Preparation method and application of steady-state modified lime powder for molten iron pretreatment
By pretreating stearic acid with nano-alumina, sodium silicate and borax are added to form a steady-state modification enhancer and quicklime powder, the problem of quicklime being susceptible to moisture is solved, and the stability and efficiency of molten iron pretreatment are improved. It enhances the ability to remove impurities from molten iron and achieves more efficient steel production.
Patent Information
- Application Number
- CN202410985848.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-15
AI Technical Summary
Quicklime is prone to moisture during pneumatic conveying, resulting in a degradation of performance, affecting the stability and efficiency of molten iron pretreatment. The existing steady-state modification process has a long construction period and average effect, which cannot meet the efficient demand for steel production.
By pretreating stearic acid with nano-alumina, sodium silicate and borax are added to form a steady-state modification enhancer and mixed with quicklime powder to improve its moisture resistance and fluidity, form a stable protective layer, and improve pneumatic conveying efficiency and ability to remove impurities from molten iron.
It significantly improves the stability and pneumatic conveying efficiency of quicklime powder, extends its service life, enhances the ability to remove impurities of molten iron, improves the efficiency of desulfurization, dephosphorization and desiliconization, extends the life of the furnace lining, and supports the sustainable development of the steel industry. develop.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of molten iron pretreatment, and particularly relates to a preparation method and application of a stable modified lime powder for molten iron pretreatment. Background Art
[0002] In order to improve the chemical composition of molten iron, reduce the impurity content and improve the quality of molten iron, the molten iron is pretreated. Through molten iron pretreatment technology, the quality of steel products can be significantly improved, energy consumption and environmental pollution can be reduced.
[0003] At present, the main domestic hot metal pretreatment processes are the injection method and the KR stirring method. Among them, the injection method uses gas to transport the desulfurization powder into the hot metal tank to react with the sulfur in the hot metal, and the reaction product is removed by slag removal, thereby achieving the purpose of hot metal desulfurization. Due to the good desulfurization effect of the injection method hot metal desulfurization process, many steel mills have been widely used.
[0004] The Ca-Mg composite rapid injection desulfurization process uses steady-state modified quicklime powder to transport steady-state modified magnesium particles through pipelines to the molten iron tank for desulfurization reaction, thereby achieving a process for removing impurities from the molten iron. It is a further optimization of the traditional injection method. Its characteristics are that the ratio of desulfurization powder can be flexibly adjusted according to the needs of the site, low powder consumption, stable control, less splashing, less slag, less iron loss, and good desulfurization effect. At present, Jiugang adopts the Ca-Mg composite rapid injection desulfurization process. As the calcium component of the Ca-Mg composite rapid injection powder, quicklime is crucial to the function of the molten iron pre-desulfurization system in terms of moisture resistance, hydrophobicity, dispersion, and flowability. However, the problem that quicklime is easily affected by moisture during pneumatic transportation brings a series of challenges to the molten iron pretreatment process. The water absorption characteristics of quicklime make it easy to absorb moisture in the air during transportation, storage and use, resulting in product performance degradation and deterioration. Especially in the injection method and its improved technology, the hygroscopic phenomenon of quicklime has a negative impact on the fluidity, stability and desulfurization efficiency of gas transportation.
[0005] Quicklime is easy to clump or scale in the pipeline, which not only affects the continuity and stability of pneumatic conveying; moisture absorption will also cause the quicklime powder to adhere and solidify, increasing the difficulty of cleaning pipelines and equipment and reducing production efficiency; in addition, moisture absorption may also cause the quicklime to block and clump, and even cause equipment damage and shutdown, which brings great instability to the production process. At the same time, other methods of stable modification of quicklime have a long construction period and general effect, which cannot meet the demand for both work efficiency and effect. In industrial production, the time required for the stable modification enhancer to complete the reaction with quicklime is usually within a few minutes to more than ten minutes. This ensures that the operation process will not be delayed. Moreover, there is no need for additional external conditions, such as high temperature, high pressure, etc. The steady-state modification process can be completed at room temperature and pressure. The rapidly generated steady-state modified product can form a stable protective layer on the surface of quicklime to prevent further reaction, ensure that the quicklime remains stable during storage and use, and further enhance its effect. At the same time, the products generated by the reaction of the above-mentioned steady-state modifiers with quicklime (such as calcium phosphate, calcium carbonate, calcium borate, calcium silicate, etc.) are all common components in the metallurgical process. Most of them form slag, help remove impurities in molten iron or form furnace walls, effectively extend the life of the furnace lining, or decompose into harmless components (stearic acid C 17 H 35 COOH decomposes into acids, aldehydes and other substances at 220℃, so it will not introduce harmful impurities into the subsequent steel production process. Solving this technical problem is crucial to further improve the molten iron pretreatment technology. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a preparation method and application of a steady-state modified lime powder for molten iron pretreatment in view of the deficiencies of the above-mentioned prior art. The method improves the moisture resistance and fluidity of quicklime through steady-state modification treatment, improves the stability of the product and the efficiency of pneumatic conveying. At the same time, the ability of quicklime to remove impurities in molten iron is further enhanced. This innovative technology can not only effectively solve the actual production problems in the molten iron pretreatment process, but also provide important support for the sustainable development of the steel industry.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a stable modified lime powder for molten iron pretreatment, the method comprising:
[0008] S1, grinding quicklime into powder to obtain quicklime powder;
[0009] S2. Pretreatment of nano-alumina:
[0010] Dissolve stearic acid in ethanol, then add nano-alumina, stir, continue stirring at a temperature of 70°C to 80°C for 2h to 3h, remove suspended matter after standing, retain precipitated matter, dry at 100°C, grind and disperse the agglomerated part after drying, and obtain pretreated nano-alumina;
[0011] S3, adding sodium silicate and borax to the pretreated nano-alumina obtained in S2 while continuing to grind, to obtain a stable modified enhancer;
[0012] S4. Add the stable modified reinforcing agent obtained in S3 to the quicklime powder obtained in S1, mix and grind at a temperature of 60° C. to 90° C., and sieve to obtain stable modified lime powder for molten iron pretreatment.
[0013] Preferably, the quicklime powder in S1 has a particle size of 60 mesh accounting for more than 98%.
[0014] Preferably, the mass ratio of stearic acid to nano-alumina in S2 is 1:10.
[0015] Preferably, the drying temperature in S2 is 100°C.
[0016] Preferably, the mass ratio of the pretreated nano-alumina, sodium silicate and borax in S3 is 3:2:1.
[0017] The present invention also provides the use of the stable modified lime powder for molten iron pretreatment prepared by the above-mentioned preparation method, characterized in that the stable modified lime powder is used for molten iron pretreatment.
[0018] Compared with the prior art, the present invention has the following advantages:
[0019] The present invention improves the moisture resistance and fluidity of quicklime through steady-state modification, thereby improving the stability of the product and the efficiency of pneumatic conveying. At the same time, the ability of quicklime to remove impurities in molten iron is further enhanced. This innovative technology can not only effectively solve the actual production problems in the process of molten iron pretreatment, but also provide important support for the sustainable development of the steel industry.
[0020] The present invention is further described in detail below in conjunction with embodiments. DETAILED DESCRIPTION
[0021] Example 1
[0022] The preparation method of the stable modified lime powder for molten iron pretreatment of this embodiment is as follows:
[0023] S1. Grind quicklime into powder to obtain quicklime powder, wherein the quicklime powder has a particle size of 60 mesh accounting for more than 98%;
[0024] S2. Pretreatment of nano-alumina:
[0025] Dissolve stearic acid in ethanol, then add nano-alumina, stir, and continue stirring at 70°C for 3 hours, remove suspended matter after standing, retain precipitated matter, and dry at 100°C to remove moisture and organic solvents. After drying, grind and disperse the agglomerated part for 1 hour to obtain pretreated nano-alumina;
[0026] The mass ratio of stearic acid to nano-alumina is 1:10; the nano-alumina after pretreatment is sealed to prevent it from getting wet in advance;
[0027] S3, adding sodium silicate and borax to the pretreated nano-alumina obtained in S2 while continuing to grind, to obtain a steady-state modified enhancer; the mass ratio of the pretreated nano-alumina, sodium silicate and borax is 3:2:1;
[0028] S4, adding the stable modified reinforcing agent obtained in S3 to the quicklime powder obtained in S1, mixing and grinding at a temperature of 90° C., performing surface coating treatment on the lime fine powder particles to isolate the moisture in the air, and obtaining the stable modified lime powder for molten iron pretreatment after screening; transporting the products that meet the product requirements to the finished product warehouse, and returning the unqualified products to the pulverizer for secondary grinding;
[0029] Among them, the stable modifier is added to the quicklime powder according to the technical requirements of Table 1:
[0030] Table 1 Content parameters and technical requirements
[0031] CaO Stable Modifier Enhancer S Burn vector Other trace elements total >90% 5% <0.05% >5% <0.1%
[0032] During the screening process, the powder selector screens and delivers the products that meet the product requirements to the finished product warehouse, while the unqualified products are returned to the grinder for secondary grinding. The finished product standards are shown in Table 2 below:
[0033] Table 2 Finished product standard table
[0034] CaO Stable Modifier Enhancer 60 mesh screening 200 mesh screening Burn vector Natural heap corner >90% 5% >98% >80% >5% <25°
[0035] The effect comparison of the finished product of this embodiment and the quicklime powder without adding the stable state modifier is as follows:
[0036] The stable modified quicklime powder of this embodiment has a longer storage time and a smaller loss amount.
[0037] ① Placed under natural conditions, ordinary quicklime powder
[0038] Within 3 days, the natural stack angle reaches 60°, the burning vector increases by 50%, and the steel becomes invalid and scrapped.
[0039] ② Placed under natural conditions, stable modified quicklime powder
[0040] Within 3 days, the natural heap angle remains unchanged, and the burning vector increases by 15%;
[0041] Within 7 days, the natural heap angle remains unchanged, and the burning vector increases by 35%;
[0042] Within 10 days, the natural pile angle increased by 2° and the burning vector increased by 54%.
[0043] The stable modified quicklime powder after stable modification can effectively block the moisture in the air while maintaining the fluidity unchanged, thus extending the service life of the quicklime powder. At the same time, the products generated by the reaction of the above-mentioned rapid stable modifier with quicklime (such as calcium phosphate, calcium carbonate, calcium borate, calcium silicate, etc.) are all common components in the metallurgical process. Most of them form slag, which is helpful to remove impurities in molten iron, or decompose into harmless components (stearic acid C 17 H 35 COOH), so it will not introduce harmful impurities into the subsequent steel production process and has certain positive effects.
[0044] The stable modified lime powder for molten iron pretreatment prepared in this embodiment is used for molten steel pretreatment. First, the prepared stable modified lime powder is added to the molten iron to be treated in a prescribed proportion. The stable modified lime powder is uniformly dispersed in the molten iron by mechanical stirring, and chemically reacts with impurities (such as sulfur, phosphorus, and silicon) in the molten iron. After the reaction, impurities such as sulfur, phosphorus, and silicon are removed from the molten iron by forming stable compounds. Finally, the molten iron after the reaction is filtered to remove the generated impurity compounds to obtain purified molten iron. This effectively improves the removal effect during molten iron pretreatment.
[0045] The desulfurization efficiency is improved, the sulfur content before treatment is 0.0075%, and the sulfur content is reduced to 0.003% after pretreatment of the molten iron. The dephosphorization efficiency is improved, the phosphorus content before treatment is 0.06%, and the sulfur content is reduced to 0.015% after pretreatment of the molten iron. The desiliconization efficiency is improved, the silicon content before treatment is 0.25%, and the silicon content is reduced to 0.1% after pretreatment of the molten iron. At the same time, the formed furnace side and the reduction of the corrosion of the impurities in the molten iron to the furnace lining can effectively extend the life of the furnace lining by more than 2 months.
[0046] Example 2
[0047] The preparation method of the stable modified lime powder for molten iron pretreatment of this embodiment is as follows:
[0048] S1. Grind quicklime into powder to obtain quicklime powder, wherein the quicklime powder has a particle size of 60 mesh accounting for more than 98%;
[0049] S2. Pretreatment of nano-alumina:
[0050] Dissolve stearic acid in ethanol, then add nano-alumina, stir, and continue stirring at 80°C for 2h, remove suspended matter after standing, retain precipitated matter, and dry at 100°C to remove moisture and organic solvents. After drying, grind and disperse the agglomerated part for 1h to obtain pretreated nano-alumina;
[0051] The mass ratio of stearic acid to nano-alumina is 1:10; the nano-alumina after pretreatment is sealed to prevent it from getting wet in advance;
[0052] S3, adding sodium silicate and borax to the pretreated nano-alumina obtained in S2 while continuing to grind, to obtain a steady-state modified enhancer; the mass ratio of the pretreated nano-alumina, sodium silicate and borax is 3:2:1;
[0053] S4, adding the stable modified reinforcing agent obtained in S3 to the quicklime powder obtained in S1, mixing and grinding at a temperature of 60° C., coating the surface of the lime fine powder particles to isolate the moisture in the air, and obtaining the stable modified lime powder for molten iron pretreatment after screening; transporting the products that meet the product requirements to the finished product warehouse, and returning the unqualified products to the pulverizer for secondary grinding;
[0054] Among them, the steady-state modifier is added to the quicklime powder according to the technical requirements of Table 1 in Example 1.
[0055] During the screening process, the powder selection machine is used to screen and deliver the products that meet the product requirements to the finished product warehouse, while the unqualified products are returned to the grinding machine for secondary grinding. The finished product standard is based on Table 2 of Example 1.
[0056] The stable modified lime powder for molten iron pretreatment prepared in this embodiment is used for molten steel pretreatment, which can effectively improve the impurity removal effect during molten iron pretreatment. The desulfurization efficiency is improved, the sulfur content before treatment is 0.0075%, and the sulfur content is reduced to 0.003% after the molten iron is pretreated. The dephosphorization efficiency is improved, the phosphorus content before treatment is 0.06%, and the sulfur content is reduced to 0.015% after the molten iron is pretreated. The desiliconization efficiency is improved, the silicon content before treatment is 0.25%, and the silicon content is reduced to 0.1% after the molten iron is pretreated. At the same time, the furnace side formed and the corrosion of the impurities in the molten iron to the furnace lining can effectively extend the life of the furnace lining by more than 2 months.
[0057] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a stable modified lime powder for molten iron pretreatment, characterized in that: The method is: S1, grinding quicklime into powder to obtain quicklime powder; S2. Pretreatment of nano-alumina: Dissolve stearic acid in ethanol, then add nano-alumina, stir, and continue stirring at a temperature of 70°C to 80°C for 2h to 3h, remove suspended matter after standing, retain precipitated matter, dry at 100°C, and grind and disperse the agglomerated part after drying to obtain pretreated nano-alumina; S3, adding sodium silicate and borax to the pretreated nano-alumina obtained in S2 while continuing to grind, to obtain a stable modifier enhancer; S4. Add the stable modified reinforcing agent obtained in S3 to the quicklime powder obtained in S1, mix and grind at a temperature of 60° C. to 90° C., and sieve to obtain stable modified lime powder for molten iron pretreatment.
2. The method for preparing a stable modified lime powder for molten iron pretreatment according to claim 1, wherein: The quicklime powder in S1 has a particle size of 60 mesh accounting for more than 98%.
3. The method for preparing a stable modified lime powder for molten iron pretreatment according to claim 1, wherein The mass ratio of stearic acid to nano-alumina in S2 is 1:
10.
4. The method for preparing a stable modified lime powder for molten iron pretreatment according to claim 1, wherein: The drying temperature in S2 is 100°C.
5. The method for preparing a stable modified lime powder for molten iron pretreatment according to claim 1, wherein: The mass ratio of the pretreated nano-alumina, sodium silicate and borax in S3 is 3:2:
1.