Blast furnace gas dechlorination hydrolysis complexing agent and preparation method thereof
By using zinc oxide desulfurization waste slag, magnesium and other materials, the blast furnace gas dechlorination hydrolysis composite agent is solved, and the problem of difficult removal of hydrogen chloride and organic sulfur in blast furnace gas is achieved, efficient dechlorination and hydrolysis are achieved, and the catalyst life is extended. The green utilization of solid waste has been achieved.
Patent Information
- Application Number
- CN202411173614.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-15
AI Technical Summary
The existing blast furnace gas purification process is difficult to effectively remove hydrogen chloride and organic sulfur at the same time, resulting in a short life of dechlorination and hydrolysis catalysts, affecting the achievement of process stability and environmental protection indicators.
Develop a blast furnace gas dechlorination hydrolysis composite agent, and prepare a hydroxide-rich dechlorination hydrolysis composite agent by combining zinc oxide desulfurization waste slag, magnesium and calcium lime, and dechlorination and hydrolysis using alkaline active centers. It complements each other and improves the dechlorination accuracy and hydrolysis conversion rate.
It achieves efficient removal of hydrogen chloride and organic sulfur, extends the catalyst life, improves the dechlorination accuracy and hydrolysis conversion rate, reduces the impact of carbon dioxide on dechlorination, and realizes the comprehensive resource utilization of solid waste.
Smart Images

Figure CN118956459A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a blast furnace gas dechlorination hydrolysis composite agent and a preparation method thereof, belonging to the field of blast furnace gas purification. Background Art
[0002] Blast furnace gas is a by-product of the iron and steel metallurgical process. It has a large volume and low heat. Its main components are CO, N 2 and CO 2 , and also contains certain sulfides and HCl and other substances. The total sulfur content of blast furnace gas is about 60~300mg / Nm 3 Organic sulfur accounts for about 70% of the total sulfur content, mainly carbonyl sulfide, with trace amounts of methyl mercaptan and carbon disulfide. Inorganic sulfur accounts for about 30% of the total, with hydrogen sulfide H2S as the main component.
[0003] Blast furnace gas dry dust removal technology is one of the six major advanced technologies promoted by the steel industry. It has many advantages, such as high dust removal efficiency, low dust content in purified gas, full utilization of gas sensible heat, high TRT power generation, and almost no water consumption. However, dry dust removal technology is difficult to handle HCl and sulfide gas in blast furnace gas. These impurities cause corrosion of pipelines and equipment, salt accumulation, etc., reduce their service life, and even cause leakage risks; the flue gas produced by gas combustion is rich in sulfur dioxide, which seriously pollutes the surrounding environment.
[0004] At present, in the blast furnace gas dechlorination process, the chemical absorption method is the most common, which uses the acid-base neutralization reaction principle to react alkali metal and alkaline earth metal compounds with HCl to form corresponding salts. Patent CN104774654B discloses a method for using a blast furnace gas dechlorinating agent, which uses cheap industrial limestone, commercial sodium carbonate and potassium hydroxide as main raw materials, and a disc ball making machine is used for ball making. Patent CN114392643B discloses a method for preparing a blast furnace gas dechlorinating agent, using solid wastes such as blast furnace slag and / or steel slag as raw materials to prepare a dechlorinating agent. In recent years, due to the unsatisfactory industrial application accuracy of fixed bed dechlorinating agents, there has been a method of spraying alkali solution in the pipeline between gravity dust removal and bag dust removal, which is similar to the liquid phase dechlorination process. Its advantages are: first, the pipeline is used as a reactor; second, the generated chloride particles are removed by the bag dust collector; its disadvantages are also obvious: first, the temperature fluctuation range of blast furnace gas is large. When the alkali solution is sprayed at a temperature below 80°C, the liquid phase cannot be quickly vaporized, and the dust in the liquid and gas is mixed and attached to the inner wall of the pipeline, causing blockage; second, the water in the alkali solution evaporates, and the alkaline components will adhere to the inner wall of the pipeline and cause corrosion.
[0005] According to national environmental protection indicators, both organic sulfur and inorganic sulfur in blast furnace gas need to be removed so that the flue gas can meet ultra-low emission standards. 2The process of removing organic sulfur is relatively mature and has been applied in many industrial fields. To remove organic sulfur, it is generally catalytically converted into inorganic sulfur before removal. The main organic sulfur in blast furnace gas is carbonyl sulfide, which has stable chemical properties and is not easy to remove. It needs to be converted into hydrogen sulfide before removal. The conversion of carbonyl sulfide can be divided into two ways: hydrogenation and hydrolysis. The hydrogenation process is usually carried out at 350-400°C, which will increase energy consumption and the operating cost is too high. It is not suitable for blast furnace gas purification. The hydrolysis process is that COS reacts with H 2 O reacts to convert into H 2 S. Reaction equation: COS+H 2 O=H 2 S+CO 2 The reaction temperature is low, and more than 90% of COS can be converted into H at 60°C. 2 S, 90℃ conversion rate exceeds 95%. Patent CN114471522A discloses a high specific surface area anti-poisoning blast furnace gas hydrolysis catalyst and its preparation method. The invention uses γ-alumina as a carrier, alkali metal oxides as active ingredients, rare earth metal oxides as additives, adds a variety of pore-forming agents, and ammonia water as a precipitant. After precipitation, standing, drying, grinding, and calcination, a COS hydrolysis catalyst is obtained. Patent CN118105979A discloses a ternary catalyst for hydrolysis of carbonyl sulfide, its preparation method and application. The invention obtains a ternary catalyst composed of Ni, Cu, and Fe by coprecipitation, which can be used for hydrolysis of carbonyl sulfide in blast furnace gas.
[0006] The residual oxygen in blast furnace gas will react with hydrogen sulfide to form elemental sulfur or sulfite, resulting in a decrease in the number of hydrolysis alkaline centers and slow deactivation. 2 O 3 ,γ-Al 2 O 3 MgAl 2 O 4 、Ti / Al 2 O 3 、V / Al 2 O 3 、TiO 2 However, the application status in blast furnace gas is not satisfactory. The main reason is that the composition and temperature of blast furnace gas fluctuate greatly. Not only oxygen and hydrogen sulfide, but also sulfur dioxide will aggravate sulfation and cause the life of the hydrolysis catalyst to fail to reach the ideal design value.
[0007] At present, the purification process of blast furnace gas often uses gravity dust removal, bag dust removal, dechlorination, organic sulfur hydrolysis, TRT power generation, and inorganic sulfur removal. The design concept is to remove hydrogen chloride in the gas phase, avoid the alkaline active center of the hydrolysis agent being consumed by acid, and ensure the service life of the hydrolysis catalyst. However, there is oxygen and sulfur dioxide in the gas phase, which will cause sulfate poisoning of the hydrolysis catalyst and reduce its activity, and the service life is less than the design value of 1 year. The life of the dechlorination agent is different from that of the hydrolysis agent, resulting in frequent shutdown of the dechlorination and hydrolysis towers for agent replacement, affecting normal production.
[0008] Therefore, the development of a blast furnace gas dechlorination and hydrolysis composite agent can not only remove the acidic gas hydrogen chloride, but also hydrolyze the organic sulfur into inorganic sulfur, which is of great significance for blast furnace gas purification. Brucite is a layered hydroxide with a theoretical MgO content of 69.12%. It is the mineral with the highest known magnesium content. The main mineral component is Mg(OH) 2 , so it is also called magnesite. Brucite is mainly used to produce refractory materials and thermal insulation materials with low added value and flame retardants with high added value. Develop the technology of preparing dechlorination agent with magnesite and expand its high added value utilization. The main components of zinc oxide desulfurization slag are zinc sulfide and unreacted zinc oxide, with a zinc content of >60%. The regeneration process includes roasting desulfurization and reprocessing of desulfurization materials, which consumes a lot of energy. The use of zinc oxide desulfurization slag and calcium hydroxide, two industrial solid wastes, to prepare dechlorination agents can realize the desire of treating waste with waste, comprehensive utilization of resources, and green development. Summary of the invention
[0009] Based on the above defects of the prior art and the problems existing in the current blast furnace gas purification, the present invention proposes a blast furnace gas dechlorination and hydrolysis composite agent and its preparation method. Dechlorination and hydrolysis complement each other. The hydroxide of the dechlorination active component provides an alkaline environment for the organic sulfur catalytic hydrolysis reaction, which is beneficial to the hydrolysis conversion rate; the strong base at the hydrolysis active center can improve the dechlorination accuracy.
[0010] The specific implementation is through the following technical solutions: S1. Add solution A to the reactor, then slowly add 200 mesh zinc oxide desulfurization agent waste residue, stir and react at 50°C for 4-8 hours, let stand for 24 hours, filter, wash, and obtain zinc liquid and filter residue; the solution A is a hydrogen peroxide-sulfuric acid solution, wherein the mass concentration of hydrogen peroxide is 1-5%, and the mass concentration of sulfuric acid is 11-14%; wherein the mass ratio of zinc oxide desulfurization waste residue to hydrogen peroxide-sulfuric acid solution is 1:8-10.
[0011] S2, the filter residue is dried, and roasted at 350-400°C for 2h in a rotary kiln or a tubular furnace with continuous air flow to obtain crude zinc, which is transferred to the solution A of S1 for dissolution; the roasting tail gas is washed with an absorption liquid B to obtain a tail absorption liquid C; the absorption liquid B is an aqueous solution with a mass concentration of hydrogen peroxide of 8%; the tail absorption liquid C is used to prepare the hydrogen peroxide solution A.
[0012] S3 and brucite were crushed to 200 mesh, calcined at 400°C for 1-3h, slowly added into water with stirring for hydrothermal reaction, and then slowly added into zinc solution of S1, and stirred continuously for 4h to obtain zinc-magnesium slurry; the mass ratio of brucite to zinc oxide desulfurization waste residue in S1 was 3:4.
[0013] S4, zinc-magnesium slurry is cooled to room temperature, calcium carbonate is added, and the solidification reaction is carried out for 8 hours; then a flocculant is added, stirred for 5 minutes, aged for 24 hours, filtered and dried to obtain alkali powder I and filtrate D; the mass ratio of flocculant to calcium carbonate is 1-2:50; the mass ratio of calcium carbonate to zinc oxide desulfurization waste residue in S1 is 13:4; filtrate D is used for the hydrothermal reaction of S3.
[0014] S5. Activated carbon powder and alumina powder are mixed evenly, and an equal amount of them are used to impregnate a mixed solution of potassium carbonate and sodium molybdate, and then dried to obtain alkali powder II; the alumina powder is a fast-de-powdering powder, and the mass ratio of activated carbon powder, fast-de-powdering powder, potassium carbonate and sodium molybdate is 1:3:1:0.1.
[0015] S6, alkali powder I and alkali powder II are mixed evenly, extruded into strips, and dried at 80° C. to obtain a dechlorination and hydrolysis composite agent; the mass ratio of the alkali powder I to the alkali powder II is 7:3.
[0016] Specifically, calcium sulfate, aluminum oxide, and activated carbon are carriers; zinc hydroxide, magnesium hydroxide, calcium hydroxide, and iron hydroxide are dechlorination active ingredients; potassium carbonate is a hydrolysis active center; and sodium molybdate is an anti-sulfation ingredient.
[0017] Specifically, zinc hydroxide, ferric hydroxide and calcium sulfate are produced by the coprecipitation of zinc sulfate, ferric sulfate and calcium hydroxide; magnesium hydroxide is produced by the hydration reaction of magnesium oxide and water.
[0018] Furthermore, the zinc oxide desulfurization waste residue in S1 is zinc sulfide waste residue generated by the dry removal of hydrogen sulfide by zinc oxide, and its main components are zinc sulfide and unreacted zinc oxide.
[0019] Furthermore, the flocculant in S4 is aluminum ferrous sulfate flocculant.
[0020] Furthermore, the mass ratio of zinc oxide desulfurization waste residue, brucite and calcium carbonate is 4:3:13.
[0021] Compared with the prior art, the present invention has the following significant advantages: 1. The composite agent can both dechlorinate and catalyze the hydrolysis of organic sulfur. Both dechlorination and hydrolysis utilize alkaline active centers. The dechlorination process consumes alkaline centers, while the hydrolysis process is a catalytic process and does not consume alkaline centers. The dechlorination process is an acid-base reaction adsorption process, and hydrogen chloride generates chloride adsorbed on the composite agent; while the organic sulfur hydrolysis process is a catalytic process, and carbonyl sulfide and carbon disulfide are adsorbed in the micropores of the composite agent, and hydrogen sulfide is generated under the action of alkaline catalysis and desorbed back to the gas phase. Zinc hydroxide, magnesium hydroxide, and iron hydroxide are weak bases, and calcium hydroxide is a strong base. They can not only remove hydrogen chloride and sulfur dioxide in the gas phase, but also provide a stronger alkaline environment for the hydrolysis of potassium carbonate and sodium molybdate active centers, which is beneficial to improve the hydrolysis conversion efficiency; at the same time, potassium carbonate is a strong base, and the reaction rate with hydrogen chloride is fast, which improves the dechlorination accuracy. The dechlorination active ingredients and the hydrolysis active centers work together to effectively improve the dechlorination accuracy and hydrolysis conversion rate.
[0022] 2. Protect the alkaline hydrolysis center and resist sulfation deactivation. Catalysts with alkali as the hydrolysis active center system will inevitably be sulfated in oxygen-containing blast furnace gas. The large amount of hydroxide contained in the composite agent can effectively adsorb the sulfate ions generated by sulfation, protect the potassium carbonate active center, and avoid acidification deactivation. Sodium molybdate can effectively inhibit the sulfation of the hydrolysis center and slow down the deactivation rate of the hydrolysis active center, thereby increasing the life of the hydrolysis catalyst.
[0023] 3. It can inhibit the effect of carbon dioxide on the dechlorination agent, and the dechlorination accuracy is high. The purification process of hydrogen chloride is an acid-base reaction. Conventional alkaline earth metal oxide dechlorination agents use calcium oxide, calcium hydroxide or calcium carbonate as the main active ingredients. The reaction rate of calcium oxide and calcium carbonate with hydrogen chloride is lower than the reaction rate of calcium hydroxide with hydrogen chloride, so the dechlorination accuracy and chlorine capacity are poor. Blast furnace gas contains hydrogen chloride and a large amount of carbon dioxide. The reaction of the two with calcium hydroxide is in a competitive relationship, and the concentration of carbon dioxide is much higher than that of hydrogen chloride. Calcium hydroxide is an active component that easily generates calcium carbonate or calcium bicarbonate, so the calcium hydroxide dechlorination agent has high dechlorination accuracy in the early stage, and the accuracy will decrease in the later stage. The dechlorination hydrolysis composite agent prepared by this technical solution is rich in zinc hydroxide, magnesium hydroxide, and iron hydroxide. At 60~200℃, in blast furnace gas with high water vapor content, it will not react with carbon dioxide, and as the temperature increases, the basic carbonate will hydrolyze into hydroxide, so it can effectively inhibit the effect of carbon dioxide on dechlorination. The active components work synergistically to achieve high dechlorination accuracy, and the outlet hydrogen chloride is less than 0.1mg / m 3 .
[0024] 4. Comprehensively utilize solid waste, treat waste with waste, and make green comprehensive utilization; use cheap and readily available mineral raw materials to expand their industrial high-value uses. Make full use of the zinc and sulfur elements in zinc oxide desulfurization waste residue, zinc becomes a dechlorination active ingredient, and sulfur becomes a calcium sulfate carrier. Brucite is a layered hydroxide with a hard texture and a small specific surface area. Through heating decomposition and hydrothermal activation, its porosity is increased, making it an excellent dechlorination active component. In addition, the entire preparation process does not discharge wastewater and harmful substances, which is green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a process flow chart for the preparation of dechlorination hydrolysis composite agent.
[0026] Figure 2 This is a flow chart for the evaluation of organic sulfur catalytic hydrolysis and sulfation resistance of dechlorination hydrolysis composite agents. DETAILED DESCRIPTION
[0027] The present invention is described in detail below with reference to the examples. The examples are only preferred embodiments of the present invention and are not intended to limit the present invention.
[0028] Example 1 S1. Prepare a hydrogen peroxide-sulfuric acid solution A with a hydrogen peroxide mass concentration of 4% and a sulfuric acid mass concentration of 14%; weigh 32 kg of solution A, slowly add 4 kg of 200 mesh zinc oxide desulfurization waste residue, stir and react at 50°C for 8 hours, let stand for 24 hours, filter, wash, and obtain zinc solution and filter residue.
[0029] S2, prepare an aqueous solution with a mass concentration of 8% of hydrogen peroxide as absorption liquid B; dry the filter residue of S1, and roast it at 350°C for 2 hours in a rotary kiln with continuous air flow to obtain crude zinc; wash the roasting tail gas with absorption liquid B to obtain tail absorption liquid C.
[0030] S3, 3kg brucite was crushed to 200 mesh, calcined at 400°C for 1h, slowly added into water with stirring for hydrothermal reaction, then slowly added into the zinc solution of S1, and continued stirring for 4h to obtain zinc-magnesium slurry.
[0031] S4, the zinc-magnesium slurry is cooled to room temperature, 13kg of calcium carbonate is added, and the solidification reaction is carried out for 8h; then 0.26kg of aluminum ferrous sulfate flocculant is added, stirred for 5min, aged for 24h, filtered and dried to obtain alkali powder I and filtrate D; S5, weigh 18kg water, add 10kg potassium carbonate and stir until completely dissolved, then add 100g sodium molybdate and stir until completely dissolved, then add 10kg activated carbon powder and 30kg quick-de-powder mixed powder, mix well, seal and stuff until the liquid is completely absorbed, and dry to obtain alkali powder II; S6, 7kg alkali powder I and 3kg alkali powder II were mixed evenly, extruded into strips, and dried at 80°C to obtain the dechlorination and hydrolysis composite agent W1.
[0032] Comparative Example 1 This comparative example provides a dechlorination and hydrolysis composite agent, which is simply the dechlorination and hydrolysis composite agent W1 obtained in step S6 of Example 1 calcined at 350°C for 3h to decompose the zinc hydroxide, magnesium hydroxide and iron hydroxide therein into corresponding zinc oxide, magnesium oxide and iron oxide to obtain the dechlorination and hydrolysis composite agent D1.
[0033] Comparative Example 2 This comparative example provides a dechlorination and hydrolysis composite agent, which is simply obtained by directly extruding the alkali powder I obtained in step S4 of Example 1 into strips, and drying at 80° C. to obtain the dechlorination and hydrolysis composite agent D2.
[0034] Comparative Example 3 This comparative example provides a dechlorination and hydrolysis composite agent, which is obtained by directly extruding the alkali powder II obtained in step S5 of Example 1 into strips and drying at 80°C to obtain the dechlorination and hydrolysis composite agent D3.
[0035] Comparative Example 4 This comparative example provides a dechlorination and hydrolysis composite agent, which is obtained by removing the sodium molybdate in step S5 of Example 1 and the remaining steps are the same as those of Example 1 to obtain a dechlorination and hydrolysis composite agent D4.
[0036] Example 2 S1. Use the tail absorption liquid C obtained in step S2 of Example 1 to prepare a hydrogen peroxide-sulfuric acid solution A with a hydrogen peroxide mass concentration of 5% and a sulfuric acid mass concentration of 11%; weigh 40 kg of solution A and add it to a reactor, then add 4 kg of zinc oxide desulfurization waste residue and the crude zinc obtained in step S2 of Example 1, stir the reaction at 50° C. for 4 h, let it stand for 24 h, filter, and wash to obtain zinc liquid and filter residue.
[0037] S2. The filter residue is dried and roasted in a rotary kiln with continuous air flow at 400° C. for 2 h to obtain crude zinc; the roasting tail gas is washed with absorption liquid B to obtain tail absorption liquid C.
[0038] S3, 3 kg of brucite was crushed to 200 mesh, calcined at 400° C. for 3 h, and slowly added to the mixture of filtrate D obtained in step S4 of Example 1 and water under stirring for hydrothermal reaction, and then slowly added with zinc solution in S1, and continued stirring for 4 h to obtain zinc-magnesium slurry.
[0039] S4. The zinc-magnesium slurry was cooled to room temperature, and 13 kg of calcium carbonate was added to solidify the slurry for 8 h. Then 0.52 kg of aluminum ferrous sulfate flocculant was added, stirred for 5 min, and aged for 24 h. The slurry was filtered and dried to obtain alkali powder I and filtrate D.
[0040] S6, 7 kg of alkali powder I and 3 kg of alkali powder II obtained in step S5 of Example 1 were mixed evenly, extruded into strips, and dried at 80°C to obtain the dechlorination and hydrolysis composite agent W2.
[0041] Example 3 Steps S1 to S4 of Example 1 were repeated multiple times, and the tail aspirate C and crude zinc were collected in step S2; and the filtrate D was collected in step S4.
[0042] S1. Use the tail aspiration liquid C collected multiple times to prepare a hydrogen peroxide-sulfuric acid solution A with a hydrogen peroxide mass concentration of 1% and a sulfuric acid mass concentration of 13%; weigh 36 kg of solution A and add it to the reactor, then add 4 kg of crude zinc collected multiple times, stir and react at 50° C. for 6 hours, and all the crude zinc solids are dissolved.
[0043] S3, 3kg brucite was crushed to 200 mesh, calcined at 400°C for 2h, and slowly added with stirring the filtrate D collected multiple times for hydrothermal reaction, and then slowly added with the zinc solution in S1, and continued stirring for 4h to obtain zinc-magnesium slurry.
[0044] S4. The zinc-magnesium slurry was cooled to room temperature, 13 kg of calcium carbonate was added, and the solidification reaction was carried out for 8 hours. Then 0.4 kg of aluminum ferrous sulfate flocculant was added, stirred for 5 minutes, and aged for 24 hours. Then, the slurry was filtered and dried to obtain alkali powder I and filtrate D.
[0045] S6, 7 kg of alkali powder I and 3 kg of alkali powder II obtained in step S5 of Example 1 were mixed evenly, extruded into strips, and dried at 80°C to obtain the dechlorination and hydrolysis composite agent W3.
[0046] Analysis example 4 In order to compare the effects of the dechlorination and hydrolysis composite agents of the embodiment and the comparative example on the catalytic hydrolysis of organic sulfur and the resistance to sulfation, a simulated hydrolysis test was conducted using the dechlorination and hydrolysis composite agents prepared in the embodiment and the comparative example, respectively. The specific test steps are as follows: Mixed gas composition: carbon dioxide 10%, carbon monoxide 30%, hydrogen 5%, carbonyl sulfide 1000mg / Nm 3 (in terms of S), and the rest is nitrogen. In a fixed bed reactor, the catalytic hydrolysis of organic sulfur and the sulfate resistance are carried out by placing a quartz tube reaction tube with an inner diameter of 1 cm in a vertical furnace and heating it. The reaction temperature and space velocity are 2000h -1 The evaluation was conducted at 80°C and atmospheric pressure. The temperature was controlled and indicated by a programmable temperature controller. The sample was a 20-40 mesh granular catalyst, filled with 3 mL. The evaluation process is as follows: Figure 2 shown.
[0047] In the test of catalytic hydrolysis of organic sulfur, the mixed gas enters the mixer after the flow rate is regulated by the liquid level flowmeter, and then enters the water saturator controlled by the constant temperature water bath to bring water vapor into the reaction atmosphere; the water vapor saturated mixed gas enters the fixed bed reactor, and COS reacts with water to generate H under the action of the catalyst. 2 S and CO 2 The tail gas is discharged after alkaline washing. The reactor is inlet and outlet at the top and bottom, and there are gas sampling ports at the upper and lower ends. The inlet and outlet concentrations of COS and the hydrolysis product H are detected by a trace sulfur gas chromatograph. 2 The outlet concentration of S (measured in S). In the initial stage of the catalytic reaction, the alkaline center has a certain adsorption effect on hydrogen sulfide gas, so the inlet and outlet COS is used as the detection index. The test results are shown in Table 1.
[0048] Table 1 Results of catalytic hydrolysis conversion of organic sulfur
[0049] It can be seen from W1 / W2 / W3 in Table 1 that the three have comparable catalytic hydrolysis activities for organic sulfur, and the conversion rates are all >99%, indicating that the dechlorination hydrolysis composite agent prepared by this technical solution has excellent catalytic hydrolysis activity for organic sulfur. The main components of D1 are oxides, potassium carbonate, and sodium molybdate, and the hydrolysis conversion rate is 75.4%; the main components of D2 are hydroxides, which have certain hydrolysis activity and a hydrolysis conversion rate of 43.8%; D3 is a hydrolysis component mainly composed of potassium carbonate, sodium molybdate, aluminum oxide, and activated carbon, and has relatively excellent catalytic hydrolysis activity for organic sulfur, with a conversion rate of 95.4%; W1 / W2 / W3 is a composite agent in which D2 and D3 are mixed in a certain proportion, and has excellent catalytic hydrolysis activity for organic sulfur, indicating that the components of D2 and D3 have a synergistic effect on the hydrolysis of organic sulfur and improve the hydrolysis activity. It can be seen from W1 / D2 / D3 that the catalytic hydrolysis activity of organic sulfur among the three is W1>D3>D2, indicating that hydroxide can promote the hydrolysis of organic sulfur and improve the conversion rate of carbonyl sulfide. After calcination of W1, the hydroxide was decomposed into oxides, and the hydrolysis activity decreased compared with W1, which confirmed that the hydroxide was beneficial to the hydrolysis of organic matter.
[0050] Sulfate resistance test, mixed gas + 1.5% oxygen. During the test, the mixed gas and oxygen are regulated by the liquid level flowmeter and then enter the mixer to achieve full mixing of the gas; then enter the water saturator controlled by the constant temperature water bath to bring water vapor into the reaction atmosphere; the water vapor saturated mixed gas enters the fixed bed reactor, and COS reacts with water under the action of the catalyst to generate H 2 S and CO 2 The tail gas is discharged after alkaline washing. The reactor is inlet and outlet at the top and bottom, and there are gas sampling ports at the upper and lower ends. The inlet and outlet concentrations of COS and the hydrolysis product H are detected by a trace sulfur gas chromatograph. 2The outlet concentration of S (in terms of S). The carbonyl sulfide conversion rate and the amount of sulfate and sulfite in the fixed bed after 96 hours were analyzed over a long period of time. The test results are shown in Table 2.
[0051] Table 2 Results of sulfation resistance of organic sulfur catalytic hydrolysis
[0052] It can be seen from the data in Table 2 that the hydrolysis activity decreased with the reaction time; the activity of W1 / W2 / W3 / D1 / D3 decreased in the early stage and stabilized in the later stage; the activity of D2 / D4 continued to decrease until it was inactivated. Sodium molybdate was added to W1 / W2 / W3 / D1 / D3, but not to D4. After 96 hours, the sulfate and sulfite in the D4 bed were significantly higher than those in W1 / W2 / W3 / D1 / D3, and the hydrolysis activity of D4 continued to decay, indicating that sodium molybdate has certain anti-sulfation properties.
[0053] Analysis example 5 In order to compare the dechlorination effects of the dechlorination hydrolysis composite agents of the embodiment and the comparative example, the dechlorination test was simulated on the dechlorination hydrolysis composite agents prepared in the embodiment and the comparative example respectively according to the standard GB / T38108-2019 "Test method for chlorine capacity of alkaline earth metal high temperature dechlorination agent".
[0054] In order to be closer to the actual working conditions, the national standard raw gas was changed to a mixed gas, which consists of 10% carbon dioxide, 30% carbon monoxide, 5% hydrogen, and the rest is nitrogen. Test conditions, air velocity 2000h -1 , temperature 100℃, normal pressure, inlet hydrogen chloride content 2000mg.Nm -3 During the test, sodium hydroxide solution was used to absorb the tail gas, and then the chlorine content in the absorption liquid was detected by microcoulometric method, and the content of hydrogen chloride in the tail gas could be calculated. 3 When the outlet hydrogen chloride concentration is greater than 1000mg / m 3 The chlorine capacity test results are shown in Table 3.
[0055] Table 3 Dechlorination results of dechlorination hydrolysis composite agent
[0056] As can be seen from Table 3, W1 / W2 / W3 have high penetration chlorine capacity and saturated chlorine capacity, and good dechlorination accuracy and activity. D1 is mainly composed of oxides, and its penetration chlorine capacity is 50% lower than that of W1 / W2 / W3, indicating that the dechlorination activity of hydroxides is better than that of oxides. The outlet hydrogen chloride concentration of D2 is 0.89 mg.m -3, the penetration chlorine capacity is low at only 9.2%, and the saturated chlorine capacity is high at 45.8%. Compared with W1 / W2 / W3, it shows that D2 has poor dechlorination accuracy and equivalent chlorine capacity. The penetration chlorine capacity and saturated chlorine capacity of D3 are both very low, but the dechlorination accuracy is higher. The difference between the penetration chlorine capacity and the saturated chlorine capacity is small at only 0.3%, that is, the penetration is close to saturation. D2 and D3 are prepared according to a certain ratio W1 / W2 / W3. W1 / W2 / W3 not only reflects the advantages of D2, high chlorine capacity, but also reflects the advantages of D3, high precision, indicating that the hydroxide chlorine capacity is high and potassium carbonate has good dechlorination precision. The dechlorination performance of D4 is equivalent to that of W1 / W2 / W3, indicating that sodium molybdate has no effect on dechlorination.
[0057] Analysis example 6 In order to verify the effect of carbon dioxide on dechlorination, pure carbon dioxide gas was first introduced into the W1 / W2 / W3 / D1 bed until it no longer absorbed carbon dioxide. The specific operation was to replace the raw gas in GB / T 38108-2019 "Test Method for Chlorine Capacity of Alkaline Earth Metal High-Temperature Dechlorination Agent" with carbon dioxide, and replace the hydrogen chloride generator with a saturated water generator. After the bed no longer absorbed carbon dioxide, the chlorine capacity was continued to be evaluated according to the analysis method of Analysis Example 5. The chlorine capacity evaluation results are shown in Table 4.
[0058] Table 4 Dechlorination results of dechlorination hydrolysis composite agent after carbon dioxide saturation
[0059] From the comparison of Table 3 and Table 4, it can be seen that the outlet hydrogen chloride, breakthrough chlorine capacity and saturated chlorine capacity of W1 / W2 / W3 changed little before and after carbon dioxide saturation, indicating that carbon dioxide had no effect on W1 / W2 / W3; after carbon dioxide saturation, the outlet hydrogen chloride of D1 increased, and the breakthrough chlorine capacity and saturated chlorine capacity dropped sharply, indicating that carbon dioxide had a great influence on the dechlorination performance of D1. Comparing W1 / W2 / W3 with D1, the main components of W1 / W2 / W3 are zinc hydroxide, magnesium hydroxide, iron hydroxide and calcium hydroxide, while D1 is zinc oxide, magnesium oxide, iron oxide and calcium hydroxide. It can be seen that zinc hydroxide, magnesium hydroxide and iron hydroxide can effectively inhibit the influence of carbon dioxide on dechlorination and improve dechlorination performance.
[0060] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention.
Claims
1. A blast furnace gas dechlorination hydrolysis composite agent and its preparation method, It is characterized in that Zinc hydroxide, magnesium hydroxide, calcium hydroxide, ferric hydroxide, potassium carbonate, and sodium molybdate are active ingredients, and calcium sulfate, aluminum oxide, and activated carbon are carriers; zinc hydroxide, magnesium hydroxide, calcium hydroxide, and ferric hydroxide are dechlorination centers, which can not only dechlorinate, but also provide an alkaline environment for hydrolysis and conversion; potassium carbonate is an organic sulfur hydrolysis center, which can catalyze the hydrolysis of organic sulfur and also react with hydrogen chloride to improve the dechlorination accuracy; The preparation method thereof comprises the following steps: S1. Add solution A to the reactor, then slowly add 200 mesh zinc oxide desulfurizer waste residue, stir at 50°C for 4 to 8 hours, let stand for 24 hours, filter, wash, and obtain zinc solution and filter residue; The solution A is a hydrogen peroxide-sulfuric acid solution, wherein the mass concentration of hydrogen peroxide is 1-5%, and the mass concentration of sulfuric acid is 11-14%; wherein the mass ratio of zinc oxide desulfurizer waste residue to solution A is 1:8-10; S2. The residue is dried and roasted in a rotary kiln or a tubular furnace with continuous air flow at 350 to 400 ° C for 2 h to obtain crude zinc, which is dissolved in solution A of step S1; the roasting tail gas is washed with an absorbing liquid B to obtain a tail absorbing liquid C; The absorption liquid B is an aqueous solution with a mass concentration of 8% hydrogen peroxide; the tail absorption liquid C is used to prepare solution A; S3. The brucite was crushed to 200 mesh, calcined at 400°C for 1-3h, slowly added to water under stirring for hydrothermal reaction, and then slowly added with zinc solution in step S1, and stirred for 4h to obtain zinc-magnesium slurry; the mass ratio of brucite to zinc oxide desulfurization agent waste residue in step S1 was 3:4; S4. The zinc-magnesium slurry is cooled to room temperature, and calcium carbonate is added to solidify for 8 hours; then a flocculant is added, stirred for 5 minutes, aged for 24 hours, filtered and dried to obtain alkali powder I and filtrate D; the mass ratio of flocculant to calcium carbonate is 1-2:50; the mass ratio of calcium carbonate to zinc oxide desulfurization agent waste residue in step S1 is 13:4; filtrate D is used for the hydrothermal reaction in step S3; S5. The activated carbon powder and the alumina powder are mixed, and an equal amount of potassium carbonate and sodium molybdate mixed solution is used for impregnation and drying to obtain alkali powder II; the alumina powder is a fast-de-powdering powder, and the mass ratio of the activated carbon powder, the fast-de-powdering powder, potassium carbonate and sodium molybdate is 1:3:1:0.1; S6. Alkali powder I and alkali powder II are mixed, extruded into strips, and dried at 80° C. to obtain a dechlorination and hydrolysis composite agent; the mass ratio of the alkali powder I to the alkali powder II is 7:
3.
2. A blast furnace gas dechlorination and hydrolysis composite agent and a preparation method thereof according to claim 1, Features: Calcium sulfate, aluminum oxide, and activated carbon are carriers; zinc hydroxide, magnesium hydroxide, calcium hydroxide, and ferric hydroxide are dechlorination active ingredients; potassium carbonate is a hydrolysis active center; and sodium molybdate is an anti-sulfation ingredient.
3. A blast furnace gas dechlorination and hydrolysis composite agent and a preparation method thereof according to claim 1, It is characterized in that Zinc hydroxide, ferric hydroxide and calcium sulfate are produced by the coprecipitation of zinc sulfate, ferric sulfate and calcium hydroxide; magnesium hydroxide is produced by the hydrothermal reaction of magnesium oxide and water.
4. A blast furnace gas dechlorination and hydrolysis composite agent and a preparation method thereof according to claim 1, Features The zinc oxide desulfurization agent waste residue in step S1 is zinc sulfide waste residue generated by removing hydrogen sulfide from zinc oxide by dry method, and its main components are zinc sulfide and unreacted zinc oxide.
5. A blast furnace gas dechlorination and hydrolysis composite agent and a preparation method thereof according to claim 1, Features The flocculant in step S4 is aluminum ferrous sulfate.
6. A blast furnace gas dechlorination and hydrolysis composite agent and a preparation method thereof according to claim 1, Features The mass ratio of zinc oxide desulfurizer waste residue, brucite and calcium carbonate is 4:3:13.
Citation Information
Cited By
Preparation method of high-BET calcium hydroxide and activated carbon supported composite desulfurizer