Coating for silver-plated bead tube as well as preparation method and application of coating

By combining water-based polyurethane emulsion, acrylic hardening emulsion and polyurethane modified alkyd resin, combined with titanium dioxide and mica powder and other materials, an environmentally friendly high-performance silver-plated bead tube coating was prepared, which solved the poor anti-oxidation performance of existing coatings. Due to the major environmental impact issues, the durable and environmentally friendly silver-plated layer protection effect is achieved.

CN118956244AActive Publication Date: 2024-11-15浙江材华科技有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411196345.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The existing silver-plated bead tube coatings have poor oxidation resistance, and solvent-based coatings are harmful to the environment and health. Traditional protection methods cannot effectively protect the silver-plated layer for a long time.

Method used

Use aqueous polyurethane emulsion, aqueous acrylic hardening emulsion and aqueous polyurethane modified alkyd resin to combine titanium dioxide, barium sulfate and mica powder, and add appropriate amounts of auxiliary materials such as base wetting agent, leveling agent and ultraviolet absorber. An environmentally friendly high-performance coating is prepared through specific ratios and processes.

Benefits of technology

It has achieved good film-forming properties, ultraviolet resistance, long service life, yellowing resistance, high hiding ability and good oxidation resistance of the coating. It has significantly improved the protection effect of the silver plating layer, and at the same time reduced the VOC content, which is simple and easy to process. Environmental friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005016515300000131
    Figure BDA0005016515300000131
Patent Text Reader

Abstract

The invention discloses a coating for a silver-plated bead tube as well as a preparation method and application thereof, and belongs to the technical field of coatings for silver-plated bead tubes. The coating is prepared from the following raw materials in parts by weight: 30 to 40 parts of waterborne polyurethane emulsion, 5 to 10 parts of waterborne acrylic acid hardening emulsion, 5 to 10 parts of waterborne polyurethane modified alkyd resin, various auxiliaries, pigments and fillers. By utilizing the film-forming assisting property of the waterborne polyurethane modified alkyd resin on the waterborne polyurethane emulsion and the waterborne acrylic hardening emulsion, a coating can form a film very well, the problem that a low-boiling-point solvent type coalescing agent is not environmentally friendly is solved, VOC is reduced, and the adverse effect of a high-boiling-point solvent type coalescing agent on the drying speed and the early performance is also avoided. The coating is low in organic volatile matter content, free of heavy metal and environmentally friendly, and a coating prepared from the coating is good in ultraviolet resistance, long in service life, resistant to yellowing, high in covering power and the like and has a good protection effect on a silver coating. The corresponding production process is simple and convenient and good in stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silver-plated bead tube coatings, and in particular to a coating for silver-plated bead tubes and a preparation method and application thereof. Background Art

[0002] Bead tube embroidery is an embroidery technique in which threaded bead tubes are fixed on the fabric with an embroidery machine. Bead tubes with silver-plated inner walls are widely used because they are more shiny, but the silver-plated layer is easily oxidized and turns yellow or even black, greatly affecting the decorative effect of embroidery.

[0003] In order to ensure the appearance stability of the silver-plated bead tube, the silver-plated layer needs to be protected. The traditional protection method is to use passivation liquid or paint protection, but the former will cause the silver-plated layer to turn yellow, and the protection time is not long enough. Using paint protection is a better solution, but currently solvent-based paints are mainly used in large quantities, the coating is thin, and the whitening effect and antioxidant protection effect are not ideal, especially when using a bleaching solution containing hypochlorous acid for antioxidant performance testing. It often fails. In addition, the VOCs of solvent-based paints are very high, which has a great impact on the environment and health.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a coating for silver-plated bead tubes and a preparation method and application thereof, so as to solve or improve the above-mentioned technical problems.

[0006] This application can be implemented as follows:

[0007] In a first aspect, the present application provides a coating for silver-plated bead tubes, wherein the raw materials thereof include, by weight, a main film-forming substance, wherein the main film-forming substance includes 30-40 parts of an aqueous polyurethane emulsion, 5-10 parts of an aqueous acrylic hardening emulsion, and 5-10 parts of an aqueous polyurethane modified alkyd resin.

[0008] In an optional embodiment, the raw materials further include a secondary film-forming substance, and the secondary film-forming substance includes 15-30 parts of titanium dioxide, 2-5 parts of barium sulfate and 2-5 parts of mica powder.

[0009] In an optional embodiment, the titanium dioxide is a chloride-process rutile type; and / or the barium sulfate is produced by a precipitation method; and / or the mica powder is a flaky structure.

[0010] In an optional embodiment, the above raw materials also include auxiliary materials; the auxiliary materials include 0.1-0.5 parts of substrate wetting agent, 0.5-1.5 parts of leveling agent, 0.1-1 parts of ultraviolet absorber, 0.1-1.0 parts of pH adjuster, 0.3-1 parts of thickener, 0.5-1.5 parts of anti-settling agent, 1-2 parts of dispersant, 0.2-0.5 parts of defoaming agent, 0.1-0.2 parts of preservative, 1-3 parts of cross-linking agent, 0.5-1 parts of adhesion promoter, 3-5 parts of slip agent and 0.01-0.05 parts of whitening agent.

[0011] In an optional embodiment, the defoaming agent includes high molecular polymer SN-6788;

[0012] and / or, the dispersant is a high molecular weight hyperdispersant containing a plurality of pigment-affinity groups;

[0013] and / or, the substrate wetting agent comprises at least one of a silicone wetting agent and a fluorocarbon wetting agent;

[0014] And / or, the leveling agent is a fluorine-modified acrylic leveling agent;

[0015] and / or, the thickener is a polyurethane associative thickener that does not contain an organic solvent;

[0016] and / or, the anti-settling agent is a water-based polyurea anti-settling agent;

[0017] and / or, the pH regulator is a special silicone-type pH regulator;

[0018] and / or, the ultraviolet absorber comprises at least one of UV1130, RQT-X-1, 2-hydroxy-4-methoxydiphenylacetone-5-sulfonic acid and a hydrophobic hydroxyphenyltriazine compound;

[0019] and / or, the brightener is a water-resistant blue macromolecular colorant;

[0020] and / or, the cross-linking agent comprises at least one of a metal ion cross-linking agent and a polycarbodiimide cross-linking agent;

[0021] and / or, the adhesion promoter is an organosilane oligomer;

[0022] And / or, the slip agent is oxidized polyethylene wax emulsion.

[0023] In an alternative embodiment, the dispersant includes at least one of SN-1790A, SN-1760, COADIS 790, and COADIS 490;

[0024] and / or, the silicone wetting agent includes at least one of WET 270, SN-4741 and Twin 4100, and the fluorocarbon wetting agent includes at least one of ZH-8004 and SN-4763;

[0025] and / or, the leveling agent comprises at least one of AKN-1181, SN-3781 and ZH-8004;

[0026] and / or, the thickener comprises at least one of FLUGO A3151 and Coapur XS83;

[0027] and / or, the anti-settling agent comprises at least one of SN-9742 and F5715;

[0028] and / or, the pH adjuster comprises BS168;

[0029] and / or, the preservative comprises at least one of BN-510 and RT-3318;

[0030] and / or, the metal ion crosslinker comprises ZINPLEX 15;

[0031] and / or, the polycarbodiimide type crosslinking agent comprises at least one of CARBODILITE E-02 and ACRAFIX FAC;

[0032] And / or, the adhesion promoter includes at least one of OS-79 and KRN8027.

[0033] In an optional embodiment, in the substrate wetting agent, the mass ratio of the silicone wetting agent to the fluorocarbon wetting agent is 2:1.

[0034] In an optional embodiment, in the cross-linking agent, the mass ratio of the metal ion type cross-linking agent to the polycarbodiimide type cross-linking agent is 1:1.

[0035] In a second aspect, the present application provides a method for preparing the above-mentioned coating for silver-plated bead tubes, comprising the following steps: mixing the raw materials according to a proportion.

[0036] In an optional embodiment, deionized water, a defoamer, a dispersant, an anti-settling agent, titanium dioxide, barium sulfate, and mica powder are prepared into a pre-dispersed slurry;

[0037] The pre-dispersed slurry is mixed with an aqueous polyurethane emulsion, an aqueous acrylic hardening emulsion and an aqueous polyurethane modified alkyd resin to obtain a first slurry;

[0038] Mixing a substrate wetting agent, a leveling agent, a cross-linking agent, an adhesion promoter, an ultraviolet absorber, a preservative, a slip agent, and a whitening agent with the first slurry to obtain a second slurry;

[0039] The pH adjuster and the thickener are mixed with the second slurry to obtain a coating.

[0040] In an optional embodiment, titanium dioxide, barium sulfate and mica powder are ground to a particle size not exceeding 20 microns, and then mixed with a mixed solution formed by deionized water, a defoaming agent, a dispersant and an anti-settling agent to obtain a pre-dispersed slurry.

[0041] In a third aspect, the present application also provides an application of the above-mentioned coating for silver-plated bead tubes, for example, for coating the inner surface of the silver-plated bead tubes.

[0042] In a fourth aspect, the present application also provides a silver-plated bead tube, the surface of which has the above-mentioned coating for silver-plated bead tubes.

[0043] The beneficial effects of the present invention include:

[0044] This application utilizes the film-forming properties of aqueous polyurethane modified alkyd resin to aqueous polyurethane emulsion and aqueous acrylic hardening emulsion, so that the coating can form a good film, solves the environmental unfriendly nature of low-boiling point solvent-based film-forming aids, reduces VOC, and avoids the adverse effects of high-boiling point solvent-based film-forming aids on drying speed and early performance. The coating has low organic volatile content, does not contain heavy metals, is environmentally friendly, and the coating prepared by the coating has good UV resistance, long service life, anti-yellowing, high hiding power, high whiteness, good antioxidant properties, and good protective effect on the silver-plated layer. The corresponding production process is simple and has good stability. The above-mentioned silver-plated bead tube coating can be used to apply to the inner surface of the silver-plated bead tube, and is particularly suitable for coating the inner wall of the glass bead tube using a stir-frying process, and can have a good whitening and antioxidant protective effect on the silver-plated layer of the inner wall of the glass bead tube. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0046] The coating for silver-plated bead tubes provided in this application and its preparation method and application are described in detail below.

[0047] The present application proposes a coating for silver-plated bead tubes, wherein the raw materials thereof include a main film-forming substance by weight, and the main film-forming substance includes 30-40 parts of waterborne polyurethane emulsion, 5-10 parts of waterborne acrylic hardening emulsion and 5-10 parts of waterborne polyurethane modified alkyd resin.

[0048] Illustratively, the content of the aqueous polyurethane emulsion in the raw materials of the coating can be 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts or 40 parts, etc., or it can be any other value within the range of 30-40 parts.

[0049] The content of the aqueous acrylic hardening emulsion in the raw materials of the coating can be 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts or 10 parts, etc., or it can be any other value within the range of 5-10 parts.

[0050] The content of the waterborne polyurethane modified alkyd resin in the raw material of the coating can be 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts or 10 parts, etc., or it can be any other value within the range of 5-10 parts.

[0051] In the present application, the main film-forming material is compounded by the three different types of aqueous emulsions or resins mentioned above, among which the aqueous polyurethane emulsion is a water-resistant single-component polyurethane emulsion with a solid content of about 35%, and this component is mainly used to provide the main properties for the coating; the aqueous acrylic hardening emulsion is a product with a high glass transition temperature, and its solid content can be about 45%; the aqueous polyurethane modified alkyd resin is a renewable plant-based environmentally friendly product, and its solid content can be about 35%.

[0052] The coating provided in the present application does not use a solvent-based film-forming aid, but instead, through the compounding of the above-mentioned resin and emulsion, the film-forming aid of the waterborne polyurethane-modified alkyd resin on the other two emulsions (waterborne polyurethane emulsion and waterborne acrylic hardening emulsion) is utilized, so that the coating can form a good film, which solves the environmentally unfriendly problem of using low-boiling point solvent-based film-forming aids (such as ethylene glycol butyl ether, diethylene glycol butyl ether, etc.) in the prior art, making the VOC of the coating lower, and avoids the adverse effects of using high-boiling point solvent-based film-forming aids (such as alcohol ester dodecahydrate, alcohol ester hexadecene, OE-300, TXIB, etc.) in the prior art on drying speed and early performance.

[0053] Furthermore, the raw materials of the coating also include secondary film-forming substances, which include 15-30 parts of titanium dioxide, 2-5 parts of barium sulfate and 2-5 parts of mica powder.

[0054] The content of titanium dioxide in the raw material of the coating can be 15 parts, 18 parts, 20 parts, 22 parts, 25 parts, 28 parts or 30 parts, etc., or any other value within the range of 15-30 parts.

[0055] The content of barium sulfate in the raw material of the coating can be 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts, etc., or any other value within the range of 2-5 parts.

[0056] The content of mica powder in the raw material of the coating can be 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts, etc., or any other value within the range of 2-5 parts.

[0057] The titanium dioxide is mainly used to provide covering power and ultraviolet shielding effect for the coating, and illustratively, it can be rutile titanium dioxide produced by the chloride process. Barium sulfate can be used as a synergist for titanium dioxide, and illustratively, it can be produced by the precipitation process. Mica powder is mainly used to enhance the shielding structure of the coating and improve the anti-oxidation performance of the coating, and illustratively, it can be a flaky structure.

[0058] Furthermore, the raw materials of the coating provided in the present application also include auxiliary materials and water.

[0059] The amount of water can be 10-15 parts, such as 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts, etc., or any other value within the range of 10-15 parts.

[0060] The auxiliary materials include 0.1-0.5 parts of substrate wetting agent, 0.5-1.5 parts of leveling agent, 0.1-1 parts of ultraviolet absorber, 0.1-1.0 parts of pH adjuster, 0.3-1 parts of thickener, 0.5-1.5 parts of anti-settling agent, 1-2 parts of dispersant, 0.2-0.5 parts of defoaming agent, 0.1-0.2 parts of preservative, 1-3 parts of cross-linking agent, 0.5-1 parts of adhesion promoter, 3-5 parts of slip agent and 0.01-0.05 parts of whitening agent.

[0061] The content of the substrate wetting agent in the raw material of the coating can be 0.1 part, 0.2 part, 0.3 part, 0.4 part or 0.5 part, etc., or any other value within the range of 0.1-0.5 part.

[0062] In some embodiments, the substrate wetting agent includes at least one of an organosilicon wetting agent and a fluorocarbon wetting agent. In some other embodiments, the substrate wetting agent includes a mixture of an organosilicon wetting agent and a fluorocarbon wetting agent with a twin structure. The former has the effects of fast flow and defoaming assistance, and the latter has extremely low surface tension and anti-oil pollution effects. Exemplarily, the above-mentioned organosilicon wetting agent may include at least one of WET 270, SN-4741 and Twin 4100, and the fluorocarbon wetting agent may include at least one of ZH-8004 and SN-4763. In the above-mentioned substrate wetting agent, the mass ratio of the organosilicon wetting agent to the fluorocarbon wetting agent may be 2:1.

[0063] The content of the leveling agent in the raw material of the coating can be 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts or 1.5 parts, etc., or any other value within the range of 0.5-1.5 parts.

[0064] In some embodiments, the leveling agent is a fluorine-modified acrylic leveling agent to have good wettability and long-wave leveling properties. Exemplarily, the leveling agent may include at least one of AKN-1181, SN-3781 and ZH-8004.

[0065] The content of the ultraviolet absorber in the raw material of the coating can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part or 1 part, etc., or any other value within the range of 0.1-1 part.

[0066] In some embodiments, the ultraviolet absorber may include at least one of UV1130, RQT-X-1, 2-hydroxy-4-methoxydiphenylacetone-5-sulfonic acid, and a hydrophobic hydroxyphenyltriazine compound.

[0067] The content of pH adjuster in the raw material of the coating can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part or 1 part, etc., or any other value within the range of 0.1-1 part.

[0068] In some embodiments, the pH adjuster is a special silicone pH adjuster, which is hydrophobic and can improve the early performance of the coating. For example, the pH adjuster may include BS168.

[0069] The content of the thickener in the raw material of the coating can be 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts or 1 parts, etc., and can also be any other value within the range of 0.3-1 parts.

[0070] In some embodiments, the thickener is a polyurethane associative thickener that does not contain an organic solvent, which may have a good thickening effect. Exemplarily, the thickener may include at least one of FLUGO A3151 and Coapur XS83.

[0071] The content of the anti-settling agent in the raw material of the coating can be 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts or 1.5 parts, etc., or any other value within the range of 0.5-1.5 parts.

[0072] In some embodiments, the anti-settling agent is a water-based polyurea anti-settling agent, which has good compatibility, good anti-settling ability, and better water resistance than inorganic anti-settling agents. Exemplarily, the anti-settling agent may include at least one of SN-9742 and F5715.

[0073] The content of the dispersant in the raw materials of the coating can be 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts or 2 parts, etc., or any other value within the range of 1-2 parts.

[0074] In some embodiments, the dispersant is a high molecular weight super dispersant containing multiple pigment-friendly groups. This type of dispersant has high dispersing efficiency for inorganic pigments and little effect on the water resistance of the paint film. Exemplarily, the above dispersant may include at least one of SN-1790A, SN-1760, COADIS 790 and COADIS 490.

[0075] The content of the defoamer in the raw material of the coating can be 0.2 parts, 0.3 parts, 0.4 parts or 0.5 parts, etc., or any other value within the range of 0.2-0.5 parts.

[0076] In some embodiments, the defoaming agent includes high molecular polymer SN-6788, which is produced by Shanghai Shenzhu Chemical Technology Co., Ltd. The defoaming agent has good defoaming ability and no shrinkage characteristics.

[0077] The content of the preservative in the raw material of the coating can be 0.1 part, 0.15 part or 0.2 part, etc., or any other value within the range of 0.1-0.2 part.

[0078] In some embodiments, the preservative may include at least one of BN-510 and RT-3318.

[0079] The content of the crosslinking agent in the raw material of the coating can be 1 part, 1.5 parts, 2 parts, 2.5 parts or 3 parts, etc., or any other value within the range of 1-3 parts.

[0080] In some embodiments, the crosslinking agent includes at least one of a metal ion crosslinking agent and a polycarbodiimide crosslinking agent. The metal ion crosslinking agent and the polycarbodiimide crosslinking agent can be complexed or crosslinked with the carboxyl group in the resin emulsion to improve the water resistance and oxidation resistance of the coating, and the metal ion crosslinking agent can also accelerate the drying speed. Exemplarily, the above-mentioned metal ion crosslinking agent may include ZINPLEX 15, and the polycarbodiimide crosslinking agent may include at least one of CARBODILITE E-02 and ACRAFIX FAC. In the above-mentioned crosslinking agent, the mass ratio of the metal ion crosslinking agent to the polycarbodiimide crosslinking agent can be 1:1.

[0081] The content of the adhesion promoter in the raw material of the coating can be 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part or 1 part, etc., and can also be any other value within the range of 0.5-1 part.

[0082] In some embodiments, the adhesion promoter is an organosilane oligomer. This type of adhesion promoter has good hydrolysis resistance and can be stably present in the coating. Through the selection of the grafting group, it has good adhesion to metal, but the adhesion effect on glass is not obvious, so as to improve the adhesion of the coating on the silver-plated layer and facilitate the cleaning of the residual coating on the glass surface. Exemplarily, the above-mentioned adhesion promoter may include at least one of OS-79 and KRN8027.

[0083] The content of the slip agent in the raw material of the coating can be 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts, etc., or any other value within the range of 3-5 parts.

[0084] In some embodiments, the slip agent is an oxidized polyethylene wax emulsion, such as at least one of LHWAX 2556 and LHWAX2558, which can provide better slipperiness for the coating, facilitate needle threading of the embroidery machine, and avoid bead jamming.

[0085] The content of the brightener in the raw material of the coating can be 0.01 part, 0.02 part, 0.03 part, 0.04 part or 0.05 part, etc., or any other value within the range of 0.01-0.05 part.

[0086] In some embodiments, the whitening agent is a water-resistant blue macromolecular colorant, which is a water-resistant blue macromolecular colorant (model PMW1374) self-made by Zhejiang Caihua Technology Co., Ltd. This type of water-resistant blue macromolecular colorant does not contain heavy metals, does not contain fluorescence, has high transparency, and can use optical principles to effectively shield the yellow phase of the coating itself, thereby improving the overall whiteness of the glass bead tube.

[0087] In continuation of the above, the silver-plated bead tube coating provided by the present application is a new type of environmentally friendly high-performance water-based coating, which has a low content of volatile organic matter, does not contain heavy metals, is environmentally friendly, and has a VOCs content of less than 100 g / L. The coating film formed by the coating after drying has good UV resistance, long service life, anti-yellowing, high hiding power, high whiteness, good antioxidant performance, and good protection for the silver-plated layer.

[0088] Correspondingly, the present application also provides a method for preparing the above-mentioned coating for silver-plated bead tubes, which may include the following steps: mixing the raw materials according to a ratio.

[0089] In some embodiments, the following steps may be performed:

[0090] S1: preparing a pre-dispersed slurry by mixing deionized water, a defoamer, a dispersant, an anti-settling agent, titanium dioxide, barium sulfate and mica powder;

[0091] S2: mixing the pre-dispersed slurry with the aqueous polyurethane emulsion, the aqueous acrylic hardening emulsion and the aqueous polyurethane modified alkyd resin to obtain a first slurry;

[0092] S3: mixing a substrate wetting agent, a leveling agent, a cross-linking agent, an adhesion promoter, an ultraviolet absorber, a preservative, a slip agent, and a whitening agent with the first slurry to obtain a second slurry;

[0093] S4: Mixing the pH adjuster, the thickener and the second slurry to obtain a coating.

[0094] In the above S1, titanium dioxide, barium sulfate and mica powder may be ground to a particle size not exceeding 20 microns, and then mixed with a mixed solution formed by deionized water, a defoaming agent, a dispersant and an anti-settling agent to obtain a pre-dispersed slurry.

[0095] In the above S4, the pH adjuster is first mixed with the second slurry to adjust to alkalinity, and then a thickener is added to adjust the viscosity. For example, the viscosity can be adjusted to 20±2S.

[0096] As mentioned above, the coating provided in this application has a simple production process and good stability.

[0097] In addition, the present application also provides an application of the above-mentioned coating for silver-plated bead tubes, for example, for coating the inner surface of the silver-plated bead tubes.

[0098] Specifically, the above-mentioned silver-plated bead tube paint can be used to apply to the inner surface of the silver-plated bead tube, and is particularly suitable for coating the inner wall of the glass bead tube using a stir-frying process. It can have a good whitening and anti-oxidation protection effect on the silver-plated layer on the inner wall of the glass bead tube.

[0099] In some embodiments, during construction, an appropriate amount of water is added to adjust the viscosity of the coating. After a period of stirring, the inner wall of the glass bead tube is evenly coated, the outer wall coating gradually dries, the glass bead tube is no longer sticky, and the glass bead tube is in a state of separation. The glass bead tube is then taken out and dried or baked until the inner wall is dry, and the outer wall coating is then polished clean by dry grinding or wet film method, the paint residue is washed clean with water, and then the water is removed by baking, and the construction of the whitening and antioxidant protective coating on the inner wall of the glass bead tube is completed.

[0100] Correspondingly, the present application also provides a silver-plated bead tube, the surface of which has the above-mentioned coating for silver-plated bead tubes. The silver-plated bead tube has good appearance stability.

[0101] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0102] Example 1

[0103] This embodiment provides a coating for silver-plated bead tubes, which is prepared by the following method:

[0104] S1: 12 parts of deionized water, 0.2 parts of defoaming agent, 1 part of dispersant, and 1 part of anti-settling agent are mixed uniformly in proportion to obtain a mixed solution; 25 parts of titanium dioxide, 5 parts of barium sulfate, and 5 parts of mica powder are added to the mixed solution, dispersed at high speed, and then ground with a sand mill to a fineness of less than 20 microns to prepare a pre-dispersed slurry;

[0105] S2: Add 35 parts of aqueous polyurethane emulsion, 8 parts of aqueous acrylic hardening emulsion and 8 parts of aqueous polyurethane modified alkyd resin to the pre-dispersed slurry, mix well, and obtain a first slurry;

[0106] S3: Add 0.3 parts of substrate wetting agent, 0.5 parts of leveling agent, 3 parts of cross-linking agent, 1 part of adhesion promoter, 0.5 parts of ultraviolet absorber, 0.1 parts of preservative, 3 parts of slip agent and 0.1 parts of brightener to the first slurry, stir evenly to obtain a second slurry;

[0107] S4: Add 0.3 parts of pH adjuster to the second slurry to adjust to alkalinity, and then add 0.5 parts of thickener to adjust the viscosity to 20S to obtain a coating.

[0108] Among them, the defoamer is SN-6788, the dispersant is SN-1790A, the anti-settling agent is F5715, the substrate wetting agent is SN-4741, the leveling agent is AKN-1181, the crosslinker is ZINPLEX 15, the adhesion promoter is OS-79, the UV absorber is UV1130, the preservative is BN-510, the slip agent is LHWAX 2556, and the brightener is PMW1374. The water-based polyurethane emulsion is WPU-100T, the water-based acrylic hardening emulsion is Houxian 8025, and the water-based polyurethane modified alkyd resin is AKD 2733.

[0109] Example 2

[0110] This embodiment provides a coating for silver-plated bead tubes, which is prepared by the following method:

[0111] S1: 10 parts of deionized water, 0.2 parts of defoaming agent, 1 part of dispersant, and 1 part of anti-settling agent are mixed uniformly in proportion to obtain a mixed solution; 28 parts of titanium dioxide, 5 parts of barium sulfate, and 3 parts of mica powder are added to the mixed solution, dispersed at high speed, and then ground with a sand mill to a fineness of less than 20 microns to prepare a pre-dispersed slurry;

[0112] S2: Add 32 parts of aqueous polyurethane emulsion, 10 parts of aqueous acrylic hardening emulsion and 8 parts of aqueous polyurethane modified alkyd resin to the pre-dispersed slurry, mix well, and obtain a first slurry;

[0113] S3: Add 0.3 parts of substrate wetting agent, 0.5 parts of leveling agent, 3 parts of cross-linking agent, 1 part of adhesion promoter, 0.5 parts of ultraviolet absorber, 0.1 parts of preservative, 3 parts of slip agent and 0.1 parts of brightener to the first slurry, stir evenly to obtain a second slurry;

[0114] S4: Add 0.3 parts of pH adjuster to the second slurry to adjust to alkalinity, and then add 0.5 parts of thickener to adjust the viscosity to 20S to obtain a coating.

[0115] Among them, the defoamer is SN-6788, the dispersant is SN-1760, the anti-settling agent is SN-9742, the substrate wetting agent is WET270, the leveling agent is SN-3781, the crosslinker is ZINPLEX 15, the adhesion promoter is KRN8027, the UV absorber is UV1130, the preservative is BN-510, the slip agent is LHWAX 2558, and the brightener is PMW1374. The water-based polyurethane emulsion is WPU-100T, the water-based acrylic hardening emulsion is Houxian 8025, and the water-based polyurethane modified alkyd resin is AKD 2733.

[0116] Example 3

[0117] This embodiment provides a coating for silver-plated bead tubes, which is prepared by the following method:

[0118] S1: 12 parts of deionized water, 0.2 parts of defoaming agent, 1 part of dispersant, and 1 part of anti-settling agent are mixed uniformly in proportion to obtain a mixed solution; 22 parts of titanium dioxide, 4 parts of barium sulfate, and 4 parts of mica powder are added to the mixed solution, dispersed at high speed, and then ground with a sand mill to a fineness of less than 20 microns to prepare a pre-dispersed slurry;

[0119] S2: Add 38 parts of aqueous polyurethane emulsion, 6 parts of aqueous acrylic hardening emulsion and 7 parts of aqueous polyurethane modified alkyd resin to the pre-dispersed slurry, mix well, and obtain a first slurry;

[0120] S3: Add 0.3 parts of substrate wetting agent, 0.5 parts of leveling agent, 3 parts of cross-linking agent, 1 part of adhesion promoter, 0.5 parts of ultraviolet absorber, 0.1 parts of preservative, 3 parts of slip agent and 0.1 parts of brightener to the first slurry, stir evenly to obtain a second slurry;

[0121] S4: Add 0.3 parts of pH adjuster to the second slurry to adjust to alkalinity, and then add 0.5 parts of thickener to adjust the viscosity to 20S to obtain a coating.

[0122] Among them, the defoamer is SN-6788, the dispersant is COADIS 490, the anti-settling agent is F5715, the substrate wetting agent is WET270, the leveling agent is ZH-8004, the crosslinker is ACRAFIX FAC, the adhesion promoter is KRN8027, the UV absorber is UV1130, the slip agent is LHWAX 2558, and the brightener is PMW1374. The water-based polyurethane emulsion is WPU-100T, the water-based acrylic hardening emulsion is Houxian 8025, and the water-based polyurethane modified alkyd resin is AKD 2733.

[0123] Test example

[0124] The coatings prepared in Examples 1-3 were tested for performance, and the results are shown in Table 1.

[0125] Table 1 Test results

[0126]

[0127] In summary, the present application utilizes the film-forming properties of aqueous polyurethane modified alkyd resin to aqueous polyurethane emulsion and aqueous acrylic hardening emulsion, so that the coating can form a good film, solves the environmental unfriendly nature of low-boiling point solvent-based film-forming aids, reduces VOC, and avoids the adverse effects of high-boiling point solvent-based film-forming aids on drying speed and early performance. The coating has a low content of volatile organic matter, does not contain heavy metals, is environmentally friendly, and the coating prepared by the coating has good UV resistance, long service life, anti-yellowing, high hiding power, high whiteness, good antioxidant properties, and good protective effect on the silver-plated layer. The corresponding production process is simple and has good stability. The above-mentioned silver-plated bead tube coating can be used to apply to the inner surface of the silver-plated bead tube, and is particularly suitable for coating the inner wall of the glass bead tube using a stir-frying process, and can have a good whitening and antioxidant protective effect on the silver-plated layer of the inner wall of the glass bead tube.

[0128] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A coating for silver-plated bead tubes, characterized in that: The raw materials of the silver-plated bead tube coating include main film-forming substances by weight, and the main film-forming substances include 30-40 parts of waterborne polyurethane emulsion, 5-10 parts of waterborne acrylic hardening emulsion and 5-10 parts of waterborne polyurethane modified alkyd resin.

2. The coating for silver-plated bead tubes according to claim 1, characterized in that: The raw materials also include secondary film-forming substances, which include 15-30 parts of titanium dioxide, 2-5 parts of barium sulfate and 2-5 parts of mica powder; Preferably, the titanium dioxide is of chloride-process rutile type; and / or the barium sulfate is produced by precipitation method; and / or the mica powder is of flaky structure.

3. The coating for silver-plated bead tubes according to claim 1 or 2, characterized in that: The raw materials also include auxiliary materials; the auxiliary materials include 0.1-0.5 parts of substrate wetting agent, 0.5-1.5 parts of leveling agent, 0.1-1 parts of ultraviolet absorber, 0.1-1.0 parts of pH regulator, 0.3-1 parts of thickener, 0.5-1.5 parts of anti-settling agent, 1-2 parts of dispersant, 0.2-0.5 parts of defoaming agent, 0.1-0.2 parts of preservative, 1-3 parts of cross-linking agent, 0.5-1 parts of adhesion promoter, 3-5 parts of slip agent and 0.01-0.05 parts of whitening agent.

4. The coating for silver-plated bead tubes according to claim 3, characterized in that: The defoamer includes high molecular polymer SN-6788; and / or, the dispersant is a high molecular weight hyperdispersant containing a plurality of pigment-affinity groups; and / or, the substrate wetting agent comprises at least one of an organosilicon wetting agent and a fluorocarbon wetting agent; And / or, the leveling agent is a fluorine-modified acrylic leveling agent; And / or, the thickener is a polyurethane associative thickener that does not contain an organic solvent; And / or, the anti-settling agent is a water-based polyurea anti-settling agent; And / or, the pH regulator is a special organosilicon type pH regulator; and / or, the ultraviolet absorber comprises at least one of UV1130, RQT-X-1, 2-hydroxy-4-methoxydiphenylacetone-5-sulfonic acid and hydrophobic hydroxyphenyltriazine compounds; And / or, the brightener is a water-resistant blue macromolecular colorant; And / or, the cross-linking agent includes at least one of a metal ion cross-linking agent and a polycarbodiimide cross-linking agent; and / or, the adhesion promoter is an organosilane oligomer; And / or, the lubricant is oxidized polyethylene wax emulsion.

5. The coating for silver-plated bead tubes according to claim 4, characterized in that: The dispersant includes at least one of SN-1790A, SN-1760, COADIS 790 and COADIS 490; and / or, the silicone wetting agent includes at least one of WET 270, SN-4741 and Twin 4100, and the fluorocarbon wetting agent includes at least one of ZH-8004 and SN-4763; and / or, the leveling agent comprises at least one of AKN-1181, SN-3781 and ZH-8004; and / or, the thickener comprises at least one of FLUGO A3151 and Coapur XS83; and / or, the anti-settling agent comprises at least one of SN-9742 and F5715; And / or, the pH adjuster includes BS168; and / or, the preservative comprises at least one of BN-510 and RT-3318; and / or, the metal ion crosslinking agent comprises ZINPLEX 15; and / or, the polycarbodiimide type cross-linking agent comprises at least one of CARBODILITE E-02 and ACRAFIX FAC; and / or, the adhesion promoter comprises at least one of OS-79 and KRN8027; Preferably, in the substrate wetting agent, the mass ratio of the silicone wetting agent to the fluorocarbon wetting agent is 2:1; Preferably, in the cross-linking agent, the mass ratio of the metal ion cross-linking agent to the polycarbodiimide cross-linking agent is 1:

1.

6. A method for preparing a coating for silver-plated bead tubes as claimed in any one of claims 1 to 5, characterized in that: The method comprises the following steps: mixing the raw materials according to a proportion.

7. The preparation method according to claim 6, characterized in that: Deionized water, defoamer, dispersant, anti-settling agent, titanium dioxide, barium sulfate and mica powder are prepared into a pre-dispersed slurry; The pre-dispersed slurry is mixed with the aqueous polyurethane emulsion, the aqueous acrylic hardening emulsion and the aqueous polyurethane modified alkyd resin to obtain a first slurry; Mixing a substrate wetting agent, a leveling agent, a cross-linking agent, an adhesion promoter, an ultraviolet absorber, a preservative, a slip agent, and a whitening agent with the first slurry to obtain a second slurry; A pH adjuster and a thickener are mixed with the second slurry to obtain the coating.

8. The preparation method according to claim 7, characterized in that: The titanium dioxide, the barium sulfate and the mica powder are ground to a particle size not exceeding 20 micrometers, and then mixed with a mixed solution formed by deionized water, the defoamer, the dispersant and the anti-settling agent to obtain the pre-dispersed slurry.

9. An application of the coating for silver-plated bead tubes as claimed in any one of claims 1 to 5, characterized in that: The paint for the silver-plated bead tube is used for coating the inner surface of the silver-plated bead tube.

10. A silver-plated bead tube, characterized in that: The surface of the silver-plated bead tube has the coating for silver-plated bead tube according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Waterborne polyurethane elastic coating

    CN106221536A

  • Water-based matte white coating and preparation method thereof

    CN112063250A

  • Single-component air-drying water-based anticorrosive paint

    CN116731579A