Biodegradable plastic film and preparation method thereof

By optimizing the biodegradable plastic film composed of polyadipic acid-butylene terephthalate, polylactic acid and starch, combined with epoxy soybean oil and antioxidants, the unreasonable composition distribution ratio and production in the prior art are solved. The high cost problem has achieved efficient biodegradation and environmentally friendly agricultural membrane preparation.

CN118956111APending Publication Date: 2024-11-15HEBEI KELUN PLASTIC TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411032352.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The problems of unreasonable composition distribution ratio of existing biodegradable plastic films, high production costs, and partially non-degradable, resulting in environmental pollution and insufficient material performance.

Method used

Biodegradable plastic film composed of polyadipic acid-butylene terephthalate, polylactic acid, starch, epoxy soybean oil and antioxidants, and is melt blended and modified inorganic materials and small amino molecules. Use to enhance the fluidity, toughness and biodegradability of the material, and enhance the intermolecular interaction force through epoxy soybean oil.

Benefits of technology

It improves the overall mechanical properties, degradation properties and production efficiency of the material, reduces production costs, and achieves efficient biodegradation and environmentally friendly agricultural membrane preparation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the field of composite materials, and particularly relates to a biodegradable plastic film and a preparation method thereof. The degradable plastic film comprises 40 to 50 parts of poly (butylene adipate-co-terephthalate), 20 to 35 parts of polylactic acid, 7 to 15 parts of starch, 5 to 10 parts of an auxiliary material a, 2 to 5 parts of an auxiliary material b, 2 to 4 parts of epoxidized soybean oil and 1 to 2 parts of an antioxidant. The preparation method comprises the following steps: mixing the poly (butylene adipate-co-terephthalate) and the auxiliary material a according to a mass ratio to obtain a mixture 1, and mixing the polylactic acid and the auxiliary material b according to a mass ratio to obtain a mixture 2; and finally, mixing the mixture 1, the mixture 2, starch, epoxidized soybean oil and an antioxidant, and then carrying out blowing, traction, printing and rolling to obtain the degradable agricultural film. The degradable plastic film prepared based on the application not only has a degradation rate of 99.6% in a natural environment, but also has relatively strong tensile property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of composite materials, and specifically relates to a biodegradable plastic film and a preparation method thereof. Background Art

[0002] In the field of modern agriculture, agricultural greenhouse films are increasingly used as an important means to regulate the growth environment of crops and improve crop yields and quality. However, traditional agricultural greenhouse films are mostly made of non-degradable plastics. These materials are abandoned in farmland after completing their use cycle, causing long-term and far-reaching harm to the environment. Although the use of non-degradable plastics in agricultural greenhouse films has met the needs of agricultural production to a certain extent, the environmental harm they bring cannot be ignored. These plastic wastes are retained in farmland for a long time, which not only destroys the soil structure and affects soil fertility, but may also pollute the groundwater system through infiltration. What is more serious is that after plastic fragments are accidentally eaten by wild animals, they may cause digestive tract diseases or even death, posing a threat to the ecological balance. In addition, the decomposition of plastics takes hundreds of years or even longer, and their large accumulation has exacerbated the global plastic pollution problem and posed a long-term challenge to the earth's environment.

[0003] With the enhancement of environmental awareness and the popularization of the concept of sustainable development, the application research of degradable plastics in the field of agricultural greenhouse film has gradually become a hot topic. Degradable plastics can be gradually degraded into harmless substances such as carbon dioxide and water through the decomposition of microorganisms in the natural environment, thereby reducing pollution to the environment. Compared with traditional plastics, degradable plastics have the following significant advantages: first, they are environmentally friendly and reduce damage to the natural environment; second, they have good biocompatibility and can be safely decomposed by microorganisms; third, they have diverse performances and can adjust the formula according to needs to meet different application scenarios; fourth, they can be recycled and reused, which improves resource utilization efficiency. There are many types of degradable plastics, which can be divided into photodegradable plastics, biodegradable plastics, and photo-biodegradable plastics according to the degradation mechanism and the source of raw materials. In the field of agricultural greenhouse film, the commonly used degradable plastics are mainly biodegradable plastics, among which PBAT and PLA have attracted widespread attention due to their excellent performance and moderate cost. PBAT has good toughness and processing properties. Due to its long chain structure, its rigidity is relatively low; while PLA has high rigidity and biodegradability, but poor toughness.

[0004] The Chinese patent with the announcement number CN109824962A discloses a degradable polyethylene mulch material and its preparation method, but its main raw materials include modified polyethylene and polylactic acid, wherein the modified polyethylene is modified by surfactants such as silane coupling agents to improve the interfacial compatibility with other substances. The application adds degradable components such as polylactic acid, but does not fundamentally solve the problem that polyethylene materials can be degraded. The Chinese patent with the announcement number CN110016217A discloses a preparation method for a degradable agricultural composite plastic mulch, in which polylactic acid is used as the base resin, and bamboo cellulose, modified nano-silicon dioxide, carboxymethyl cellulose, sweet potato starch, chitosan and tributyl citrate are added to prepare a degradable agricultural composite plastic mulch. Although the formula ingredients can be degraded and do not pollute the environment, the amount of bamboo cellulose added in the formula is 30-40 points, which is a large amount and may reduce the toughness of the material. The Chinese patent with the announcement number CN111607203B discloses a reinforced and toughened poly(adipate / butylene terephthalate)-poly(lactic acid) composite film and its preparation method, wherein poly(lactic acid), poly(adipate / butylene terephthalate) and a cage-shaped polysilsesquioxane containing an octaepoxy group are melt-extruded to prepare a degradable plastic film, and the prepared degradable film has high performance, but the cage-shaped polysilsesquioxane containing an octaepoxy group in the patent has a high cost and is not suitable for preparing agricultural films or industrial production. The Chinese patent with the announcement number CN112063126B discloses a fully biodegradable starch composite mulch film and its preparation method, comprising the following components: poly(adipate / butylene terephthalate) resin particles, an antioxidant, a cross-linking agent, a plasticizer, and a modified starch, but does not solve the problem that the long-chain structure of the poly(adipate / butylene terephthalate) resin particles leads to relatively low rigidity.

[0005] To sum up, the existing preparation of degradable plastic films has problems such as unreasonable component ratio, high production cost, and partial non-degradability. It is urgent to propose a biodegradable plastic film and its preparation method to solve the problems of unreasonable formula and high production cost in the current production of degradable plastic films. Summary of the invention

[0006] In view of the problems existing in the existing biodegradable plastic film production technology, such as unreasonable component ratio, high production cost, and partial non-degradability, the present application proposes a biodegradable plastic film and a preparation method thereof.

[0007] The technical solution of this application is as follows:

[0008] On the one hand, the present application provides a composition ratio of a biodegradable plastic film, which is as follows:

[0009] A biodegradable plastic film, comprising the following components:

[0010] 40-50 parts of polybutylene adipate-terephthalate, 20-35 parts of polylactic acid, 7-15 parts of starch, 5-10 parts of auxiliary material a, 2-5 parts of auxiliary material b, 2-4 parts of epoxidized soybean oil, and 1-2 parts of antioxidant.

[0011] Preferably, 40-45 parts of polybutylene adipate-terephthalate, 30-32 parts of polylactic acid, 10-11 parts of starch, 7-9 parts of auxiliary material a, 2-4 parts of auxiliary material b, 2-4 parts of epoxidized soybean oil, and 1-2 parts of antioxidant.

[0012] Preferably, the auxiliary material a is a modified inorganic material, specifically any one of modified calcium carbonate, modified glass fiber, and modified talc; and the auxiliary material b is a small molecule substance containing amino groups.

[0013] Preferably, the modifier of the auxiliary material a is any one of fatty acids, phosphates, quaternary ammonium salts, silane coupling agents, and titanate coupling agents.

[0014] Preferably, the auxiliary material b is any one of thiourea or amino acid.

[0015] Preferably, the auxiliary material b is thiourea.

[0016] Preferably, the antioxidant is any one of antioxidant 1010 or antioxidant 1076.

[0017] On the other hand, the present application provides a method for preparing a biodegradable plastic film, which is as follows:

[0018] Step S1. Polybutylene adipate-terephthalate and auxiliary material a are mixed in a mass ratio to obtain a mixture 1, wherein the mixing time is 0.5 to 1 h and the mixing temperature is 80 to 120° C.;

[0019] By adopting the above technical solution, auxiliary material a is melt-blended with polybutylene adipate-terephthalate, thereby improving the fluidity of polybutylene adipate-terephthalate, and the physical blending operation is simple and suitable for industrial production. Auxiliary material a is a modified inorganic material, and the inorganic filler is treated with a surface modifier to weaken the interaction between the inorganic fillers, improve the affinity with the polymer, and improve the performance of the biodegradable plastic.

[0020] Step S2. polylactic acid and auxiliary material b are mixed according to the mass ratio, stirred at 170-185° C. for 1-2 h, then reduced to -0.5-0.1 MPa, cooled to 130-140° C., stirred for 0.5-1 h, and obtained mixture 2;

[0021] By adopting the above technical solution, small molecule substances containing amino groups are added to polylactic acid for modification, and the toughness of the polylactic acid molecules is improved by combining the amino groups with the carbonyl groups in the molecular chains of the polylactic acid.

[0022] Step S3. Mix mixture 1, mixture 2, starch, epoxidized soybean oil and antioxidant at a blending temperature of 120 to 140° C. for 0.5 to 1 hour, and then obtain a degradable agricultural film by blowing, pulling, printing and rolling.

[0023] By adopting the above technical solution, epoxy soybean oil is introduced as an additive. The epoxy group in its molecular structure can promote the ring-opening reaction with the terminal hydroxyl and carboxyl groups in the molecular chains of biodegradable polymers such as polylactic acid, polybutylene adipate-terephthalate and starch. The interaction between molecules is enhanced, thereby greatly improving the interfacial adhesion of the composite material. The overall mechanical properties of the material are improved. The introduction of starch as a filler not only enhances the volume stability and processing performance of the material as a physical filler, but also further improves the biodegradability of the material. Based on the wide source of starch, the production cost of the degradable film is reduced.

[0024] Beneficial effects of this application:

[0025] (1) In the present application, the long chain structure of the degradable component polybutylene adipate-terephthalate leads to its weak rigidity and strong toughness. The auxiliary material a is melt-blended with polybutylene adipate-terephthalate to improve the fluidity of polybutylene adipate-terephthalate, and the physical blending operation is simple and suitable for industrial production. On the other hand, the auxiliary material a of the present application adopts modified inorganic materials, and the inorganic filler has the advantages of excellent weather resistance, heat resistance and degradability. The inorganic filler is treated with a surface modifier to weaken the interaction between the inorganic fillers, improve the affinity with the polymer, and improve the performance of the biodegradable plastic.

[0026] (2) In the polylactic acid of the present application, the carbonyl group is coplanar with the adjacent oxygen atom in the molecular chain and is close to the adjacent carbon atom, making it difficult to rotate. This results in poor flexibility of the molecular chain, and the material appears to be hard and brittle, with poor impact resistance. Therefore, the present application modifies the polylactic acid by adding small molecule substances containing amino groups, and improves the toughness of the polylactic acid molecules by combining the amino groups with the carbonyl groups in the molecular chain of the polylactic acid.

[0027] (3) The present application introduces epoxidized soybean oil as an additive. As a naturally derived plasticizer and interfacial modifier, epoxidized soybean oil has the advantages of low cost, environmental friendliness and non-toxicity to the human body. The molecular structure of epoxidized soybean oil is rich in epoxy groups. These active groups can promote ring-opening reactions with terminal hydroxyl groups and carboxyl groups in the molecular chains of biodegradable polymers such as polylactic acid, polybutylene adipate-terephthalate and starch. The intermolecular interaction force is enhanced, thereby greatly improving the interfacial adhesion of the composite material. Improve the overall mechanical properties of the material. In addition, the addition of epoxidized soybean oil also gives the degradable film more excellent processing properties, such as lower melt viscosity, making the material easier to plasticize, extrude or injection mold during processing, improving production efficiency and reducing energy consumption.

[0028] (4) The introduction of starch as a filler in this application not only has significant economic advantages, but its wide source also ensures the sustainability and stability of the raw materials. The addition of starch not only enhances the volume stability and processing performance of the material as a physical filler, but more importantly, it further improves the biodegradability of the material. In the natural environment, starch can be completely decomposed into carbon dioxide and water by the action of microorganisms, reducing the long-term pollution of plastic waste to the environment. The granular morphology of starch can form a good interface with the polymer matrix, which helps to disperse stress and improve the overall strength of the material. DETAILED DESCRIPTION

[0029] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, features and effects of the present invention are described in detail below in combination with the preferred embodiments.

[0030] At present, in the agricultural production process, the main components of commonly used plastic films are polyethylene (PE), polypropylene (PP), etc., because these materials are difficult to decompose in the natural environment, and plastic shed film is indispensable in agricultural production. According to the data reported, non-degradable plastics are buried underground, and it takes about two hundred years to rot, causing long-term pollution to the soil environment, affecting soil pH, and deteriorating soil quality. The production process of non-degradable plastics is simple and low in cost, so it is still a mainstream commercial product, but from a long-term development perspective, degradable plastics have a greater development prospect, because the main raw materials of degradable plastics, such as polybutylene adipate-terephthalate (PBAT), polylactic acid (PLA), etc., are relatively high in price relative to plastic cost, and polybutylene adipate-terephthalate (PBAT) and polylactic acid (PLA) have some shortcomings due to the structural reasons of the molecules, such as the problems pointed out in the background technology, so it is necessary to perform some modifications before use. The applicant has modified the two materials through searching the literature in the early stage to improve the performance of the materials. Starch-based degradable plastics can be made from corn starch, wheat starch, etc., based on the wide range of starch sources. However, since starch itself is a polysaccharide, its water resistance is poor, which will inevitably affect its performance during use. Therefore, this application attempts to add a small amount of starch as a filler to reduce production costs without degrading the performance of the plastic film. It should be noted that the substances mentioned in this application are all commercially available.

[0031] Embodiment 1

[0032] This embodiment provides a method for preparing a biodegradable plastic film, which is as follows:

[0033] Step S1. Preheat the mixer and set the preheating temperature to 100°C, then add 4.3kg of polybutylene adipate-terephthalate and 0.7kg of KH550 modified calcium carbonate into the mixer, then start the stirring function, set the stirring speed to 80r / min, the stirring time to 50min, and control the temperature of the mixed material at 100°C to obtain a mixture 1;

[0034] Step S2. 3 kg of polylactic acid and 0.5 kg of thiourea were added to a mixer, the temperature of the mixture was controlled to be 180°C, the stirring speed was 80 r / min, and the mixture was stirred for 1.5 h, then the pressure was reduced to -0.3 MPa, and the temperature was lowered to 135°C, and the mixture was stirred for 0.8 h to obtain a mixture 2;

[0035] Step S3. Mix mixture 1, mixture 2, 1.1 kg starch, 0.2 kg epoxidized soybean oil and 0.2 kg antioxidant 1010 in a mixer at a rotation speed of 80 r / min and a temperature of the mixture of 130° C. The mixture is blended for 0.7 h, and then the biodegradable agricultural film is obtained by blowing, pulling, printing and winding.

[0036] Embodiment 2

[0037] This embodiment provides a method for preparing a biodegradable plastic film, which is as follows:

[0038] Step S1. Preheat the mixer and set the preheating temperature to 100°C, then add 4.5 kg of polybutylene adipate-terephthalate and 0.5 kg of benzyl alkyl methyl quaternary ammonium peroxide modified glass fiber into the mixer, then start the stirring function, set the stirring speed to 80 r / min, the stirring time to 30 min, and control the temperature of the mixed material at 120°C to obtain a mixture 1;

[0039] Step S2. 2.7 kg of polylactic acid and 0.3 kg of aspartic acid were added to a mixer, the temperature of the mixture was controlled to be 170°C, the stirring speed was 80 r / min, and the mixture was stirred for 2 h, then the pressure was reduced to -0.1 MPa, and the temperature was lowered to 140°C, and the mixture was stirred for 1 h to obtain a mixture 2;

[0040] Step S3. Mix mixture 1, mixture 2, 1.5 kg starch, 0.4 kg epoxidized soybean oil and 0.1 kg antioxidant 1010 in a mixer at a rotation speed of 80 r / min and a temperature of the mixture of 135° C. for 0.5 h, and then obtain a degradable agricultural film by blowing, pulling, printing and winding.

[0041] Embodiment 3

[0042] This embodiment provides a method for preparing a biodegradable plastic film, which is as follows:

[0043] Step S1. Preheat the mixer and set the preheating temperature to 100°C, then add 5 kg of polybutylene adipate-terephthalate and 0.9 kg of talc modified by alkyl polyoxyethylene ether phosphate salt into the mixer, then start the stirring function, set the stirring speed to 80 r / min, the stirring time to 60 min, and control the temperature of the mixture at 80°C to obtain a mixture 1;

[0044] Step S2. 2.5 kg of polylactic acid and 0.4 kg of lysine were added to a mixer, the temperature of the mixture was controlled to be 185° C., the stirring speed was 80 r / min, and the mixture was stirred for 1 h, then the pressure was reduced to -0.5 MPa, and the temperature was lowered to 130° C. The mixture was stirred for 0.5 h to obtain a mixture 2;

[0045] Step S3. Mix mixture 1, mixture 2, 0.7 kg starch, 0.35 kg epoxidized soybean oil and 1.5 kg antioxidant 1076 in a mixer at a rotation speed of 80 r / min and a temperature of the mixture of 140° C. The mixture is blended for 1 hour, and then the biodegradable agricultural film is obtained by blowing, pulling, printing and winding.

[0046] Embodiment 4

[0047] This embodiment provides a method for preparing a biodegradable plastic film, which is as follows:

[0048] Step S1. Preheat the mixer and set the preheating temperature to 100°C, then add 4 kg of polybutylene adipate-terephthalate and 1 kg of stearic acid-modified calcium carbonate into the mixer, then start the stirring function, set the stirring speed to 80 r / min, the stirring time to 40 min, and control the temperature of the mixed material at 110°C to obtain a mixture 1;

[0049] Step S2. 3.5 kg of polylactic acid and 0.2 kg of aspartic acid were added to a mixer, the temperature of the mixture was controlled to be 170° C., the stirring speed was 80 r / min, and the mixture was stirred for 1.6 h, then the pressure was reduced to -0.2 MPa, and the temperature was lowered to 133° C. The mixture was stirred for 0.5 h to obtain a mixture 2;

[0050] Step S3. Mix mixture 1, mixture 2, 1 kg starch, 0.2 kg epoxidized soybean oil and 0.1 kg antioxidant 1076 in a mixer at a rotation speed of 80 r / min and a temperature of the mixture of 120° C. The mixture is blended for 0.6 h, and then the biodegradable agricultural film is obtained by blowing, pulling, printing and winding.

[0051] Comparative Example 1

[0052] The main difference between this comparative example and Example 1 is that the calcium carbonate in step S1 of this comparative example is not modified.

[0053] Comparative Example 2

[0054] The main difference between this comparative example and Example 1 is that no KH550-modified calcium carbonate is added in step S1 of this comparative example.

[0055] Comparative Example 3

[0056] The main difference between this comparative example and Example 1 is that no thiourea is added in step S2 of this comparative example.

[0057] Comparative Example 4

[0058] The main difference between this comparative example and Example 1 is that there is no epoxidized soybean oil in step S3 of this comparative example.

[0059] Performance Testing

[0060] (1) Degradation performance test: The sample material is mixed with the compost inoculum and placed in a composting container. The composting is carried out under certain temperature (58±2℃) and humidity (50%~55%) conditions. The final release of CO2 after the material is degraded is measured. The ratio of the actual CO2 release to its theoretical maximum release is used to express the biodegradation rate of the material.

[0061] (2) Mechanical properties test: Refer to standard GB / T35795-2017 "Fully biodegradable agricultural ground covering film" to test the tensile load (unit: N).

[0062] Table 1

[0063] sample 45d degradation rate (%) 180d degradation rate (%) Tensile load (N) Embodiment 1 85.3 99.6 6.15 Embodiment 2 86.7 98.7 5.98 Embodiment 3 80.1 96.5 5.81 Embodiment 4 79.9 99.1 5.79 Comparative Example 1 82.7 96.9 4.02 Comparative Example 2 78.5 98.3 3.97 Comparative Example 3 79.8 97.6 3.85 Comparative Example 4 81.6 98.9 4.50

[0064] Results Analysis

[0065] In combination with Examples 1 to 4, Comparative Examples 1 to 4 and Table 1, it can be seen that by using the method of the present application, the degradation rate of the 180-day degradation test can reach up to 99.6%. This is because the preparation raw materials used in the present application are all biodegradable materials; at the same time, they have high tensile strength, among which Example 1 has the best effect. It may be that under the parameter ratio conditions, the performance of each component can fully cooperate with each other to improve the performance of the degradable film. The materials in Comparative Examples 1 to 4 have good degradation performance, but because some components are indeed or not modified during the preparation process, their mechanical properties are reduced. This may be due to uneven dispersion of the material or poor interface compatibility of the material, resulting in the tensile load of the comparative material being lower than that of the degradable film prepared based on the method of the present application.

[0066] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A biodegradable plastic film, characterized in that: The components include the following parts: 40-50 parts of polybutylene adipate-terephthalate, 20-35 parts of polylactic acid, 7-15 parts of starch, 5-10 parts of auxiliary material a, 2-5 parts of auxiliary material b, 2-4 parts of epoxidized soybean oil, and 1-2 parts of antioxidant.

2. The biodegradable plastic film according to claim 1, characterized in that: The invention comprises the following components: 40-45 parts of polybutylene adipate-terephthalate, 30-32 parts of polylactic acid, 10-11 parts of starch, 7-9 parts of auxiliary material a, 2-4 parts of auxiliary material b, 2-4 parts of epoxidized soybean oil and 1-2 parts of antioxidant.

3. The biodegradable plastic film according to claim 1, characterized in that: The auxiliary material a is a modified inorganic material, specifically any one of modified calcium carbonate, modified glass fiber, and modified talcum powder; the auxiliary material b is a small molecule substance containing amino groups.

4. The biodegradable plastic film according to claim 1, characterized in that: The modifier of the auxiliary material a is any one of fatty acids, phosphates, quaternary ammonium salts, silane coupling agents, and titanate coupling agents.

5. The biodegradable plastic film according to claim 1, characterized in that: The auxiliary material b is any one of thiourea or amino acid.

6. The biodegradable plastic film according to claim 1, characterized in that: The auxiliary material b is thiourea.

7. The biodegradable plastic film according to claim 1, characterized in that: The antioxidant is any one of antioxidant 1010 and antioxidant 1076.

8. The method for preparing a biodegradable plastic film according to any one of claims 1 to 7, characterized in that: The steps include: Step S1. Polybutylene adipate-terephthalate and auxiliary material a are mixed in a mass ratio to obtain a mixture 1, wherein the mixing time is 0.5 to 1 h and the mixing temperature is 80 to 120° C.; Step S2. polylactic acid and auxiliary material b are mixed according to the mass ratio, stirred at 170-185° C. for 1-2 h, then reduced to -0.5-0.1 MPa, cooled to 130-140° C., stirred for 0.5-1 h, and obtained mixture 2; Step S3. Mix mixture 1, mixture 2, starch, epoxidized soybean oil and antioxidant at a blending temperature of 120 to 140° C. for 0.5 to 1 hour, and then obtain a degradable agricultural film by blowing, pulling, printing and rolling.

Citation Information

Cited By

  • Degradable protective film and preparation method thereof

    CN119875335A

  • Degradable starch-based plastic bag and preparation method thereof

    CN120988374A