All-steel radial tire formula of modified zinc oxide and preparation method of all-steel radial tire formula
By preparing modified zinc oxide and adding it in stages to a mixer, the problem of fatigue failure of tire airtight layer rubber material caused by replacing traditional zinc oxide with low-content zinc oxide was solved. This method also achieved good dispersion of zinc oxide and carbon black, thus improving the physical and mechanical properties of tires.
Patent Information
- Application Number
- CN202411460828.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-18
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In existing technologies, when low-content zinc oxide directly replaces traditional zinc oxide, the tire airtight layer rubber material is prone to fatigue failure, mainly due to microscopic defects caused by large or agglomerated zinc oxide particles and uneven carbon black dispersion.
Modified zinc oxide was used to replace traditional zinc oxide. Loaded zinc oxide was prepared by using the rubber additive Nanoprene as a carrier. The rubber mixture was added to the internal mixer in three parts. Combined with mechanical shearing, the dispersibility of zinc oxide and carbon black was improved.
It improves the dispersion of zinc oxide in the rubber compound, reduces micro-defects, and enhances the physical and mechanical properties and performance of the tire compound, making it suitable for all-steel radial tires.
Smart Images

Figure CN118956025A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tire formulations, and in particular relates to a modified zinc oxide all-steel radial tire formulation and a preparation method thereof. Background Art
[0002] Zinc oxide is an indispensable active agent in the sulfur vulcanization system, but because soluble zinc compounds are harmful to aquatic organisms, the coexistence of zinc and lead in the mine causes zinc to always contain lead that is harmful to the human body, which has an impact on the ecological environment and human health. With the increasing awareness of environmental protection in countries around the world, it is a general trend to use low-content zinc oxide instead of ordinary zinc oxide in the rubber formula.
[0003] In recent years, low-content zinc oxide products have appeared on the market. The zinc content in low-content zinc oxide is low. Due to its smaller particle size, larger specific surface area and better affinity with rubber, it exhibits better permeability and dispersion properties during the rubber mixing process, and higher vulcanization activity during the rubber vulcanization process, thereby making the vulcanized rubber have higher tensile strength, tensile strength, elasticity and tear resistance.
[0004] In actual use, if the low-content zinc oxide is directly used to replace the traditional indirect zinc oxide in the tire airtight layer, after the tire product is replaced, during the tire driving process, the tire airtight layer will gradually separate from the rubber matrix due to stress concentration, inducing the initial failure point, and then gradually develops to cause macroscopic damage to the rubber material, seriously affecting the use of rubber products.
[0005] Through the analysis of microscopic morphological characteristics, it was found that the microscopic defects that cause fatigue failure of the tire tire airtight layer rubber material mainly include large or agglomerated zinc oxide particles when low-content zinc oxide directly replaces traditional indirect zinc oxide, and uneven dispersion of filler carbon black in the tread. Summary of the invention
[0006] The purpose of the present invention is to solve the technical problems that the microscopic defects of the tire airtight layer rubber material appear when the modified zinc oxide directly replaces the traditional indirect method zinc oxide, including large zinc oxide particles and agglomeration, uneven dispersion of filler carbon black in the tread, and thus easy fatigue damage of the rubber material.
[0007] One purpose of the present invention is to prepare a new type of modified zinc oxide to replace the traditional indirect method zinc oxide, and at the same time the modified zinc oxide can be better dispersed in the rubber material and can reduce the micro defects caused by large zinc oxide particles or agglomeration.
[0008] Another purpose of the present invention is to improve the formulation components, increase the dispersion of carbon black in the tread formulation and reduce the agglomeration of zinc oxide particles, thereby improving the physical and mechanical properties and performance of the tire formulation without affecting the vulcanization process, and is suitable for application in all-steel radial tires.
[0009] In order to achieve the above two purposes of the present invention, the present invention adopts the following technical solutions: A modified zinc oxide all-steel radial tire formula, the formula is a tire airtight layer formula, comprising the following raw materials in parts by weight: 100 parts of rubber mixture, 40-50 parts of N2 series carbon black, 3-3.5 parts of modified zinc oxide, 1 part of stearic acid, 2-4 parts of amine antioxidant, 0.5-1.5 parts of accelerator, 0.8-2 parts of sulfur, and 5 parts of others; The modified zinc oxide is a loaded zinc oxide prepared by using the rubber additive Nanoprene as a carrier, and the preparation method thereof comprises: adding the rubber additive Nanoprene to tetrahydrofuran, stirring, dissolving, filtering, and then adding anhydrous ethanol to obtain the rubber additive Nanoprene carrier, and then adding zinc acetate and sodium hydroxide in sequence to the prepared rubber additive Nanoprene carrier for reaction, washing, filtering, and drying to obtain the modified zinc oxide; The rubber mixture is a mixture of natural rubber NR and epoxidized natural rubber ENR-40 with an epoxidation degree of 40%, and the N2 series carbon black is N234 model carbon black.
[0010] In the above technical scheme, firstly, in a basic tire formula mainly composed of natural rubber, the traditional indirect zinc oxide is replaced with loaded zinc oxide (modified zinc oxide) prepared by using the rubber additive Nanoprene as a carrier. Compared with traditional zinc oxide, the loaded zinc oxide has smaller particles and can be better dispersed in the rubber compound, which can reduce the micro defects caused by the large particles of zinc oxide. In addition, the prepared loaded zinc oxide has a low zinc content, thereby achieving the purpose of reducing zinc in the tire formula.
[0011] Secondly, the specific ratio of the rubber mixture is: 10-15 parts of epoxidized natural rubber ENR-40 and 85-90 parts of natural rubber NR. Epoxidized natural rubber is prepared by partially epoxidizing the double bonds on the natural rubber molecular chain. Therefore, it can be blended with natural rubber and has the polarity of epoxy groups. It can interact with the natural rubber matrix and inorganic fillers, and has a strong interface interaction with carbon black, thereby improving the dispersion of carbon black in the tread formula, and interacting with zinc oxide particles to reduce agglomeration. It can improve the physical and mechanical properties and performance of the tire formula without affecting the vulcanization process, and is suitable for use in all-steel radial tires.
[0012] The present invention also provides a method for preparing an airtight layer of an all-steel radial tire wheel of modified zinc oxide, comprising the following contents: Firstly, a mixture of natural rubber NR and epoxy natural rubber ENR40, N2 series carbon black, modified zinc oxide, stearic acid, amine antioxidant and other materials are added in a series internal mixer in sequence; Then, the pressing weight is operated in the internal mixer; the specific process of pressing the weight is: pressing the weight for 45 seconds, lifting the pressing weight, and then pressing the weight for 60 seconds; Finally, the rubber in the internal mixer was discharged to the lower internal mixer at 150°C; the specific mixing process in the lower internal mixer was as follows: mixing at 150°C for 150 seconds, discharging the rubber to the open mixer, then tamping the rubber for 80 seconds, adding the accelerator and sulfur, mixing for 180 seconds, tamping the rubber and discharging the rubber.
[0013] The mixture of natural rubber NR and epoxy natural rubber ENR40 is added in three times. The first time, 50% of the mixture is added, and then N2 series carbon black and modified zinc oxide are added; the second time, 30% of the mixture is added, and then stearic acid, amine antioxidants and other materials are added; the third time, the remaining 20% of the mixture is added.
[0014] The mixture of natural rubber NR and epoxidized natural rubber ENR40 is added in three times, 50%, 30% and 20% at the beginning, 3 minutes and 4 minutes and 50 seconds respectively.
[0015] The mixture of natural rubber NR and epoxy natural rubber ENR40 is added three times to improve the mechanical shearing effect on zinc oxide in the internal mixer, which can make zinc oxide better dispersed in the rubber compound and improve the micro defects in the rubber compound caused by zinc oxide dispersion.
[0016] It should be noted that: because the mixing in the internal mixer is carried out in a closed space, the mechanical shear force to which the zinc oxide is subjected in the rubber is greater. In order to enable the zinc oxide to better participate in the vulcanization reaction, it is considered that if the rubber mixture, zinc oxide and carbon black are added to the internal mixer all at once, it may affect the dispersion of zinc oxide in the rubber mixture; or during the internal mixing of the rubber, the torque of the internal mixer may suddenly increase to exceed the specified value and cause shutdown due to excessive addition of filler at one time. Therefore, the present application adds the rubber mixture in three times.
[0017] In the initial stage, due to the different order of adding materials, the length of time that zinc oxide and carbon black stay in the internal mixer is different. Through the rotation of the internal mixer rotor and the extrusion and shearing between the material chambers, zinc oxide can be better dispersed in the rubber compound, and then can contact with accelerators, sulfur, etc. during vulcanization, so that it can more effectively adsorb accelerators and nitrogen bases in the rubber mixture to form complexes, thereby increasing the dispersion of zinc oxide in the rubber mixture and thus increasing the crosslinking density of the vulcanized rubber; At the beginning of the reaction (the reaction time of rubber in the normal mixing process is about 4 minutes), the main thing is to break up the rubber mixture. At this time, 50% of the rubber mixture is added. Because the speed of the internal mixer is too high, the temperature of the rubber will also be too high, which makes the heat generated by the rubber high. Under the action of heat, oxygen can easily react with the molecular chain of the rubber mixture to generate free radicals, and then the free radicals quickly undergo oxidation reaction. As a result, the main chain of the rubber molecule is broken, and the hardness and tensile stress of the rubber are reduced. Therefore, this application chooses 3 minutes to prevent the rubber mixture from oxidizing, and it is necessary to add a new 30% rubber mixture to lower the reaction temperature.
[0018] At 4 minutes and 50 seconds, the clumps of carbon black rubber will be destroyed under the action of mechanical shear force. Under the mechanical shear and the extrusion of the material chamber wall, the particle size is broken and reduced. At this time, zinc oxide is released, making the zinc oxide better dispersed in the unoxidized rubber mixture. Therefore, the remaining 20% of the rubber mixture is added at this time to enable the zinc oxide to be better dispersed in all the rubber materials.
[0019] Another reason for adding the rubber mixture at 3 minutes and 4 minutes and 50 seconds is that it is to appropriately lower the reaction temperature of the mixed rubber and reduce the oxidation reaction of the rubber mixture, which can increase the shearing effect between the rubber and other materials and achieve the purpose of reducing the aggregation of zinc oxide.
[0020] The beneficial effects of the present invention are: The invention provides a novel method for preparing modified zinc oxide. The prepared loaded zinc oxide can directly replace the traditional indirect method zinc oxide. At the same time, the modified zinc oxide can be better dispersed in the rubber material, and the microscopic defects caused by large zinc oxide particles or agglomeration can be reduced.
[0021] Adding a certain amount of epoxidized natural rubber to natural rubber interacts with carbon black to improve the dispersion of carbon black in the airtight layer formula; it reacts with zinc oxide particles to reduce agglomeration, promotes the dispersion of zinc oxide in the rubber compound, and improves the microscopic defects in the rubber compound caused by zinc oxide agglomeration.
[0022] The mixture of natural rubber NR and epoxy natural rubber ENR40 is added three times to improve the mechanical shearing effect on zinc oxide in the internal mixer, which can make zinc oxide better dispersed in the rubber compound and reduce micro defects caused by large zinc oxide particles or agglomeration. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 For the 1# formulation and 2# formulation rubber mix in the embodiment - strain curve; Figure 2 For the 3# and 4# formula rubber mixes in the embodiment -Strain curve. DETAILED DESCRIPTION
[0024] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0025] The natural rubber (NR) used in the present invention can be selected from commercially available standard rubbers known to those skilled in the art. The carbon black used in the present invention is commercially available super wear-resistant carbon black N234 known to those skilled in the art. Other reagents are all commercially available industrial-grade reagents.
[0026] Example 1: 1# formula, basic formula (parts by weight): epoxy natural rubber ENR-40: 10, natural rubber NR: 90, N234 model carbon black: 45, indirect zinc oxide: 3.5, stearic acid: 1, amine antioxidant: 2.5, sulfur and accelerator each: 1.5, others: 5.
[0027] Formula 2# (experimental formula): An equal amount of loaded zinc oxide prepared by using rubber additive Nanoprene as a carrier is used to replace the indirect method zinc oxide. The other components and amounts are the same as those of Formula 1#.
[0028] The modified zinc oxide is a loaded zinc oxide prepared by using the rubber additive Nanoprene as a carrier, and the preparation method thereof comprises: cutting 100g of the rubber additive Nanoprene into small particles, adding tetrahydrofuran, stirring, dissolving for 48h, filtering, and then adding 150ml of anhydrous ethanol to obtain the rubber additive Nanoprene carrier, and then adding 20ml of zinc acetate and 30ml of sodium hydroxide in sequence to the prepared rubber additive Nanoprene carrier for reaction for 1h, washing, filtering, and drying to obtain the modified zinc oxide.
[0029] Example 2: 3# formula, basic formula (parts by weight): epoxy natural rubber ENR-40: 15, natural rubber NR: 85, N234 type carbon black: 50, indirect zinc oxide: 3.5, stearic acid: 1, amine antioxidant: 3, sulfur 1.8, accelerator: 1, others: 5.
[0030] Formula 4# (experimental formula): An equal amount of loaded zinc oxide prepared by using rubber additive Nanoprene as carrier replaces indirect zinc oxide, and the remaining components and amounts are the same as those of Formula 3#.
[0031] The modified zinc oxide is a loaded zinc oxide prepared by using the rubber additive Nanoprene as a carrier, and the preparation method thereof comprises: cutting 100g of the rubber additive Nanoprene into small particles, adding tetrahydrofuran, stirring, dissolving for 48h, filtering, and then adding 150ml of anhydrous ethanol to obtain the rubber additive Nanoprene carrier, and then adding 20ml of zinc acetate and 30ml of sodium hydroxide in sequence to the prepared rubber additive Nanoprene carrier for reaction for 1h, washing, filtering, and drying to obtain the modified zinc oxide.
[0032] Main equipment and instruments: GK320 / GK550E tandem internal mixer, a product of Germany's HF company; XKJ-480 open mixer, a product of Dalian Rubber and Plastic Machinery Co., Ltd.; GK400 internal mixer, a product of Yiyang Rubber and Plastic Machinery Group Co., Ltd.; HS100T-FTMO-90 flat plate vulcanizer, a product of Jiaxin Electronic Equipment Technology (Shenzhen) Co., Ltd.; MDR2000 rotorless vulcanizer, etc.
[0033] Preparation process: Mixing process of formulations 1# and 2# in Example 1: First, add a mixture of natural rubber NR and epoxy natural rubber ENR40, N234 carbon black, indirect zinc oxide (formula 1#) or modified zinc oxide (formula 2#), stearic acid, amine antioxidants and other materials in a series internal mixer in sequence, and then operate the pressing weight in the internal mixer: the specific process is to press the pressing weight for 45 seconds, lift the pressing weight, and then press the pressing weight for 60 seconds, and finally discharge the rubber in the internal mixer to the lower internal mixer at a temperature of 150°C. The specific rubber mixing process in the lower internal mixer is: mixing at 150°C for 150 seconds, discharging the rubber to the open mixer, then pounding the rubber for 80 seconds, adding accelerator and sulfur, and finally mixing for 180 seconds, pounding the rubber, and discharging the rubber.
[0034] Among them, the mixture of natural rubber NR and epoxy natural rubber ENR40 described in the test formula (formula 2#) was added three times. In the first addition, 50% of the mixture was added, and then N234 carbon black and modified zinc oxide were added; in the second addition, 30% of the mixture was added, and then stearic acid, amine antioxidants and other materials were added; in the third addition, the remaining 20% of the mixture was added.
[0035] The mixture of natural rubber NR and epoxidized natural rubber ENR40 is added in three times, 50%, 30% and 20% at the beginning, 3 minutes and 4 minutes and 50 seconds respectively.
[0036] Mixing process of formulations 3# and 4# in Example 2: First, add a mixture of natural rubber NR and epoxy natural rubber ENR40, N234 carbon black, indirect zinc oxide (3# formulation) or modified zinc oxide (4# formulation), stearic acid, amine antioxidants and other materials in the series internal mixer in sequence, and then operate the pressing weight in the internal mixer: the specific process is to press the pressing weight for 45 seconds, lift the pressing weight, and then press the pressing weight for 60 seconds, and finally discharge the rubber in the internal mixer to the lower internal mixer at a temperature of 150°C. The specific rubber mixing process in the lower internal mixer is: mixing at 150°C for 150 seconds, discharging the rubber to the open mixer, and then tamping the rubber for 80 seconds, adding accelerators and sulfur, and finally mixing for 180 seconds, tamping the rubber, and discharging the rubber.
[0037] The difference between the mixing process in Example 2 and Example 1 is that the mixture of natural rubber NR and epoxidized natural rubber ENR40 in the test formula (formulation #4) is added at one time.
[0038] The physical properties of different formula vulcanized rubber are shown in Table 1 Table 1 Physical properties of vulcanized rubber
[0039] As can be seen from Table 1, compared with the basic formula 1# and 3# vulcanized rubber, the hardness, tensile stress and tensile strength of the test formula 2# and 4# vulcanized rubber replaced in equal amounts are comparable. Since the zinc content of the equal replacement is low and the physical property test results of the vulcanized rubber are comparable, it shows that the zinc ions in the loaded zinc oxide prepared by the rubber additive Nanoprene as a carrier have a higher reaction efficiency, and the actual zinc oxide content in the rubber compound that participates in the reaction can reach the same level as the total amount of zinc oxide in the indirect method, so the remaining zinc ions that do not participate in the reaction are less (if there are too many remaining zinc ions, the physical property test results of the vulcanized rubber will be poor), thereby improving the environmental protection of the test formula rubber compound, and the addition of the loaded zinc oxide prepared by the rubber additive Nanoprene as a carrier has no effect on the physical properties of the rubber compound.
[0040] like Figure 1 and Figure 2 As shown, the compound The (storage modulus)-strain curve is one of the important indicators of the dynamic mechanical properties of rubber materials. It describes the relationship between the storage modulus and strain of the compound rubber under continuous sinusoidal shear strain. The change reflects the change of the microstructure of the mixed rubber and the interaction between the filler and the rubber matrix. Curves 1 to 4 in the figure correspond to the mixed rubber of formulation 1#, formulation 2#, formulation 3#, and formulation 4# in Example (Storage modulus)-strain curve.
[0041] Compound With low strain amplitude max and high strain amplitude The difference between min and min can be used to characterize the Payne effect. Specifically, when the strain is greater than 1%, the will decrease significantly, and The size of can reflect the dispersion of filler in rubber matrix. For example, if If is small, the Payne effect is not significant, which means that the filler is well dispersed; on the contrary, if Larger values may indicate that the filler dispersion is not ideal.
[0042] Based on the above curve description, Figure 1 and Figure 2 It can be seen that the Payne effect of the rubber compound is weakened when the 1# formula is replaced by the 2# formula in equal amounts, and the Payne effect of the rubber compound is weakened when the 3# formula is replaced by the 4# formula in equal amounts, indicating that the dispersion of fillers in the 2# and 4# formula rubber compounds is better.
[0043] Because the zinc oxide in formula 1# and formula 3# is replaced by the same amount of formula 2# and formula 4#, the dispersion of fillers in the compound is better, indicating that more zinc participates in the reaction, so there are fewer zinc ions remaining that do not participate in the reaction (if there are more zinc ions remaining, the dispersion of fillers in the compound will be worse, and the corresponding Figure 1 and Figure 2 that is will be larger).
[0044] Compared with the 1# and 3# formula rubber mixes, the filler dispersion in the 2# and 4# formula rubber mixes is better because: first, the loaded zinc oxide can directly replace the traditional indirect zinc oxide, and the modified zinc oxide can be better dispersed in the rubber, which can reduce the micro defects caused by large zinc oxide particles or agglomeration; second, the carbon black in the formula interacts with ENR40, thereby promoting the dispersion of carbon black in the rubber, and at the same time, ENR40 interacts with zinc oxide particles, reducing agglomeration and promoting the dispersion of zinc oxide in the rubber; Compared with the 4# formula rubber mix, the dispersion of fillers in the 2# formula rubber mix is better. This is because: the mixture of natural rubber NR and ENR40 in the 2# formula rubber mix is added in three times, which improves the mechanical shearing effect on zinc oxide and reduces the micro defects caused by large zinc oxide particles or agglomeration.
Claims
1. A modified zinc oxide all-steel radial tire formula, characterized in that: The formula is a formula for a tire airtight layer, comprising the following raw materials in parts by weight: 100 parts of a rubber mixture, 40-50 parts of N2 series carbon black, 3-3.5 parts of modified zinc oxide, 1 part of stearic acid, 2-4 parts of an amine antioxidant, 0.5-1.5 parts of an accelerator, 0.8-2 parts of sulfur, and 5 parts of others; The modified zinc oxide is a loaded zinc oxide prepared by using the rubber additive Nanoprene as a carrier, and the preparation method thereof comprises: adding the rubber additive Nanoprene to tetrahydrofuran, stirring, dissolving, filtering, and then adding anhydrous ethanol to obtain the rubber additive Nanoprene carrier, and then adding zinc acetate and sodium hydroxide in sequence to the prepared rubber additive Nanoprene carrier for reaction, washing, filtering, and drying to obtain the modified zinc oxide; The rubber mixture is a mixture of natural rubber NR and epoxidized natural rubber ENR-40 with an epoxidation degree of 40%, and the N2 series carbon black is N234 model carbon black.
2. A modified zinc oxide all-steel radial tire formulation as claimed in claim 1, characterized in that: The specific ratio of the rubber mixture is: 10-15 parts of epoxy natural rubber ENR-40 and 85-90 parts of natural rubber NR.
3. A method for preparing a modified zinc oxide all-steel radial tire formulation as claimed in claim 1 or 2, characterized in that: Includes the following: Firstly, a mixture of natural rubber NR and epoxy natural rubber ENR40, N2 series carbon black, modified zinc oxide, stearic acid, amine antioxidant and other materials are added in a series internal mixer in sequence; Then, the pressing weight is operated in the internal mixer; the specific process of pressing the weight is: pressing the weight for 45 seconds, lifting the pressing weight, and then pressing the weight for 60 seconds; Finally, the rubber in the internal mixer was discharged to the lower internal mixer at a temperature of 150°C; the specific mixing process in the lower internal mixer was as follows: mixing at 150°C for 150 seconds, discharging the rubber to the open mixer, then tamping the rubber for 80 seconds, adding accelerator and sulfur, mixing for 180 seconds, tamping the rubber and discharging the rubber.
4. The method for preparing a modified zinc oxide all-steel radial tire formulation as claimed in claim 3, characterized in that: The mixture of natural rubber NR and epoxy natural rubber ENR40 is added in three times. The first time, 50% of the mixture is added, and then N2 series carbon black and modified zinc oxide are added; the second time, 30% of the mixture is added, and then stearic acid, amine antioxidants and other materials are added; the third time, the remaining 20% of the mixture is added.
5. The method for preparing a modified zinc oxide all-steel radial tire formulation as claimed in claim 4, characterized in that: The mixture of natural rubber NR and epoxidized natural rubber ENR40 was added in three times, 50%, 30% and 20% at the beginning, 3 minutes and 4 minutes and 50 seconds respectively.
Citation Information
Patent Citations
Method for preparing cladded modified zinc oxide
CN108456329A
Preparation method of wet-process zinc oxide pre-dispersion master batch
CN110028708A
Mercapto-group-containing curable rubber composition
JP1999012467A
Rubber composition for use in tires, and pneumatic tire
US20130296477A1