Lignin asphalt modifier as well as one-step preparation method and application thereof
By using melt blending technology of lignin with polyethylene and ethylene-octene copolymers, a simple process and low-cost lignin asphalt modifier was prepared, which solved the high-temperature resistance of existing asphalt modifiers The problem of insufficient rut and low-temperature elastic performance has achieved the long-term stability and environmental protection of asphalt pavement.
Patent Information
- Application Number
- CN202411172517.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The existing asphalt modifiers have shortcomings in improving the high-temperature rutting resistance and low-temperature elasticity of asphalt pavement, and the process is complex and costly, making it difficult to meet the long-term use needs of highways and other roads.
Using lignin as a modifier, a kind of lignin is prepared by melt blending with materials such as polyethylene and ethylene-octene copolymer and adding an appropriate amount of additives to improve the compatibility and cross-linking network of lignin with polymers. Simple process, low-cost lignin asphalt modifier.
It significantly improves the high-temperature rutting resistance and low-temperature elasticity of asphalt pavement, extends the service life, reduces production costs and equipment requirements, simplifies the preparation and construction process, and has the advantages of environmental protection and resource recycling.
Smart Images

Figure BDA0005009717980000101
Abstract
Description
Technical Field
[0001] The invention belongs to the field of asphalt modification preparation, and specifically relates to a lignin asphalt modifier and a one-step preparation method and application thereof. Background Art
[0002] Asphalt pavement is the pavement form of my country's expressways and main roads, with the advantages of comfortable driving, low noise and easy maintenance. In recent years, my country's expressway system and other road traffic networks have been rapidly built, and the demand for asphalt pavement paving materials has increased greatly. With the increase in freight logistics volume, the service life and load of asphalt pavement have increased. The heat generated by the friction between vehicle tires and the road surface causes the road surface temperature to rise. In addition, asphalt pavement is subjected to high and low temperature climate changes all year round, making asphalt pavement prone to high temperature rutting, low temperature cracking, easy aging and other problems, affecting the service life of asphalt pavement. Ordinary asphalt is difficult to meet the requirements of road use. Therefore, it is generally necessary to add modifiers to asphalt pavement materials to solve the above problems. There are many types of asphalt modifiers. At present, the main modifiers are SBS (styrene-butadiene-styrene triblock copolymer), rubber, polyolefins and other categories.
[0003] SBS modified asphalt is a physical mixture of SBS particles and asphalt to improve the high and low temperature performance of asphalt. At present, SBS modifier has become the mainstream asphalt modifier because of its advantages such as high and low temperature performance and good application effect. However, there are double bonds in the molecular structure of SBS, which are easily destroyed and oxidized, resulting in poor anti-aging performance, weak high-temperature rutting resistance of asphalt pavement, and short life. This fundamental problem in the molecular structure is difficult to improve through other technologies; in addition, the composition and structure of SBS particles and matrix asphalt are very different, and segregation is easy to occur, which requires the addition of additives to improve. The existing technology generally adds sulfur to cross-link SBS with asphalt to improve the stability of the system. However, the addition of sulfur can easily cause cross-linking reactions between SBS, asphalt and sulfur, which reduces the mechanical properties of modified asphalt. Patent 202311642790.9 proposes an SBS asphalt modifier that slowly releases crosslinking agent active sulfur, introducing an additive compounded from cellulose acetate, diluent, porogen, sulfur, vulcanizer, activator and curing agent to prevent violent polymerization and improve system stability, but the formula is complex. SBS modified asphalt needs to go through pre-swelling, grinding, development and other processes, and the use process is complicated. The problems of poor high temperature rutting resistance and short life have not been effectively solved.
[0004] Rubber-modified asphalt generally uses rubber powder or rubber powder from waste tires to improve the low-temperature brittleness, cracking and ductility of the base asphalt. The sulfur content of rubber powder prepared from waste tires is too high and needs to be desulfurized. The high-temperature resistance of the rubber powder after desulfurization decreases; at the same time, in the application of rubber-modified asphalt, there are problems such as poor compatibility between rubber and base asphalt, easy sedimentation of rubber powder particles from the blended asphalt mixture, and poor storage stability. Patent 202311102440.3 invented a device for high-dosage rubber-modified asphalt to solve the problem that high-dosage rubber-modified asphalt is difficult to prepare and prone to segregation, but it failed to improve the high-temperature rutting resistance.
[0005] Polyolefin modified asphalt is generally modified by adding one or more of polyethylene, polypropylene, polyolefin elastomer, etc. to the base asphalt. Asphalt modified with waste plastics PE and PP improves the viscosity and stiffness modulus of asphalt mixture, and improves anti-rutting performance, but its anti-rutting effect on heavy-load sections is limited, and high modulus will lead to a decrease in low-temperature crack resistance. Polyolefin modified asphalt also has poor compatibility with asphalt, resulting in easy segregation and poor thermal storage stability; low-temperature brittleness, low elastic recovery and other disadvantages. Patent ZL02133489.7 mixes polyethylene, polyolefin elastomer and modifier, and melt blends with asphalt to prepare modified asphalt masterbatch for modified base asphalt; the results of the embodiment show that the needle penetration is less than 40 (0.1mm), which is less than the national standard GB / T15180 index 41-60 (0.1mm), and the softening point is greater than 70°C, which is slightly higher than the national standard GB / T15180 (45-55°C). Patent 202310394824.0 uses waste plastics and waste rubber powder as raw materials to prepare a composite modifier, the main components of which are 30-60 parts of waste plastics, 20-30 parts of waste rubber powder, 5-10 parts of styrene-butadiene-styrene block copolymer (SBS), antioxidants, lubricants, inorganic materials, etc., which are used to improve the performance of asphalt. The examples show that the needle penetration is low and the softening point is improved. Patent 201710089546.2 invented a method of producing asphalt modifiers using waste polyvinyl chloride mulch, which makes use of waste resources and improves the stability of asphalt, but its raw materials and production process are complicated. Patent 202111506729.2 uses ethylene through cyclohexane, methylaluminoxane, catalysts, etc. to produce terminal amino polyethylene through multi-step reactions, which is used as an asphalt modifier to overcome the problem of poor stability of PE asphalt modifiers. The process is complicated and the cost is increased. The above technologies show that the use of polyolefin modified asphalt can reduce the penetration of the base asphalt and increase the softening point, but it does not improve the high-temperature thermal storage stability, anti-aging performance, and low-temperature anti-brittle cracking performance.
[0006] With the implementation of environmental protection concepts and the advancement of the "dual carbon" goals, the environmental protection and functionalization of asphalt modifiers will become a new trend. The application of biomass materials in asphalt modifiers will further promote its green development. Lignin comes from natural plants, while industrial lignin mainly comes from the pulp and paper industry. Lignin has a three-dimensional network structure and has natural anti-ultraviolet and anti-aging functions. It can play an anti-aging and weathering function when used in materials. Some technicians use lignin as a modifier component to modify asphalt. Patent 201810490946.9 uses soluble lignin, insoluble lignin, residual oil and / or vegetable oil mixed in a certain mass ratio to make a lignin asphalt modifier. The lignin is lignin obtained by pretreatment of biomass raw materials, enzymatic hydrolysis, saccharification and fermentation, biological degradation and oil extraction; the embodiment shows that the modifier can improve the ductility and softening point of asphalt. Patent 201811022852.5 copolymerizes lignin with hydrogenated waste cooking oil, adds styrene-butadiene rubber and adjuvants to obtain a lignin hydrogenated oil copolymer asphalt modifier. The results of the embodiments show that the needle penetration, elongation and softening point performance of the modifier are comparable to those of traditional modified asphalts such as SBS and SBR. Patent 202111102820.8 invented an asphalt modifier containing diatomaceous earth, maleic anhydride-benzyl methacrylate copolymer, phenolic epoxy vinyl ester resin, ethylene-vinyl acetate copolymer, enzymatic lignin-sulfonated acetone-formaldehyde condensation product, sodium dodecyl sulfate, stearic acid, etc., wherein the enzymatic lignin-sulfonated acetone-formaldehyde condensation product is obtained by multi-step chemical reaction of sodium bisulfite, sodium metabisulfite, acetone, formaldehyde and enzymatic lignin / alkali lignin. The lignin acquisition process route in the above patents is cumbersome and costly. Patent 201310388313.4 invented an asphalt modifier containing polyethylene, waste rubber powder, and bio-based filler, wherein the bio-based filler is a filler powder composed of lignin organic matter and silicate inorganic matter, which is used to improve the low temperature resistance of asphalt, but the high temperature anti-rutting performance is not improved. Patent 201410542014.6 invented an asphalt modifier containing low-density polyethylene and bio-based filler, wherein the bio-based filler is an organic modified clay prepared by acid precipitation, flocculation precipitation, ball milling, and drying of papermaking black liquor and montmorillonite. This patent solution can improve the softening point of asphalt and improve the dynamic stability, but it does not improve the low-temperature brittleness of asphalt.
[0007] Based on the above problems of asphalt modifiers and the advantages of lignin, it is necessary to research and develop lignin-based asphalt modifiers, so as to provide a low-cost, natural lignin asphalt modifier that can improve asphalt's resistance to high-temperature rutting, low-temperature elasticity and weather resistance. Summary of the invention
[0008] In order to solve the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a lignin asphalt modifier.
[0009] Another object of the present invention is to provide a method for preparing the above-mentioned lignin asphalt modifier.
[0010] Another object of the present invention is to provide an application of the above-mentioned lignin asphalt modifier.
[0011] The purpose of the present invention is achieved through the following technical solutions:
[0012] A lignin asphalt modifier is prepared by comprising the following components, measured by weight: 50-95 parts of polyethylene, 0.1-30 parts of lignin, 0.5-49 parts of ethylene-octene copolymer (polyolefin elastomer), 0-10 parts of additive A, 0-10 parts of additive B, 0-10 parts of additive C, and 0-10 parts of additive D, wherein the contents of additives A, B, C, and D are not all zero.
[0013] Preferably, the lignin asphalt modifier is prepared by including the following components in parts by mass: 50-95 parts of polyethylene, 1-20 parts of lignin, 4-30 parts of ethylene-octene copolymer (polyolefin elastomer), 0.5-5 parts of additive A, 0.5-5 parts of additive B, 0.5-5 parts of additive C, and 0.5-5 parts of additive D.
[0014] The polyethylene is new polyethylene or recycled polyethylene, or a mixture of the two; the recycled polyethylene does not contain metal, fiber and other impurities.
[0015] More preferably, the polyethylene is linear low density polyethylene.
[0016] Preferably, the lignin is industrial lignin powder, which is at least one of alkali lignin and enzymatic lignin, and has a particle size distribution of D50 less than 5 μm.
[0017] Preferably, the additive A is maleic anhydride, which is used to modify polyolefin elastomers, and the obtained maleic anhydride grafted ethylene-octene copolymer is used to further modify lignin.
[0018] Preferably, the additive B is at least one of 3-amino-1,2,4-triazole, 1,2,4-triazole and imidazole, which is used to further modify the maleic anhydride grafted ethylene-octene copolymer.
[0019] Preferably, the additive C is at least one of zinc chloride, ferric chloride, zinc acetate and zinc stearate, which is used to enhance the interaction between lignin and polyethylene and maleic anhydride grafted ethylene-octene copolymer.
[0020] Preferably, the additive D is at least one of rosin ester and rosin ester-modified compound, which is used to improve the interfacial compatibility between lignin and polyethylene.
[0021] Preferably, the lignin asphalt modifier further includes color powder, in an amount of 0-10 parts by mass.
[0022] More preferably, the toner is carbon black.
[0023] More preferably, the color powder is 0.2-1 part.
[0024] The preparation method of the above-mentioned lignin asphalt modifier comprises the following steps:
[0025] Polyethylene, lignin, ethylene-octene copolymer (polyolefin elastomer), additive A, additive B, additive C, additive D, or polyethylene, lignin, ethylene-octene copolymer (polyolefin elastomer), additive A, additive B, additive C, additive D, and color powder are uniformly mixed in a mixer, added into a twin-screw extruder for melt blending, and extruded into granules to obtain a lignin asphalt modifier.
[0026] Preferably, the mixing time in the mixer is 1-5 min, and the rotation speed is 200-2000 r / min.
[0027] Preferably, the temperature of the melt blending is 150-190° C., the screw speed is 50-200 r / min, and the vacuum degree is 0-(-0.08) MPa.
[0028] The above-mentioned application of a lignin asphalt modifier in asphalt.
[0029] Preferably, the application comprises, by weight, 0.1-10 parts of the above-mentioned lignin asphalt modifier and 90-99.9 parts of base asphalt.
[0030] More preferably, the application comprises 0.5-7 parts of the above-mentioned lignin asphalt modifier and 93-99.5 parts of base asphalt, calculated by weight.
[0031] Preferably, the specific method of the application is: heating the base asphalt to 120-200°C, adding the above-mentioned lignin asphalt modifier and mixing evenly to obtain an asphalt composition for construction.
[0032] More preferably, the uniform mixing speed is 2000-5000 r / min, and the stirring time is 2-10 min.
[0033] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0034] (1) The lignin asphalt modifier provided by the present invention has a simple preparation process, low requirements on equipment, uses biomass materials, and can use recycled waste polyethylene as raw materials, which reduces costs, and can promote the recycling of resources, improve resource utilization, and has environmental significance. The lignin asphalt modifier prepared by the present invention is a dry granular material, which can be directly added to the base asphalt later, is easy to operate, and is easy to be constructed on site.
[0035] (2) The addition of lignin in the present invention can provide support for the matrix asphalt by utilizing its three-dimensional network structure, enhance the hardness of the asphalt material, and improve the high-temperature anti-rutting performance; and lignin has good anti-ultraviolet and anti-aging properties, and can be used as an antioxidant in asphalt to delay road aging and extend the service life of the asphalt pavement. The added polyolefin elastomer and additive A are melt-blended and in-situ grafted and modified, and additive B is further melt-modified and in-situ modified with it; as an interface modifier of lignin, the compatibility of lignin in asphalt can be improved, and the stability of asphalt materials can be improved; at the same time, the polyolefin elastomer can provide low-temperature ductility for the asphalt pavement and reduce the low-temperature brittleness of asphalt. Additive C acts as an interface modifier to form an interface coordination bond between lignin and the polymer, strengthen the interaction between lignin and the polymer, and further improve the compatibility of lignin in asphalt. Additive D is an auxiliary interface modifier, which improves the interaction between the polymer and sand and gravel, and assists in improving the compatibility of lignin and asphalt. The lignin asphalt modifier prepared from the above raw materials constructs a synergistic coordination cross-linking network, which can provide a skeleton support for the asphalt material and produce excellent high and low temperature resistance. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.
[0037] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. All raw materials, reagents, etc., whose manufacturers are not specified, are conventional products that can be purchased commercially.
[0038] The parts mentioned in the embodiments and comparative examples of the present invention are parts by mass, and the parts can be enlarged or reduced in the same proportion.
[0039] Example 1
[0040] 95 parts of polyethylene (Guangzhou Petrochemical M2320), 1 part of alkali lignin powder (D50 less than 5 μm), 4 parts of polyolefin elastomer (Dow Chemical 8150), 0.5 parts of maleic anhydride, 0.5 parts of 3-amino-1,2,4-triazole, 0.5 parts of zinc chloride, and 0.5 parts of rosin ester were mixed in a mixer for 2 minutes at a speed of 500 r / min.
[0041] The obtained mixture is added into a twin-screw extruder for melting, shear blending and melting into one; the melt blending temperature is 180°C, the screw speed is 50r / min, and the vacuum degree is -0.05MPa; the molten blend is extruded into strands through an extrusion port, and the lignin asphalt modifier is prepared by water cooling, air drying and pelletizing.
[0042] Add 0.5 parts of the lignin asphalt modifier prepared above to 99.5 parts of molten base asphalt at a melting temperature of 185°C, stir evenly at a rotation speed of 4000 r / min and a stirring time of 5 minutes; then an asphalt composition for construction can be obtained.
[0043] Example 2
[0044] 95 parts of polyethylene (Guangzhou Petrochemical M2320), 1 part of alkali lignin powder (D50 less than 5 μm), 4 parts of polyolefin elastomer (Dow Chemical 8150), 0.5 parts of maleic anhydride, 0.5 parts of 3-amino-1,2,4-triazole, 0.5 parts of zinc chloride, and 0.5 parts of rosin ester were mixed in a mixer for 2 minutes at a speed of 500 r / min.
[0045] The obtained mixture is added into a twin-screw extruder for melting, shear blending and melting into one; the melt blending temperature is 180°C, the screw speed is 50r / min, and the vacuum degree is -0.05MPa; the molten blend is extruded into strands through an extrusion port, and the lignin asphalt modifier is prepared by water cooling, air drying and pelletizing.
[0046] Add the 7 parts of lignin asphalt modifier prepared above to 93 parts of molten base asphalt at a melting temperature of 185°C, stir evenly at a rotation speed of 4000r / min and a stirring time of 5min; then an asphalt composition for construction can be obtained.
[0047] Example 3
[0048] Mix 50 parts of polyethylene (Guangzhou Petrochemical M2320), 20 parts of alkali lignin powder (D50 less than 5 μm), 30 parts of polyolefin elastomer (Dow Chemical 8150), 5 parts of maleic anhydride, 5 parts of 3-amino-1,2,4-triazole, 5 parts of zinc chloride, and 5 parts of rosin ester in a mixer for 2 minutes at a speed of 500 r / min.
[0049] The obtained mixture is added into a twin-screw extruder for melting, shear blending and melting into one; the melt blending temperature is 180°C, the screw speed is 50r / min, and the vacuum degree is -0.05MPa; the molten blend is extruded into strands through an extrusion port, and the lignin asphalt modifier is prepared by water cooling, air drying and pelletizing.
[0050] Add 0.5 parts of the lignin asphalt modifier prepared above to 99.5 parts of molten base asphalt at a melting temperature of 185°C, stir evenly at a rotation speed of 4000 r / min and a stirring time of 5 minutes; then an asphalt composition for construction can be obtained.
[0051] Example 4
[0052] Mix 50 parts of polyethylene (Guangzhou Petrochemical M2320), 20 parts of alkali lignin powder (D50 less than 5 μm), 30 parts of polyolefin elastomer (Dow Chemical 8150), 5 parts of maleic anhydride, 5 parts of 3-amino-1,2,4-triazole, 5 parts of zinc chloride, and 5 parts of rosin ester in a mixer for 2 minutes at a speed of 500 r / min.
[0053] The obtained mixture is added into a twin-screw extruder for melting, shear blending and melting into one; the melt blending temperature is 180°C, the screw speed is 50r / min, and the vacuum degree is -0.05MPa; the molten blend is extruded into strands through an extrusion port, and the lignin asphalt modifier is prepared by water cooling, air drying and pelletizing.
[0054] Add the 7 parts of lignin asphalt modifier prepared above to 93 parts of molten base asphalt at a melting temperature of 185°C, stir evenly at a rotation speed of 4000r / min and a stirring time of 5min; then an asphalt composition for construction can be obtained.
[0055] Example 5
[0056] 70 parts of polyethylene (Guangzhou Petrochemical M2320), 10 parts of alkali lignin powder (D50 less than 5 μm), 20 parts of polyolefin elastomer (Dow Chemical 8150), 2.5 parts of maleic anhydride, 2.5 parts of 3-amino-1,2,4-triazole, 2.5 parts of zinc chloride, and 2.5 parts of rosin ester were mixed in a mixer for 2 minutes at a speed of 500 r / min.
[0057] The obtained mixture is added into a twin-screw extruder for melting, shear blending and melting into one; the melt blending temperature is 180°C, the screw speed is 50r / min, and the vacuum degree is -0.05MPa; the molten blend is extruded into strands through an extrusion port, and the lignin asphalt modifier is prepared by water cooling, air drying and pelletizing.
[0058] Add 3.5 parts of the lignin asphalt modifier prepared above to 96.5 parts of molten base asphalt at a melting temperature of 185°C, stir evenly at a rotation speed of 4000 r / min and a stirring time of 5 minutes; then an asphalt composition for construction can be obtained.
[0059] Example 6
[0060] 95 parts of polyethylene (Guangzhou Petrochemical M2320), 1 part of alkali lignin powder (D50 less than 5 μm), 4 parts of polyolefin elastomer (Dow Chemical 8150), 0.5 parts of maleic anhydride, 0.5 parts of 3-amino-1,2,4-triazole, 0.5 parts of zinc chloride, 0.5 parts of rosin ester and 0.5 parts of carbon black (N330) were mixed in a mixer for 2 minutes at a speed of 500 r / min.
[0061] The obtained mixture is added into a twin-screw extruder for melting, shear blending and melting into one; the melt blending temperature is 180°C, the screw speed is 50r / min, and the vacuum degree is -0.05MPa; the molten blend is extruded into strands through an extrusion port, and the lignin asphalt modifier is prepared by water cooling, air drying and pelletizing.
[0062] Add 0.5 parts of the lignin asphalt modifier prepared above to 99.5 parts of molten base asphalt at a melting temperature of 185°C, stir evenly at a rotation speed of 4000 r / min and a stirring time of 5 minutes; then an asphalt composition for construction can be obtained.
[0063] Comparative Example 1
[0064] 95 parts of polyethylene (Guangzhou Petrochemical M2320), 4 parts of polyolefin elastomer (Dow Chemical 8150), 0.5 parts of maleic anhydride, 0.5 parts of 3-amino-1,2,4-triazole, 0.5 parts of zinc chloride, and 0.5 parts of rosin ester were mixed in a mixer for 2 minutes at a speed of 500 r / min.
[0065] The obtained mixture is added into a twin-screw extruder for melting, shear blending and melting into one; the melt blending temperature is 180°C, the screw speed is 50r / min, and the vacuum degree is -0.05MPa; the molten blend is extruded into strips through the extrusion port, and the lignin-free asphalt modifier is prepared by water cooling, air drying and pelletizing.
[0066] Add 0.5 parts of the lignin asphalt modifier prepared above to 99.5 parts of molten base asphalt at a melting temperature of 185°C, stir evenly at a rotation speed of 4000 r / min and a stirring time of 5 minutes; then an asphalt composition for construction can be obtained.
[0067] Comparative Example 2
[0068] 95 parts of polyethylene (Guangzhou Petrochemical M2320), 1 part of alkali lignin powder (D50 less than 5 μm), and 4 parts of polyolefin elastomer (Dow Chemical 8150) were mixed in a mixer for 2 minutes at a speed of 500 r / min.
[0069] The obtained mixture is added into a twin-screw extruder for melting, shear blending and melting into one; the melt blending temperature is 180°C, the screw speed is 50r / min, and the vacuum degree is -0.05MPa; the molten blend is extruded into strips through an extrusion port, and a lignin asphalt modifier without interface modification is prepared by water cooling, air drying and pelletizing.
[0070] Add 0.5 parts of the lignin asphalt modifier prepared above to 99.5 parts of molten base asphalt at a melting temperature of 185°C, stir evenly at a rotation speed of 4000 r / min and a stirring time of 5 minutes; then an asphalt composition for construction can be obtained.
[0071] The asphalt used in the comparative example is No. 70 road petroleum asphalt, and the oil-stone ratio is 4.3wt%; the mass proportion of crushed stone is: 10-20mm crushed stone: 10-15mm crushed stone: 5-10mm crushed stone: 0-3mm stone chips: mineral powder = 33:11:28:27:1.
[0072] The test methods for dynamic stability, penetration, softening point, etc. in rutting tests refer to the Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering JTG E 20-2011. The specific data are shown in Table 1.
[0073]
[0074] It can be seen from the data in Table 1 that the lignin asphalt modifier prepared by the present invention is used for modified asphalt pavement, and its high temperature rutting resistance far exceeds the latest standard of 5000 times / mm; the needle penetration is lower than that of patents 202410417728.8, 202310394824.0, 201310388313.4, 201810490946.9, and 201811022852.5, and the softening point is higher than that of patents 202410417728.8, 202310394824.0, 201810490946.9, and 201811022852.5; the needle penetration decreases and the softening point increases, indicating that the plasticity and shear resistance increase, and the high temperature stability improves; it indicates that the asphalt modifier prepared by the present invention has good improvement in the high temperature and low temperature resistance of asphalt, and has good comprehensive performance. In the asphalt mixing process, the lignin asphalt modifier is directly added, which greatly saves the time and construction difficulty of mixing with asphalt, reduces energy consumption, does not produce dust pollution, and the system does not have segregation phenomenon. The present invention realizes the application of biomass material-lignin and waste recycled plastics.
[0075] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A lignin asphalt modifier, characterized in that: The invention is prepared by including the following components in parts by mass: 50-95 parts of polyethylene, 0.1-30 parts of lignin, 0.5-49 parts of ethylene-octene copolymer, 0-10 parts of additive A, 0-10 parts of additive B, 0-10 parts of additive C, and 0-10 parts of additive D, wherein the additives A, B, C, and D are not zero.
2. A lignin asphalt modifier according to claim 1, characterized in that: The invention comprises the following components by weight: 50-95 parts of polyethylene, 1-20 parts of lignin, 4-30 parts of ethylene-octene copolymer, 0.5-5 parts of additive A, 0.5-5 parts of additive B, 0.5-5 parts of additive C and 0.5-5 parts of additive D.
3. A lignin asphalt modifier according to claim 1 or 2, characterized in that: The lignin is at least one of alkali lignin and enzymatic lignin, and the particle size distribution is D50 less than 5 μm.
4. A lignin asphalt modifier according to claim 1 or 2, characterized in that: The polyethylene is a linear low-density polyethylene; The additive A is maleic anhydride.
5. A lignin asphalt modifier according to claim 1 or 2, characterized in that: The additive B is at least one of 3-amino-1,2,4-triazole, 1,2,4-triazole and imidazole; The additive C is at least one of zinc chloride, ferric chloride, zinc acetate and zinc stearate; The additive D is at least one of rosin ester and rosin ester-modified compound.
6. A lignin asphalt modifier according to claim 1 or 2, characterized in that: The lignin asphalt modifier also includes color powder, which is 0-10 parts by mass.
7. A method for preparing a lignin asphalt modifier according to any one of claims 1 to 6, characterized in that: The following steps are involved: Polyethylene, lignin, ethylene-octene copolymer, additive A, additive B, additive C, additive D, or polyethylene, lignin, ethylene-octene copolymer, additive A, additive B, additive C, additive D, and color powder are uniformly mixed in a mixer, added into a twin-screw extruder for melt blending, extruded and granulated to obtain a lignin asphalt modifier.
8. The method for preparing a lignin asphalt modifier according to claim 7, characterized in that: The mixing time in the mixer is 1-5 min, and the rotation speed is 200-2000 r / min; The temperature of the melt blending is 150-190° C., the screw speed is 50-200 r / min, and the vacuum degree is 0-(-0.08) MPa.
9. Use of the lignin asphalt modifier according to any one of claims 1 to 6 in asphalt.
10. The use of a lignin asphalt modifier in asphalt according to claim 9, characterized in that: Calculated by weight, it comprises 0.1-10 parts of the lignin asphalt modifier according to any one of claims 1-6 and 90-99.9 parts of base asphalt; The specific method is: heating the base asphalt to 120-200° C., adding the lignin asphalt modifier described in any one of claims 1-6 and mixing them evenly to obtain an asphalt composition for construction.
Citation Information
Patent Citations
Traffic anti-track asphalt modifier and its modified asphalt and asphalt mixture
CN101165102A
Anti-rut high-viscosity asphalt modifier, and preparation method and application thereof
CN102796388A
Road asphalt mixture rut resisting additive and preparation method thereof
CN102964525A
Lignin / polyolefin thermoplastic elastomer composite and preparation method thereof
CN107474374A
High-viscosity and high-elasticity modified asphalt as well as preparation and application thereof
CN107722648A
Cited By
Preparation method of composite modified asphalt
CN119570272A