Method for imitating surface texture of titanium alloy by compounding titanium film layer on surface of aluminum alloy

By combining sandblasting, titanium plating, and hydrophobic coating on aluminum alloy surfaces with magnetron sputtering technology and vacuum coating equipment, the problem of simulating the appearance and feel of titanium alloys without increasing cost and complexity has been solved, achieving cost-effectiveness and performance improvement.

CN118957522APending Publication Date: 2024-11-15LUXCASE PRECISION TECH (YANCHENG) CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411057993.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing technologies struggle to simulate the look and feel of titanium alloys, and to provide similar physical and chemical properties, without increasing cost and complexity.

Method used

A composite film layer that mimics the surface texture of titanium alloy is formed on the surface of aluminum alloy by sandblasting, titanium plating, and hydrophobic coating, combined with magnetron sputtering technology and vacuum coating equipment. The process includes sandblasting, titanium plating, and hydrophobic coating steps.

Benefits of technology

It significantly reduces material costs, improves durability and aesthetics, meets environmental standards, ensures uniformity and adhesion of the film layer, and achieves a titanium alloy-like appearance and feel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957522A_ABST
    Figure CN118957522A_ABST
Patent Text Reader

Abstract

The invention provides a method for imitating the surface texture of a titanium alloy by compounding a titanium film layer on the surface of an aluminum alloy, and belongs to the technical field of metal surface composite films, and the method comprises the following steps: S1, sand blasting: polishing an aluminum alloy material by using CNC (Computer Numerical Control) equipment; then carrying out sand blasting treatment on the appearance surface to obtain a sand-blasted aluminum alloy product; s2, pretreatment before titanium plating is conducted, specifically, a cleaning agent and pure water are sequentially used for cleaning the sand-blasted aluminum alloy product, then constant-temperature heating operation is conducted, and finally ion cleaning is conducted; s3, titanium plating: plating a layer of pure titanium on the surface of the sandblasted aluminum alloy product by using a magnetron sputtering technology by using coating equipment to obtain a titanium-plated aluminum alloy product; and S4, titanium plating post-treatment is conducted, specifically, vacuum coating equipment is used for plating a hydrophobic coating on the surface of the titanium-plated aluminum alloy product, the texture of the surface of the imitated titanium alloy is achieved, and in addition, the product is additionally provided with the characteristics of abrasion resistance, pollution resistance and easy cleaning.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal surface composite films, in particular to a method for imitating the surface texture of a titanium alloy by composite titanium film layers on the surface of an aluminum alloy. Background Art

[0002] In modern industrial applications, especially in precision manufacturing and consumer electronics, the surface texture and durability of materials have a decisive influence on the market competitiveness of products. Titanium alloys are widely used in many high-end application fields due to their excellent mechanical properties and excellent corrosion resistance, especially in aviation, medical and high-end consumer goods (such as watches). However, the cost of titanium alloy materials (such as TC4) is relatively high, which includes not only the cost of raw materials, but also the high cost of processing and forming. These cost factors have greatly limited the application of titanium alloys in the wider consumer goods market.

[0003] The processing of TC4 material involves multiple steps, including forging, CNC machining, polishing, sandblasting, anodizing and coating. Each step requires special equipment and technology, which increases the complexity and cost of the manufacturing process. In particular, CNC machining and anodizing are not only time-consuming and energy-intensive, but also cause great wear and tear on the equipment. In addition, although the high strength and corrosion resistance of titanium alloys are its advantages, they also make processing more difficult, further pushing up production costs.

[0004] For example, Chinese patent literature has disclosed an automatic lifting door bottom sealing strip [Chinese Patent No.: 202311170002.0]. The present invention discloses a composite material surface magnetron sputtering coating process and method, which relates to the field of magnetron sputtering coating technology. The composite material surface magnetron sputtering coating process includes the following operation steps: S1, substrate preparation; S2, processing environment preparation; S3, target material preparation; S4, magnetron sputtering; S5, post-plating treatment. The composite material surface magnetron sputtering coating process and method, by synchronously cleaning the workpiece and the sputtering chamber before magnetron sputtering coating, compressed air is used to remove the sputtering residues around the cavity during cleaning, and then the surface is gently polished with sandpaper impregnated with sodium chloride to remove the attachments on the chamber wall. Sodium chloride can react with the residues of the metal titanium target on the sputtering chamber to increase the ease of cleaning. During polishing, an industrial vacuum cleaner is used for auxiliary cleaning, and finally, alcohol, acetone and deionized water are used to clean the sputtering chamber to ensure the cleanliness of the sputtering chamber and avoid the influence of the indoor residues on the subsequent magnetron sputtering coating.

[0005] Although the above technical solution adopts magnetron sputtering technology, the preliminary processing technical means are different. The above technical solution uses: 600#, 800# and 1000# sandpaper to coarsely grind the coated surface of the composite material, and after coarse grinding, use a polishing cloth coated with polishing paste to polish the sample; while the present invention adopts sandblasting, and the purpose to be achieved is different.

[0006] Therefore, in view of the challenges of cost and process, how to develop a method that can simulate the appearance and feel of titanium alloy and provide similar physical and chemical properties to a certain extent is an urgent problem that needs to be solved. Summary of the invention

[0007] The purpose of the present invention is to solve the above problems in the prior art and to propose a method for imitating the surface texture of titanium alloy by compounding a titanium film layer on the surface of aluminum alloy.

[0008] The purpose of the present invention can be achieved by the following technical scheme: A method for imitating the surface texture of titanium alloy by composite titanium film layer on the surface of aluminum alloy, comprising the following contents:

[0009] S1 Sandblasting: The aluminum alloy material is polished by CNC equipment; then the appearance surface is sandblasted to obtain the aluminum alloy product after sandblasting;

[0010] S2 Pretreatment before titanium plating: Use cleaning agent and pure water to clean the aluminum alloy products after sandblasting, then perform constant temperature heating operation, and finally perform ion cleaning;

[0011] S3 titanium plating: Use coating equipment to use magnetron sputtering technology to plate a layer of pure titanium on the surface of the aluminum alloy product after sandblasting to obtain a titanium-plated aluminum alloy product;

[0012] S4 titanium plating post-treatment: Use vacuum coating equipment to plate a hydrophobic coating on the surface of titanium-plated aluminum alloy products.

[0013] Preferably, in step S1, in the sandblasting process, the sandblasting is specifically zirconium sand.

[0014] Preferably, in step S3, during the titanium plating process, the operating parameters are set as follows: the Ti target uses a 40KW medium frequency power supply; the bias power supply uses a 30Kw DC pulse bias power supply.

[0015] Preferably, the Ar flux is 100 Sccm, 2 pairs of Ti target powers are 10 KW, the negative bias is 45 V / 50%, and the sputtering is for 60 min; the Ar flux is 100 Sccm, 2 pairs of Ti target powers are 10 KW, the negative bias is 60 V / 50%, and the sputtering is for 80 min; the Ar flux is 100 Sccm, 2 pairs of Ti target powers are 10 KW, the negative bias is 80 V / 50%, and the sputtering is for 90 min.

[0016] Preferably, in step S4, the specific steps of coating the hydrophobic coating on the surface of the titanium-plated aluminum alloy product are as follows:

[0017] S4.1 Product cleaning: Clean the titanium-plated aluminum alloy products to remove impurities and contaminants on the surface;

[0018] S4.2 Vacuuming the furnace: Place the titanium-plated aluminum alloy product in the vacuum coating equipment, and then adjust the vacuum degree;

[0019] S4.3 Ion cleaning: Ion cleaning of titanium-plated aluminum alloy products;

[0020] S4.4 Vapor deposition of silicon dioxide: Vapor deposition of silicon dioxide is performed on the surface of the titanium-plated aluminum alloy product to obtain a vapor-deposited product;

[0021] S4.5 Chemical evaporation: Use chemicals to evaporate the deposited product to form a hydrophobic coating on the surface of the deposited product.

[0022] Reasons for using silica: Chemical resistance and stability: Silica has excellent chemical stability and can resist corrosion from most acids and alkalis. This property allows the aluminum alloy surface coated with silica to have a longer service life in chemical exposure environments.

[0023] Scratch and wear resistance: The silicon dioxide film layer can provide good hardness and wear resistance, protecting the surface of the material from scratches.

[0024] Transparency: Silicon dioxide has good optical transparency. After coating, it will not affect the color and appearance of the material, and maintain the beauty of aluminum alloy products.

[0025] Improved surface smoothness: Silicon dioxide coating can smooth the surface of the material and reduce surface defects at the microscopic level, thereby improving the surface finish and brightness.

[0026] Preferably, during the furnace extraction operation, the vacuum degree is adjusted to 1.0-2 Pa; during the ion cleaning operation and the silicon dioxide vapor deposition operation, the argon gas is 3-9 Sccm, the oxygen is 30-70 Sccm, the voltage is 400-700 V, and the current is 400-700 mA.

[0027] Preferably, in step S4.4, the thickness of the evaporated silicon dioxide is 15 nm.

[0028] Preferably, in step S4.5, the reagent is a mixture of fluororesin and fluorine-containing solvent; the evaporation temperature is 200° C. to 500° C., and the thickness of the hydrophobic coating is 6 nm.

[0029] The application of fluororesins and fluorinated solvent mixtures in hydrophobic coatings has the following advantages:

[0030] Excellent hydrophobicity and oil resistance: Fluororesin is highly hydrophobic and oil-resistant, effectively preventing the accumulation of moisture and grease on the surface of the material, reducing the difficulty of cleaning and maintenance, while extending the life of the product.

[0031] Chemical corrosion resistance: Fluororesin has extremely high chemical stability and can resist corrosion from a variety of chemical substances.

[0032] Temperature resistance: Fluororesin maintains stable performance over a wide temperature range and is not prone to aging.

[0033] Excellent mechanical properties: Fluororesin coating not only provides chemical and physical protection, but also enhances the tensile and compressive properties of the material.

[0034] Compared with the prior art, the method of imitating the surface texture of titanium alloy by composite titanium film layer on the surface of aluminum alloy has the following beneficial effects:

[0035] 1. Significant cost-effectiveness: By coating a pure titanium film layer on the surface of a relatively low-cost aluminum alloy, this method significantly reduces the material cost compared to directly using titanium alloy. The raw materials and processing costs of titanium alloy are high, especially in applications requiring high precision. Aluminum alloy is cheap and easy to process. Through the processing of the present invention, a similar appearance and touch to titanium alloy can be achieved without sacrificing too much performance.

[0036] 2. Improve durability and aesthetics: Through the steps of sandblasting, titanium plating and hydrophobic coating, not only the wear resistance of the aluminum alloy surface is enhanced, but also its corrosion resistance and appearance are improved. In particular, the addition of hydrophobic coating provides the product with additional anti-pollution and easy-to-clean properties, which is particularly important for maintaining the long-term appearance and texture of the product.

[0037] 3. Environmental friendliness and equipment compatibility: The sputtering technology and chemical treatment steps used in this method are in line with modern environmental standards, reducing the use and emission of harmful chemicals. In addition, the equipment used, such as CNC machine tools and vacuum coating equipment, are widely available in the industry and do not require special customization, which is conducive to the rapid deployment and popularization of the technology.

[0038] 4. Optimized operating parameters: By finely adjusting the parameters in the coating process, such as power supply, bias voltage and sputtering time, the coating process is made more precise and controllable. This precise control helps to ensure the uniformity and adhesion of the film layer and ensure the quality of the final product. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a schematic diagram of the appearance of the product prepared in specific embodiment 2.

[0040] Figure 2 It is a roughness schematic diagram of the product prepared in specific embodiment 2.

[0041] Figure 3 This is a roughness profile diagram of the product prepared in specific embodiment 2. DETAILED DESCRIPTION

[0042] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments. Specific embodiment one:

[0044] After aluminum extrusion and cutting, the aluminum alloy substrate is processed by CNC equipment according to manufacturing requirements. The specific process is CNC processing of dome features; laser tracking barcode processing; CNC processing of side profile, belt groove, BRB groove rough processing and BRB chamfering; cleaning; rolling and grinding; cleaning; CNC processing of side holes, chamfers, round holes and burrs; cleaning; inspection; finally, CNC equipment is used for surface polishing, and after polishing, sandblasting is performed to obtain sandblasted aluminum alloy products; by adjusting the sandblasting parameters, the surface effect after sandblasting reaches the TC4 sandblasting effect; the sandblasting is specifically zirconium sand. Specific embodiment 2:

[0046] The aluminum alloy product after sandblasting in the first specific embodiment is cleaned with a cleaning agent and pure water in sequence, then subjected to a constant temperature heating operation, and finally subjected to ion cleaning;

[0047] Use coating equipment to coat a layer of pure titanium on the surface of the aluminum alloy product after sandblasting using magnetron sputtering technology, and the appearance will achieve the surface effect of TC4 material; obtain titanium-coated aluminum alloy products;

[0048] During the titanium plating process, the operating parameters were set as follows: the Ti target used a 40KW medium frequency power supply; the bias power supply used a 30Kw DC pulse bias power supply;

[0049] Ar flux 100 Sccm, 2 pairs of Ti target power 10 KW, negative bias 45 V / 50%, sputtering 60 min; Ar flux 100 Sccm, 2 pairs of Ti target power 10 KW, negative bias 60 V / 50%, sputtering 80 min; Ar flux 100 Sccm, 2 pairs of Ti target power 10 KW, negative bias 80 V / 50%, sputtering 90 min. Specific embodiment three:

[0051] Using vacuum coating equipment, a hydrophobic coating is applied to the surface of the titanium-plated aluminum alloy product in the second specific embodiment, and the color and appearance are consistent with the TC4 material;

[0052] The specific steps for coating the hydrophobic coating on the surface of titanium-plated aluminum alloy products are as follows:

[0053] Product cleaning: Clean titanium-plated aluminum alloy products to remove impurities and pollutants on the surface;

[0054] Vacuuming into the furnace: Place the titanium-plated aluminum alloy product in the vacuum coating equipment, and then adjust the vacuum degree;

[0055] Ion cleaning: ion cleaning of titanium-plated aluminum alloy products;

[0056] Evaporation of silicon dioxide: Evaporation of silicon dioxide is performed on the surface of the titanium-plated aluminum alloy product to obtain an evaporation product;

[0057] Chemical evaporation: Use chemicals to evaporate the deposited product to form a hydrophobic coating on the surface of the deposited product.

[0058] During the furnace extraction operation, the vacuum degree is adjusted to 1.0-2 Pa; during the ion cleaning operation and the silicon dioxide vapor deposition operation, the argon gas is 3-9 Sccm, the oxygen is 30-70 Sccm, the voltage is 400-700 V, and the current is 400-700 mA.

[0059] The thickness of the evaporated silicon dioxide is 15 nm.

[0060] The agent is a mixture of fluororesin and fluorine-containing solvent; the evaporation temperature is 200°C to 500°C, and the hydrophobic coating thickness is 6nm.

[0061] The product prepared in the second embodiment is subjected to appearance surface and roughness inspection, such as Figures 1 to 3 As stated,

[0062] The main ISO 25178-surface characteristic parameter data are as follows:

[0063] Main height parameters: Sq is 1.67406um; Sv is 7.60365um; Sz is 13.2752um; Sa is 1.29954um;

[0064] Spatial parameters: Sal is 16.8979um;

[0065] Mixing parameters: Sdq is 0.429719um;

[0066] Characteristic parameters: Spd is 0.000787359 1 / μm 2

[0067] Functional parameters (layered surface): Sk is 3.39729um; Spk is 1.57437um;

[0068] The data and schematic diagram are analyzed as follows: The main ISO 4287-roughness parameter data are as follows:

[0069] Rz is 8.30291um; Ra is 1.42383um; Rq is 1.79444um.

[0070] Compliance with ISO 25178-Surface characteristic parameter data:

[0071] Sq (mean square root height) is 1.67406μm: This parameter shows the overall roughness level of the surface, which is consistent with the average surface height of TC4 titanium alloy, ensuring consistency in vision and touch.

[0072] Sv (volume parameter) is 7.60365μm: it reflects the peak-to-valley height distribution of the surface, which is consistent with the undulating characteristics of the TC4 surface and is crucial to the simulation effect of the appearance.

[0073] Sz (maximum height) is 13.2752 μm: This indicates the maximum height difference of the surface, matching the characteristics of the TC4 surface and ensuring texture and visual unity at the microscopic scale.

[0074] Sa (average height) is 1.29954μm: It shows the average roughness level of the surface, which is similar to the surface characteristics of TC4 titanium alloy, ensuring the consistency of product appearance and the simulation effect of texture.

[0075] Compliance with ISO 4287-Roughness parameter data:

[0076] Rz (maximum peak height) is 8.30291μm: it reflects the overall undulation of the surface, which is similar to the Rz value of the TC4 titanium alloy surface, ensuring the simulation of the product's appearance and texture.

[0077] Ra (average roughness) is 1.42383 μm: It shows the average roughness level of the surface, which is related to the consistency of the TC4 surface, ensuring the consistency of the surface texture and visual appearance.

[0078] Rq (root mean square roughness) is 1.79444μm: It reflects the overall roughness level of the surface, which matches the Rq value of the TC4 titanium alloy surface, further ensuring the simulation effect of the product in appearance and texture.

[0079] Based on the above analysis, this method successfully formed a composite titanium film layer on the surface of aluminum alloy that imitated the surface texture of titanium alloy through sophisticated process steps and parameter control.

[0080] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A method for imitating the surface texture of titanium alloy by composite titanium film layer on the surface of aluminum alloy. It is characterized in that The method for imitating the surface texture of titanium alloy by composite titanium film layer on the surface of aluminum alloy specifically comprises the following contents: S1 Sandblasting: The aluminum alloy material is polished by CNC equipment; then the appearance surface is sandblasted to obtain the aluminum alloy product after sandblasting; S2 Pretreatment before titanium plating: Use cleaning agent and pure water to clean the aluminum alloy products after sandblasting, then perform constant temperature heating operation, and finally perform ion cleaning; S3 titanium plating: Use coating equipment to use magnetron sputtering technology to plate a layer of pure titanium on the surface of the aluminum alloy product after sandblasting to obtain a titanium-plated aluminum alloy product; S4 titanium plating post-treatment: Use vacuum coating equipment to plate a hydrophobic coating on the surface of titanium-plated aluminum alloy products.

2. The method of imitating the surface texture of titanium alloy by compounding a titanium film layer on the surface of aluminum alloy as claimed in claim 1, It is characterized in that In step S1, during the sand blasting process, the sand blasting is specifically zirconium sand.

3. The method of imitating the surface texture of titanium alloy by compounding a titanium film layer on the surface of aluminum alloy as claimed in claim 1, It is characterized in that In step S3, during the titanium plating process, the operating parameters are set as follows: the Ti target uses a 40KW medium frequency power supply; the bias power supply uses a 30Kw DC pulse bias power supply.

4. The method of imitating the surface texture of titanium alloy by compounding a titanium film layer on the surface of aluminum alloy as claimed in claim 3, It is characterized in that In step S3, the Ar flux is 100 Sccm, the power of 2 pairs of Ti targets is 10 KW, the negative bias voltage is 45 V / 50%, and the sputtering is carried out for 60 min; the Ar flux is 100 Sccm, the power of 2 pairs of Ti targets is 10 KW, the negative bias voltage is 60 V / 50%, and the sputtering is carried out for 80 min; the Ar flux is 100 Sccm, the power of 2 pairs of Ti targets is 10 KW, the negative bias voltage is 80 V / 50%, and the sputtering is carried out for 90 min.

5. The method of imitating the surface texture of titanium alloy by compounding a titanium film layer on the surface of aluminum alloy as claimed in claim 1, It is characterized in that In step S4, the specific steps of coating the hydrophobic coating on the surface of the titanium-plated aluminum alloy product are as follows: S4.1 Product cleaning: Clean the titanium-plated aluminum alloy products to remove impurities and contaminants on the surface; S4.2 Vacuuming the furnace: Place the titanium-plated aluminum alloy product in the vacuum coating equipment, and then adjust the vacuum degree; S4.3 Ion cleaning: Ion cleaning of titanium-plated aluminum alloy products; S4.4 Vapor deposition of silicon dioxide: Vapor deposition of silicon dioxide is performed on the surface of the titanium-plated aluminum alloy product to obtain a vapor-deposited product; S4.5 Chemical evaporation: Use chemicals to evaporate the deposited product to form a hydrophobic coating on the surface of the deposited product.

6. The method of imitating the surface texture of titanium alloy by compounding a titanium film layer on the surface of aluminum alloy as claimed in claim 5, It is characterized in that During the furnace extraction operation, the vacuum degree is adjusted to 1.0-2 Pa; during the ion cleaning operation and the silicon dioxide vapor deposition operation, the argon gas is 3-9 Sccm, the oxygen is 30-70 Sccm, the voltage is 400-700 V, and the current is 400-700 mA.

7. The method of imitating the surface texture of titanium alloy by compounding a titanium film layer on the surface of aluminum alloy as claimed in claim 5, It is characterized in that In step S4.4, the thickness of the evaporated silicon dioxide is 15 nm.

8. The method of imitating the surface texture of titanium alloy by compounding a titanium film layer on the surface of aluminum alloy as claimed in claim 5, It is characterized in that In step S4.5, the reagent is a mixture of fluororesin and fluorine-containing solvent; the evaporation temperature is 200°C to 500°C, and the thickness of the hydrophobic coating is 6nm.

Citation Information

Patent Citations

  • Magnetron sputtering coating process and method for surface of composite material

    CN117187765A