mass fraction, 0.5 parts of calcium carbonate as a nucleating agent, and 50 parts of deionized water in a high-temperature and high-pressure reactor, sealing the high-temperature and high-pressure reactor, starting a stirring device, and filling the reactor with nitrogen to replace the residual air therein, repeating the gas replacement 10 times, and retaining 0.5 MPa of nitrogen in the reactor as a protective gas after the replacement is completed;
[0029] Step 2: After the components are mixed, the high temperature and high pressure polymerization reactor is heated to 90° C., the stirring rate is 300 r / min, and the temperature is maintained for 2 hours until the reaction is complete to form a polyamide salt;
[0030] Step 3, after the insulation is completed, the high-temperature and high-pressure polymerization reactor is continued to be heated and stirred. After the pressure in the reactor reaches 2.5MPa, the solvent system is released to make the reactor in a constant pressure state. After the temperature in the reactor continues to rise to 280°C and then maintained for 3h, the reactor is depressurized to normal pressure within 3h, and the stirring speed is reduced to 50r / min. At this time, the temperature in the reactor is controlled to be maintained at 280°C for 3h, and then the temperature is kept unchanged, and the reactor is evacuated to -0.1MPa and maintained for 1h to obtain a polyamide prepolymer;
[0031] Step 4: Grind the polyamide prepolymer obtained in step 3 into a powder of 0.1-1 mm and then perform solid phase polycondensation. The reactor is evacuated to a pressure of -0.1 MPa and the temperature is set to 280° C. After 12 hours, a polyamide polymer is obtained.
[0032] Embodiment 2 A naphthalene ring-containing bio-based polyamide copolymer material, the preparation method is as follows:
[0033] Step 1, weighing 90 parts of 2,6-naphthalene dicarboxylic acid dimethyl ester, 10 parts of dodecanedioic acid, 102 parts of decanediamine, 0.2 parts of sodium phosphite catalyst, 0.1 parts of magnesium hypophosphite, 0.1 parts of stannous chloride, 0.4 parts of barium sulfate nucleating agent, and 100 parts of deionized water in a high temperature and high pressure reactor, sealing the high temperature and high pressure reactor, starting the stirring device, and filling the reactor with carbon dioxide to replace the residual air therein, repeating the gas replacement 9 times, and retaining 0.4MPa of carbon dioxide in the reactor as a protective gas after the replacement is completed;
[0034] Step 2: After the components are mixed, the high temperature and high pressure polymerization reactor is heated to 80° C., the stirring rate is 250 r / min, and the temperature is maintained for 3 hours until the reaction is complete to form a polyamide salt;
[0035] Step 3: After the insulation is completed, the high-temperature and high-pressure polymerization reactor is heated and stirred continuously. After the pressure in the reactor reaches 2.0 MPa, the solvent system is released to keep the reactor in a constant pressure state. After the temperature in the reactor continues to rise to 270°C, it is maintained for 2.5 hours. The reactor is depressurized to normal pressure within 2.5 hours, and the stirring speed is reduced to 40 r / min. At this time, the temperature in the reactor is controlled to be maintained at 270°C for 2.5 hours. Then, the temperature is kept constant, and the pressure is evacuated to -0.1 MPa and maintained for 1 hour to obtain a polyamide prepolymer.
[0036] Step 4: Grind the polyamide prepolymer obtained in step 3 into a powder of 0.1-1 mm and then perform solid phase polycondensation. The reactor is evacuated to a vacuum pressure of -0.1 MPa and the temperature is set to 280° C. After 11 hours, a polyamide polymer is obtained.
[0037] Embodiment 3 A naphthalene ring-containing bio-based polyamide copolymer material, the preparation method is as follows:
[0038] Step 1, weighing 90 parts of diethyl 2,6-naphthalene dicarboxylate, 10 parts of dodecanedioic acid, 101 parts of decanediamine, 0.2 parts of sodium phosphite, 0.1 parts of calcium hypophosphite, 0.1 parts of stannous chloride, 0.5 parts of barium sulfate, and 200 parts of deionized water in a high-temperature and high-pressure reactor, sealing the high-temperature and high-pressure reactor, starting a stirring device, and filling the reactor with argon to replace the residual air therein, repeating the gas replacement 8 times, and retaining 0.3MPa of argon in the reactor as a protective gas after the replacement is completed;
[0039] Step 2: After the components are mixed, the high temperature and high pressure polymerization reactor is heated to 70° C., the stirring rate is 200 r / min, and the temperature is maintained for 2.5 hours until the reaction is complete to form a polyamide salt;
[0040] Step 3: After the insulation is completed, the high-temperature and high-pressure polymerization reactor is heated and stirred continuously. After the pressure in the reactor reaches 1.5 MPa, the solvent system is released to keep the reactor in a constant pressure state. After the temperature in the reactor continues to rise to 270°C and then maintained for 2 hours, the reactor is depressurized to normal pressure within 1.5 hours, and the stirring speed is reduced to 10 r / min. At this time, the temperature in the reactor is controlled to be maintained at 270°C for 3 hours. Then, the temperature is kept constant, and the pressure is evacuated to -0.1 MPa and maintained for 1 hour to obtain a polyamide prepolymer.
[0041] Step 4: Grind the polyamide prepolymer obtained in step 3 into a powder of 0.1-1 mm and then perform solid phase polycondensation. The reactor is evacuated to a vacuum pressure of -0.1 MPa and the temperature is set to 280° C. After 11 hours, a polyamide polymer is obtained.
[0042] Embodiment 4 A naphthalene ring-containing bio-based polyamide copolymer material, prepared by:
[0043] Step 1, weighing 90 parts of 2,7-naphthalene dicarboxylic acid dimethyl ester, 10 parts of dodecanedioic acid, 101 parts of dodecane diamine, 0.2 parts of sodium hypophosphite, 0.2 parts of magnesium hypophosphite, 0.1 parts of stannous chloride, 0.3 parts of calcium carbonate, and 150 parts of deionized water in a high-temperature and high-pressure reactor, sealing the high-temperature and high-pressure reactor, starting a stirring device, and filling the reactor with helium to replace the residual air therein, repeating the gas replacement 10 times, and retaining 0.1MPa of helium in the reactor as a protective gas after the replacement is completed;
[0044] Step 2: After the components are mixed, the high temperature and high pressure polymerization reactor is heated to 70° C., the stirring rate is 200 r / min, and the temperature is maintained for 2 hours until the reaction is complete to form a polyamide salt;
[0045] Step 3: After the insulation is completed, the high-temperature and high-pressure polymerization reactor is heated and stirred continuously. After the pressure in the reactor reaches 1.5 MPa, the solvent system is released to keep the reactor in a constant pressure state. After the temperature in the reactor continues to rise to 280°C and then maintained for 3 hours, the reactor is depressurized to normal pressure within 1.5 hours, and the stirring speed is reduced to 30 r / min. At this time, the temperature in the reactor is controlled to be maintained at 280°C for 3 hours. Then, the temperature is kept constant, and the pressure is evacuated to -0.1 MPa and maintained for 1 hour to obtain a polyamide prepolymer.
[0046] Step 4: Grind the polyamide prepolymer obtained in step 3 into a powder of 0.1-1 mm and then perform solid phase polycondensation. The reaction kettle is evacuated to a pressure of -0.1 MPa and the temperature is set to 270° C. After 8 hours, a polyamide polymer is obtained.
[0047] Embodiment 5 A naphthalene ring-containing bio-based polyamide copolymer material, prepared by:
[0048] Step 1, weighing 60 parts of 2,6-naphthalene dicarboxylic acid, 40 parts of sebacic acid, 102 parts of dodecane diamine, 0.2 parts of sodium hypophosphite, 0.2 parts of magnesium hypophosphite, 0.1 parts of stannous chloride, 0.5 parts of silicon dioxide, and 50 parts of deionized water in a high-temperature and high-pressure reactor, sealing the high-temperature and high-pressure reactor, starting a stirring device, and filling the reactor with nitrogen to replace the residual air therein, repeating the gas replacement 5 times, and retaining 0.2MPa of nitrogen in the reactor as a protective gas after the replacement is completed;
[0049] Step 2: After the components are mixed, the high temperature and high pressure polymerization reactor is heated to 70° C., the stirring rate is 200 r / min, and the temperature is maintained for 2 hours until the reaction is complete to form a polyamide salt;
[0050] Step 3: After the insulation is completed, the high-temperature and high-pressure polymerization reactor is heated and stirred continuously. After the pressure in the reactor reaches 1.5 MPa, the solvent system is released to keep the reactor in a constant pressure state. After the temperature in the reactor continues to rise to 270°C and then maintained for 2 hours, the reactor is depressurized to normal pressure within 1.5 hours, and the stirring speed is reduced to 10 r / min. At this time, the temperature in the reactor is controlled to be maintained at 270°C for 2 hours. Then, the temperature is kept constant, and the pressure is evacuated to -0.1 MPa and maintained for 1 hour to obtain a polyamide prepolymer.
[0051] Step 4: Grind the polyamide prepolymer obtained in step 3 into a powder of 0.1-1 mm and then perform solid phase polycondensation. The reactor is evacuated to a vacuum pressure of -0.1 MPa and the temperature is set to 245° C. After 8 hours, a polyamide polymer is obtained.
[0052] Embodiment 6 A naphthalene ring-containing bio-based polyamide copolymer material, the preparation method is as follows:
[0053] Step 1, weighing 60 parts of 1,5-naphthalene dicarboxylic acid dimethyl ester, 40 parts of dodecanedioic acid, 100 parts of dodecane diamine, 0.3 parts of potassium hypophosphite, 0.1 parts of magnesium hypophosphite, 0.1 parts of stannous chloride, 0.5 parts of titanium dioxide, and 100 parts of deionized water in a high-temperature and high-pressure reactor, sealing the high-temperature and high-pressure reactor, starting a stirring device, and filling the reactor with nitrogen to replace the residual air therein, repeating the gas replacement 5 times, and retaining 0.2MPa of nitrogen in the reactor as a protective gas after the replacement is completed;
[0054] Step 2: After the components are mixed, the high temperature and high pressure polymerization reactor is heated to 80° C., the stirring rate is 200 r / min, and the temperature is maintained for 2 hours until the reaction is complete to form a polyamide salt;
[0055] Step 3: After the insulation is completed, the high-temperature and high-pressure polymerization reactor is heated and stirred continuously. After the pressure in the reactor reaches 1.5 MPa, the solvent system is released to keep the reactor in a constant pressure state. After the temperature in the reactor continues to rise to 280°C, it is maintained for 2 hours. The reactor is depressurized to normal pressure within 1.5-3 hours, and the stirring speed is reduced to 10-50 r / min. At this time, the temperature in the reactor is controlled to be maintained at 280°C for 2-3 hours. Then, the temperature is kept constant, and the reactor is evacuated to -0.1 MPa and maintained for 1 hour to obtain a polyamide prepolymer.
[0056] Step 4: Grind the polyamide prepolymer obtained in step 3 into a powder of 0.1-1 mm and then perform solid phase polycondensation. The reactor is evacuated to a pressure of -0.1 MPa and the temperature is set to 245° C. After 10 hours, a polyamide polymer is obtained.
[0057] Embodiment 7 A naphthalene ring-containing bio-based polyamide copolymer material, the preparation method is:
[0058] Step 1, weighing 60 parts of 1,3-naphthalene dicarboxylic acid, 40 parts of tetradecanedioic acid, 100 parts of tetradecanediamine, 0.3 parts of magnesium hypophosphite, 0.2 parts of stannous chloride, 0.3 parts of nucleating agent talc, and 150 parts of deionized water in a high-temperature and high-pressure reactor, sealing the high-temperature and high-pressure reactor, starting a stirring device, and filling the reactor with nitrogen to replace the residual air therein, repeating the gas replacement 10 times, and retaining 0.5MPa of nitrogen in the reactor as a protective gas after the replacement is completed;
[0059] Step 2: After the components are mixed, the high temperature and high pressure polymerization reactor is heated to 90° C., the stirring rate is 200 r / min, and the temperature is maintained for 2 hours until the reaction is complete to form a polyamide salt;
[0060] Step 3: After the insulation is completed, the high-temperature and high-pressure polymerization reactor is heated and stirred continuously. After the pressure in the reactor reaches 1.5 MPa, the solvent system is released to keep the reactor in a constant pressure state. After the temperature in the reactor continues to rise to 280°C and then maintained for 3 hours, the reactor is depressurized to normal pressure within 1.5 hours, and the stirring speed is reduced to 10 r / min. At this time, the temperature in the reactor is controlled to be maintained at 280°C for 2 hours. Then, the temperature is kept constant, and the pressure is evacuated to -0.1 MPa and maintained for 1 hour to obtain a polyamide prepolymer.
[0061] Step 4: Grind the polyamide prepolymer obtained in step 3 into a powder of 0.1-1 mm and then perform solid phase polycondensation. The reactor is evacuated to a pressure of -0.1 MPa and the temperature is set to 240° C. After 8 hours, a polyamide polymer is obtained.
[0062] Embodiment 8 A naphthalene ring-containing bio-based polyamide copolymer material, the preparation method is as follows:
[0063] Step 1, weighing 60 parts of 2,7-naphthalene dicarboxylic acid dimethyl ester, 40 parts of dodecanedioic acid, 102 parts of tetradecane diamine, 0.1 parts of sodium hypophosphite, 0.1 parts of magnesium hypophosphite, 0.1 parts of calcium hypophosphite, 0.1 parts of stannous chloride, 0.5 parts of calcium carbonate, and 200 parts of deionized water in a high-temperature and high-pressure reactor, sealing the high-temperature and high-pressure reactor, starting a stirring device, and filling the reactor with nitrogen to replace the residual air therein, repeating the gas replacement 10 times, and retaining 0.2MPa of inert gas in the reactor as a protective gas after the replacement is completed;
[0064] Step 2: After the components are mixed, the high temperature and high pressure polymerization reactor is heated to 70° C., the stirring rate is 200 r / min, and the temperature is maintained for 2.5 hours until the reaction is complete to form a polyamide salt;
[0065] Step 3: After the insulation is completed, the high-temperature and high-pressure polymerization reactor is heated and stirred continuously. After the pressure in the reactor reaches 1.5 MPa, the solvent system is released to keep the reactor in a constant pressure state. After the temperature in the reactor continues to rise to 280°C and then maintained for 3 hours, the reactor is depressurized to normal pressure within 2 hours, and the stirring speed is reduced to 35 r / min. At this time, the temperature in the reactor is controlled to be maintained at 280°C for 3 hours. Then, the temperature is kept constant, and the pressure is evacuated to -0.1 MPa and maintained for 1 hour to obtain a polyamide prepolymer.
[0066] Step 4: Grind the polyamide prepolymer obtained in step 3 into a powder of 0.1-1 mm and then perform solid phase polycondensation. The reactor is evacuated to a pressure of -0.1 MPa and the temperature is set to 250° C. After 10 hours, a polyamide polymer is obtained.
[0067] Embodiment 9 A naphthalene ring-containing bio-based polyamide copolymer material, the preparation method is as follows:
[0068] Step 1, weighing 20 parts of 1,5-naphthalene dicarboxylic acid dimethyl ester, 80 parts of tetradecanedioic acid, 101 parts of tetradecanediamine, 0.2 parts of sodium hypophosphite, 0.1 parts of magnesium hypophosphite, 0.1 parts of zinc hypophosphite, 0.1 parts of stannous chloride, 0.4 parts of calcium carbonate, and 200 parts of deionized water in a high-temperature and high-pressure reactor, sealing the high-temperature and high-pressure reactor, starting a stirring device, and filling the reactor with argon to replace the residual air therein, repeating the gas replacement 6 times, and retaining 0.2MPa of argon in the reactor as a protective gas after the replacement is completed;
[0069] Step 2: After the components are mixed, the high temperature and high pressure polymerization reactor is heated to 75° C., the stirring rate is 200 r / min, and the temperature is maintained for 2 hours until the reaction is complete to form a polyamide salt;
[0070] Step 3: After the insulation is completed, the high-temperature and high-pressure polymerization reactor is heated and stirred continuously. After the pressure in the reactor reaches 1.7 MPa, the solvent system is released to keep the reactor in a constant pressure state. After the temperature in the reactor continues to rise to 240°C, it is maintained for 2 hours. The reactor is depressurized to normal pressure within 2 hours, and the stirring speed is reduced to 10 r / min. At this time, the temperature in the reactor is controlled to be maintained at 240°C for 3 hours. Then, the temperature is kept constant, and the pressure is evacuated to -0.1 MPa and maintained for 1 hour to obtain a polyamide prepolymer.
[0071] Step 4: Grind the polyamide prepolymer obtained in step 3 into a powder of 0.1-1 mm and then perform solid phase polycondensation. The reaction kettle is evacuated to a pressure of -0.1 MPa and the temperature is set to 140° C. After 8 hours, a polyamide polymer is obtained.
[0072] Embodiment 10 A naphthalene ring-containing bio-based polyamide copolymer material, prepared by:
[0073] Step 1, weighing 20 parts of 1,4-naphthalene dicarboxylic acid dimethyl ester, 80 parts of dodecanedioic acid, 100 parts of decanediamine, 0.1 parts of sodium hypophosphite, 0.1 parts of magnesium hypophosphite, 0.2 parts of zinc hypophosphite, 0.1 parts of stannous chloride, 0.5 parts of calcium carbonate, and 200 parts of deionized water in a high-temperature and high-pressure reactor, sealing the high-temperature and high-pressure reactor, starting a stirring device, and filling the reactor with nitrogen to replace the residual air therein, repeating the gas replacement 5 times, and retaining 0.4MPa of nitrogen in the reactor as a protective gas after the replacement is completed;
[0074] Step 2: After the components are mixed, the high temperature and high pressure polymerization reactor is heated to 70° C., the stirring rate is 200 r / min, and the temperature is maintained for 2 hours until the reaction is complete to form a polyamide salt;
[0075] Step 3: After the insulation is completed, the high-temperature and high-pressure polymerization reactor is heated and stirred continuously. After the pressure in the reactor reaches 1.5 MPa, the solvent system is released to keep the reactor in a constant pressure state. After the temperature in the reactor continues to rise to 240°C and then maintained for 2 hours, the reactor is depressurized to normal pressure within 1.5 hours, and the stirring speed is reduced to 20 r / min. At this time, the temperature in the reactor is controlled to be maintained at 240°C for 3 hours. Then, the temperature is kept constant, and the pressure is evacuated to -0.1 MPa and maintained for 1 hour to obtain a polyamide prepolymer.
[0076] Step 4: Grind the polyamide prepolymer obtained in step 3 into a powder of 0.1-1 mm and then perform solid phase polycondensation. The reactor is evacuated to a pressure of -0.1 MPa and the temperature is set to 140° C. After 10 hours, a polyamide polymer is obtained.
[0077] The structural characterization and performance test results of the embodiment are as follows Figure 1 As shown in Table 1. The infrared structure was characterized by total reflection mode of Bruker infrared spectrometer; the thermal properties were tested by differential scanning calorimeter and thermogravimetric analyzer under nitrogen atmosphere and heating rate of 10°C / min; the relative viscosity was tested by relative viscosity meter in 1g / dL concentrated sulfuric acid; the density was tested by true density meter; the tensile strength and elongation at break were measured by GB / T 2918-2018.
[0078] Table 1
[0079]
[0080] Table 1 above gives the glass transition temperature, melting point, decomposition temperature, relative viscosity, density, tensile strength, elongation at break and other properties of the embodiments of the present invention. As can be seen from Table 1, the embodiments have a high decomposition temperature of more than 418°C, a relative viscosity of 1.98-2.16, and a true density of 1.07-1.23g / ml. Embodiments 1-4 contain 90% of naphthalene ring structure diacid / diester, have excellent thermal properties and tensile strength, glass transition temperature above 100°C, melting point above 300°C, tensile strength above 85MPa, and elongation at break of about 83%. Embodiments 5-8 contain 60% of naphthalene ring structure diacid / diester, have higher thermal properties and mechanical properties, glass transition temperature between 66-72°C, melting point between 269-280°C, tensile strength between 58-61MPa, and elongation at break between 145-150%. Embodiments 9-10 contain 20% naphthalene ring structure diacid / diester. Although the thermal properties and tensile strength are reduced, the glass transition temperature is below 46°C, the melting point is below 168°C, and the tensile strength is below 43MPa, the ductility of the material is improved, and the elongation at break is more than 280%. Through the above data analysis, the thermal properties and mechanical properties of the naphthalene ring-containing polyamide synthesized by the present invention have a wide range of spans, and the performance characteristics are obvious. It can be used in different scenarios within a certain range of use, and the application prospects are very broad.
[0081] Figure 1 The infrared structural characterization shown indicates the successful synthesis of the polymer. Since the infrared structural characterization diagrams of the remaining examples are almost the same as those of Example 1, Example 5, and Example 9, they are not shown.
[0082] The experimental schemes described above can be further combined or replaced, and the implementation schemes are only descriptions of preferred embodiments of the present invention, and do not limit the concept and scope of the present invention. Without departing from the design concept of the present invention, various changes and improvements made by ordinary technicians in this field to the technical scheme of the present invention belong to the protection scope of the present invention. The protection scope of the present invention is given by the attached claims and any equivalents thereof.
Claims
1. A naphthalene ring-containing bio-based polyamide copolymer material, It is characterized in that The material includes the following raw materials: 100 mole parts of naphthalene ring structure diacid / diester and bio-based long carbon chain dibasic acid, wherein the naphthalene ring structure diacid / diester is 20-90 parts and the rest is bio-based long carbon chain dibasic acid; 100-102 mole parts of a bio-based long carbon chain diamine; 0.3-0.5 parts by mass of a catalyst; 0.3-0.5 parts by mass of a nucleating agent; 50-200 parts by mass of deionized water; The naphthalene ring structure diacid / diester is one of 1,3-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid dimethyl ester, 2,6-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid dimethyl ester, 2,6-naphthalene dicarboxylic acid dimethyl ester, 2,7-naphthalene dicarboxylic acid dimethyl ester, and 2,6-naphthalene dicarboxylic acid diethyl ester; The bio-based long carbon chain dibasic acid is one of sebacic acid, dodecanedioic acid and tetradecanedioic acid; The bio-based long carbon chain diamine is one of decanediamine, dodecanediamine and tetradecanediamine; The catalyst is a combination of one or more of sodium hypophosphite, sodium phosphite, potassium hypophosphite, magnesium hypophosphite, calcium hypophosphite or zinc hypophosphite and stannous chloride; The nucleating agent is one of calcium carbonate, barium sulfate, silicon dioxide, titanium dioxide and talc.
2. A method for preparing a naphthalene ring-containing bio-based polyamide copolymer material according to claim 1, Features The following steps are involved: Step 1, weighing naphthalene ring structure diacid / diester, bio-based long carbon chain dibasic acid, bio-based long carbon chain diamine, catalyst, nucleating agent, and deionized water according to the above components into a high temperature and high pressure reactor, sealing the high temperature and high pressure reactor, starting a stirring device, and filling the reactor with inert gas to replace the residual air therein, repeating the gas replacement 5-10 times, and retaining 0.1-0.5 MPa of inert gas in the reactor as a protective gas after the replacement is completed; Step 2: After the components are mixed, the high temperature and high pressure polymerization reactor is heated to 70-90°C, the stirring rate is 200-300 r / min, and the temperature is maintained for 2-3 hours until the reaction is complete to form a polyamide salt; Step 3: After the insulation is completed, the high-temperature and high-pressure polymerization reactor is continued to be heated and stirred. After the pressure in the reactor reaches 1.5-2.5 MPa, the solvent system is released to keep the reactor in a constant pressure state. After the temperature in the reactor continues to rise to 240-280 ° C, it is maintained for 2-3 hours. The reactor is depressurized to normal pressure within 1.5-3 hours, and the stirring speed is reduced to 10-50 r / min. At this time, the temperature in the reactor is controlled to be maintained at 240-280 ° C for 2-3 hours, and then the temperature is kept unchanged, and the reactor is evacuated to -0.1 MPa and maintained for 1 hour before discharging; Step 4: Grind the polyamide prepolymer obtained in step 3 into a powder of 0.1-1 mm and then perform solid phase polycondensation. The reactor is evacuated to a pressure of -0.1 MPa and the temperature is set 20-30°C lower than the melting point of the prepolymer. After 8-12 hours, a polyamide polymer is obtained.
3. The method for preparing a naphthalene ring-containing bio-based polyamide copolymer material according to claim 2, Features The inert gas in step 1 is one of nitrogen, carbon dioxide, argon or helium.
Citation Information
Cited By
Naphthalene-containing nylon material, hydrogen storage container inner container and preparation methods of naphthalene-containing nylon material and hydrogen storage container inner container
CN120504828A
Bio-based dipolyamine polyamide and preparation method of flexible sensor of bio-based dipolyamine polyamide