Chiral-magnetic composite material, preparation method thereof and application of chiral-magnetic composite material as oxygen evolution reaction electrocatalyst
Through the synergistic effect of the spin selection effect of chiral-magnetic composite materials and the magnetic effect of magnetic materials, the problems of high overpotential and H2O2 by-product generation of OER electrocatalysts are solved, and low overpotential and efficient electrolytic water conversion is achieved.
Patent Information
- Application Number
- CN202411009894.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
OER electrocatalysts have problems with high overpotential and H2O2 by-product generation during electrolysis, resulting in low energy conversion efficiency.
Using chiral-magnetic composite materials, the spin polarization efficiency of OH· is improved through the magnetic effect of magnetic materials, and the spin selection effect induced by chiral molecules is used to shield unpolarized OH· and inhibit H2O2 and singlet oxygen. Generation of .
It significantly reduces the overpotential of OER, improves the conversion efficiency of electrolytic water, enhances the Faraday conversion efficiency, and improves the stability of the catalyst.
Smart Images

Figure CN118957626A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrocatalysts, and in particular to a chiral-magnetic composite material, a preparation method thereof and an application thereof as an electrocatalyst for oxygen evolution reaction. Background Art
[0002] The electrocatalytic oxygen evolution reaction (OER) is an anode half-reaction commonly involved in energy conversion systems such as carbon dioxide electroreduction, water splitting, and rechargeable metal-air batteries. However, the slow four-electron kinetics of the OER process leads to low energy conversion efficiency in related systems.
[0003] Although substantial progress has been made in the research of OER electrocatalysts in recent years, there are still two outstanding problems: 1) The OER overpotential is high. Even the most active OER catalyst generally requires an overpotential of about 200 mV to reach 10 mA / cm 2 current density; 2) the generation of H2O2 by-product makes the Faraday conversion efficiency low.
[0004] At present, the research on OER electrocatalysis mainly focuses on optimizing the thermodynamic properties related to the adsorption and desorption of reactants / intermediates on the catalyst surface. However, in addition to thermodynamic characteristics, the electron spin state of the intermediates is also a key factor affecting the OER reaction. According to the law of conservation of spin angular momentum in chemical reactions, the spin-degenerate hydroxyl radical (OH·) is preferentially converted into singlet oxygen ( 1 Δ g ), and then decays to the ground state triplet oxygen ( 3 Σ g ), since the energy of singlet oxygen is about 1eV higher than that of triplet oxygen, the water electrolysis system needs to provide a voltage greater than 1.23V to overcome the energy barrier, which will generate a certain overvoltage; in addition, spin-degenerate OH· is easy to combine to form singlet H2O2, which will reduce the OER conversion efficiency of anode electrons. If the OER electrocatalyst can effectively control the spin state of OH·, it will be expected to break through the activity bottleneck of OER.
[0005] Magnetic materials can provide an external magnetic field acting on the electron spin magnetic moment, inducing OH· spin polarization and promoting the direct generation of ground state oxygen. Magnetic materials used in OER mainly include ferromagnetic compounds containing iron, cobalt, and nickel, oxides with magnetic crystal faces, and some perovskite oxides. At present, the OER electrocatalytic activity of some magnetic materials has surpassed that of commercial precious metal ruthenium (iridium) oxide catalysts. Although magnetic materials have the advantage of promoting electron spin polarization, it is difficult for magnetic materials to achieve all OH· spin polarization in the actual catalytic process, and unpolarized OH· will inevitably generate H2O2 or singlet oxygen.
[0006] Therefore, how to improve the above-mentioned properties of magnetic materials and provide a method with low OER overpotential and inhibiting the generation of H2O2 is a technical problem that needs to be solved urgently in this field. Summary of the invention
[0007] One of the purposes of the present invention is to provide a chiral-magnetic composite material to solve the above-mentioned problems.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0009] A chiral-magnetic composite material, wherein the composite material is a magnetic material loaded with a chiral material on its surface.
[0010] The transport of electrons in a chiral field is closely related to their spins. Only electrons whose spin orientation matches the chiral molecular configuration can pass through the chiral structure. This spin filtering property caused by chirality is called the chirality-induced spin selection effect. The chiral structure can inhibit the generation of H2O2 by shielding OH· whose spin orientation does not match its structure.
[0011] Schematic diagram of chirality-induced electron spin selection effect Fig.11 As shown, from Fig.11 It can be seen that when electrons pass through the chiral field, some electrons are forced to stop transmitting. Only electrons whose spin direction matches the chirality can continue to participate in the reaction after passing through the chiral field and directly generate ground state oxygen.
[0012] The present invention constructs a novel chiral-magnetic composite material through molecular self-assembly technology: the magnetic effect of the magnetic unit is used to improve the spin polarization efficiency of OH· generated in the water electrolysis process, thereby improving the direct conversion efficiency of ground state oxygen; the spin selection effect induced by the chiral molecules is then used to shield OH· that has not achieved spin polarization, thereby inhibiting the generation of H2O2 and singlet oxygen, thereby achieving the purpose of synergistically improving the conversion efficiency of water electrolysis.
[0013] The second object of the present invention is to provide a method for preparing the chiral-magnetic composite material, comprising the following steps:
[0014] (1) Preparation of magnetic materials;
[0015] (2) The chiral material is loaded onto the surface of the magnetic material to obtain a chiral-magnetic composite material.
[0016] As a preferred technical solution, the magnetic material includes but is not limited to nickel-based magnetic material or iron-based magnetic material.
[0017] As a further preferred technical solution, when preparing the magnetic material in step (1), a metal precursor is selected for preparation, and the metal precursor is one of a metal salt, a metal powder or a metal oxide. In order to prepare a nanomagnetic unit with a high specific surface area, provide more sites to combine with the chiral sites, and realize the synergistic coupling of the functionalized sites, the present invention preferably uses a metal salt.
[0018] It should be noted that there is no limitation on the synthesis method of the magnetic material described in step (1). From the perspective of reducing equipment cost and energy consumption, the present invention is more preferably a hydrothermal method or a high-temperature calcination method known in the art.
[0019] A further preferred technical solution is to grow the magnetic structure on a conductive base material such as carbon cloth and nickel foam, which can effectively avoid the problem of nanomaterials stacking on each other and being unable to load more chiral small molecules; at the same time, it can alleviate the problem of oxygen evolution stripping the adsorbed chiral molecules from the magnetic material when the composite material is used as a catalyst.
[0020] It should be noted that the conductive substrate used in the present invention is preferably cleaned with a solvent such as ethanol or acetone to remove residual grease on the surface. The conductive substrate may also be further treated with an acidic solvent, including but not limited to hydrochloric acid, nitric acid, etc., to remove the oxide layer on the surface of the substrate or to improve the hydrophilicity of the material.
[0021] In step (2) of the present invention, the chiral material can be a chiral small molecule, an inorganic nanoparticle with a chiral group or a chiral morphology constructed by self-assembly of a (chiral) small molecule. However, from the perspective of saving time cost and equipment investment cost, the present invention preferably uses a chiral small molecule as a chiral unit to construct a chiral-magnetic composite material, which exhibits an activity that is significantly better than that of a pure magnetic material.
[0022] As a preferred technical solution, the present invention selects chiral small molecules to be directly loaded onto the surface of the magnetic unit as chiral units for filtering intermediates that have not achieved spin polarization during the OER process, and the chiral small molecules are selected from at least one of tartaric acid, L-cysteine, L-tryptophan, and L-ascorbic acid.
[0023] That is, the selection of the above-mentioned chiral small molecules is extremely wide, including common tartaric acid, L-cysteine, L-tryptophan, and L-ascorbic acid, and there are no obvious requirements for the configuration, conformation, and molecular weight of the chiral small molecules.
[0024] According to a further preferred technical solution, the present invention disperses chiral materials such as chiral small molecules into an aqueous solution, and the concentration of the chiral materials is preferably between 5 mmol / L and 20 mmol / L.
[0025] More preferably, the present invention immerses the magnetic material into an aqueous solution containing the chiral material, and utilizes intermolecular forces to uniformly modify the chiral small molecules on the surface of the magnetic material.
[0026] It should be noted that the immersion of the magnetic material in the aqueous solution containing the chiral material may be assisted by shaking, ultrasound or stirring to ensure that the concentration of the solution in the container containing the chiral material is consistent, thereby ensuring that the chiral molecules are loaded onto the surface of the magnetic material as evenly and firmly as possible.
[0027] It should be further explained that there is no strict requirement on temperature in the process of modifying the magnetic unit with the chiral unit. From the perspective of saving equipment purchase cost and energy consumption cost of temperature control, the present invention preferably adopts room temperature environment to carry out the corresponding process.
[0028] The third object of the present invention is to provide an application of the chiral-magnetic composite material as an electrocatalyst for oxygen evolution reaction, wherein the electrolyte for the oxygen evolution reaction of the present invention is an alkaline electrolyte.
[0029] Compared with the prior art, the advantages of the present invention are: the present invention can significantly reduce the overpotential of OER and inhibit the generation of H2O2 by-products through the synergy of chiral materials and magnetic materials, thereby improving the Faraday conversion efficiency; the composite material of the present invention only requires the magnetic unit to have magnetism and a large specific surface area at the nanoscale, and there are almost no other requirements. The choice of chiral materials is also very wide. This flexibility is conducive to production enterprises to make reasonable choices based on their own budgets, equipment and other conditions, and has significant universality and potential economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The scanning electron microscope image (A) and the high-resolution transmission electron microscope image (B) of the pure nickel-based magnetic unit prepared in Example 1 of the present invention;
[0031] Figure 2 is an X-ray diffraction diagram of a chiral-nickel-based magnetic composite material and a pure nickel-based magnetic material prepared in Example 1 of the present invention;
[0032] Figure 3 It is the Fourier infrared transform spectrum of the chiral-nickel-based magnetic composite material and the pure nickel-based magnetic material prepared in Example 1 of the present invention;
[0033] Figure 4 is an OER activity curve of the chiral-nickel-based magnetic composite material and the pure nickel-based magnetic material prepared in Example 1 of the present invention in 1.0M KOH electrolyte;
[0034] Figure 5It is an ultraviolet-visible spectrum diagram of the amount of H2O2 produced by the chiral-nickel-based magnetic composite material and the pure nickel-based magnetic material prepared in Example 1 of the present invention during the OER process detected by using an ultraviolet-visible spectrometer.
[0035] Figure 6 OER stability test curve of the chiral-nickel-based magnetic composite material prepared in Example 1 of the present invention in 1.0 M KOH electrolyte.
[0036] Figure 7 is an OER activity curve of the chiral-nickel-based magnetic composite material containing the same chiral small molecule but different chiral molecule concentrations prepared in Example 1 of the present invention and Comparative Example 1 in 1.0 M KOH electrolyte;
[0037] Figure 8 is an OER activity curve of the chiral-nickel-based magnetic composite material containing different chiral small molecules prepared in Example 1 and Comparative Example 2 of the present invention in 1.0M KOH electrolyte;
[0038] Fig. 9 is an OER activity curve of a chiral-nickel-based magnetic composite material having magnetic units with different morphologies prepared in Comparative Example 3 of the present invention in a 1.0 M KOH electrolyte;
[0039] Fig.10 1. A transmission electron microscope scanning image (A) of a chiral-iron-based magnetic composite material having different magnetic unit compositions prepared in Comparative Example 4 of the present invention and a graph of its OER activity in a 1.0 M KOH electrolyte (B);
[0040] Fig.11 Schematic diagram of the chirality-induced electron spin selection effect. DETAILED DESCRIPTION
[0041] The present invention will be further described below in conjunction with the accompanying drawings.
[0042] Embodiment 1:
[0043] A chiral-nickel-based magnetic composite material, the preparation method of which comprises the following steps:
[0044] (1) Preparation of nickel-based nanosheet arrays (Ni(oxy)hydroxide) loaded on carbon cloth
[0045] Soak the carbon cloth in ethanol and concentrated nitric acid for 15 minutes respectively to remove possible stains on its surface, then rinse it with deionized water for several times for use; weigh 1.4g nickel chloride hexahydrate and 1.18g hexamethylenetetramine, and dissolve them in 36mL deionized water to obtain a solution; then transfer the solution to a 50mL reactor and add the treated carbon cloth
[0046] (2cm*2cm), react at 100℃ for 10h; after the reaction is completed, naturally cool to room temperature to obtain Ni(oxy)hydroxide;
[0047] (2) Preparation of carbon nanotubes containing nickel (CNT@Ni)
[0048] The Ni(oxy)hydroxide prepared in step (1) was placed in a 50 mL beaker and 20 mL of deionized water was added. The mixture was ultrasonicated for 15 min to remove the unstable Ni(oxy)hydroxide deposited on the surface of the carbon cloth. After completion, the mixture was washed with deionized water and dried in an oven.
[0049] Weigh 1g polyvinyl pyrrolidone (PVP) and 2g melamine, disperse them in 5mL N,N-dimethylformamide, and transfer part of the solution to evenly apply it on the dried carbon cloth, let it air-dry naturally, and repeat twice; weigh another 2g melamine in a porcelain boat, place the air-dried carbon cloth on top of the porcelain boat, put it in a tube furnace, sinter it at 500℃ for 2h under argon atmosphere, then continue to heat up to 700℃ and continue calcining for 2h; after completion, take it out and cool it naturally to obtain nickel-embedded carbon nanotubes, referred to as "CNT@Ni";
[0050] (3) Preparation of chiral-nickel-based composite materials (cys-CNT@Ni)
[0051] Weigh L-cysteine (abbreviated as "cys") and prepare it into a 10 mmol / L solution; then, put the CNT@Ni obtained in step (2) into it and shake it in a shaker for 1 hour; then, take out the product and put it in an oven for drying to obtain a cysteine-modified nickel-based magnetic material, abbreviated as "cys-CNT@Ni".
[0052] Application examples:
[0053] The cys-CNT@Ni composite nanomaterial prepared in Example 1 was used as an anode material for alkaline water electrolysis to catalyze the OER process, and the effect of the introduction of the chiral structure on the OER activity was evaluated.
[0054] In the above-mentioned Example 1, a CNT@Ni magnetic unit platform was prepared by chemical vapor deposition (CVD). Scanning electron microscope images show (eg Figure 1 A), the interconnected CNT@Ni completely covers the carbon cloth, forming a highly porous nanostructure. Transmission electron microscopy images show that the metallic Ni is tightly wrapped in the cavity of the carbon nanotubes, ensuring the structural stability of the magnetic unit (as shown in Figure 1 B).
[0055] Since chiral molecules are not crystalline materials, there is no obvious difference in the X-ray diffraction images of CNT@Ni and cys-CNT@Ni ( Figure 2 ).
[0056] In order to verify that the chiral molecules have been successfully loaded onto the CNT@Ni surface, the inventors conducted a detailed analysis of the Fourier transform infrared spectra of cys-CNT@Ni and CNT@Ni. The results are as follows Figure 3 As shown, the spectrum of cys-CNT@Ni is at 1063 cm -1 The sharp peak near 3234 cm corresponds to CN vibration. -1 、3409cm -1 The two significant peaks at correspond to NH vibrations. Due to the inherent properties of low chiral molecular content and low FTIR intensity of -SH groups, the SH and CS peaks in cys-CNT@Ni are not significant. Even so, the research results can fully prove the existence of chiral molecules cys on the surface of CNT@Ni.
[0057] The present invention uses a synthesized chiral material as a working electrode material, a carbon rod as a counter electrode, and mercury / mercuric oxide as a reference electrode to perform electrochemical testing in a 1.0M KOH electrolyte. The voltage test range of the electrochemical activity test is 0-1V, and the scanning speed is 5mV s -1 The calculation formula of the overvoltage in the present invention is: μ = E 测 +0.96-1.23, the current density is normalized according to the area size of the electrode.
[0058] The results show that the cys-CNT@Ni prepared in Example 1 reaches 100mA / cm 2 The current density required an overpotential of 547 mV. In contrast, CNT@Ni without chiral small molecule modification showed poor activity and required an overpotential of 572 mV to reach 100 mA / cm 2 The current density is , which is 25 mV higher than the overpotential required for cys-CNT@Ni. The electrochemical test results show that chiral small molecules can effectively reduce the overpotential of the OER process and improve the efficiency of water electrolysis.
[0059] It should be noted that: it is well known to those skilled in the art that since cys itself is a non-conductive organic small molecule, cys alone will not have any OER activity. Therefore, this embodiment does not use cys alone to perform relevant OER comparison tests.
[0060] In order to verify the role of the spin-selective effect induced by chiral small molecules in the catalytic OER process, the inventors used a UV-visible spectrophotometer to track the amount of H2O2 in different materials during the electrochemical OER process.
[0061] The specific method is as follows: first, the chiral-magnetic composite material (cys-CNT@Ni) and the magnetic material (CNT@Ni) are used as the anode for electrolysis of water, respectively, and the electrolysis is carried out continuously for 2 hours at a constant current of 0.6V to obtain two different electrolytes; 2mL of one of the above electrolytes is electrolyzed, and o-toluidine is used as a redox indicator, and the amount of H2O2 generated is quantitatively analyzed by ultraviolet spectroscopy within the wavelength range of 200-800nm. The results are shown in FIG. Figure 5 As shown, the electrolyte obtained by electrolysis with CNT@Ni without chiral modification as the anode exhibits a large absorption peak at 436nm, while the electrolyte obtained with cys-CNT@Ni as the anode does not produce an obvious absorption peak at 436nm, proving that cys-CNT@Ni can effectively inhibit the generation of H2O2.
[0062] The present invention uses a constant voltage test method, at a constant voltage of 50mA cm -2 The long-term stability test of the chiral-magnetic composite material was investigated at a current density of . Figure 6 As shown, after a stability test lasting 100 h, the activity of cys-CNT@Ni was significantly attenuated, indicating that it has good stability and is conducive to industrial application.
[0063] Comparative Example 1
[0064] This comparative example investigates the effect of chiral material concentration on catalytic activity.
[0065] Compared with Example 1, this comparative example only changed the concentration of L-cysteine in step (3), and synthesized two chiral materials according to the concentrations of L-cysteine being 5 mmol / L and 20 mmol / L respectively.
[0066] like Figure 7 As shown in Figure 2, when the concentration of L-cysteine is 5mmol / L, 10mmol / L and 20mmol / L, the corresponding cys-CNT@Ni electrocatalyst requires an overpotential of 600mV, 548mV and 569mV to reach 100mA / cm 2 This result highlights the importance of optimizing the concentration of chiral molecules. When the concentration of chiral molecules is low, fewer chiral sites cannot effectively filter intermediates with opposite electronic spin states; when the concentration of chiral molecules is high, too many non-conductive chiral molecules will reduce the overall conductivity of the composite material, resulting in poor apparent activity.
[0067] Comparative Example 2
[0068] This comparative example discusses the effect of improving the OER activity of nickel-based magnetic composite materials modified with different chiral molecules.
[0069] Compared with Example 1, this comparative example only changes the type of chiral molecules in step (3). The chiral small molecules include tartaric acid (TA) and L-glutamic acid (GA). The obtained chiral-magnetic composite material is referred to as ta-CNT@Ni, ga-CNT@Ni.
[0070] like Figure 8 As shown in Figure 2, when ta-CNT@Ni and ga-CNT@Ni are used as OER anodes, only 506mV and 479mV overvoltage are required to reach 100mA / cm 2 The OER catalytic activities of ta-CNT@Ni and ga-CNT@Ni are significantly better than those of CNT@Ni without chiral modification, indicating that the chirality-induced spin selection effect has obvious universality.
[0071] In addition, since the OER catalytic activity of ta-CNT@Ni and ga-CNT@Ni is better than that of cys-CNT@Ni, the test results of this comparative example also show that the spin selection effect of chiral small molecules with different structures will also be different, which will lead to differences in the effect of improving OER activity. In practical applications, the type, conformation, and configuration of chiral molecules can be further optimized to obtain higher catalytic activity.
[0072] Comparative Example 3
[0073] The present invention also explores the influence of the morphology of the magnetic unit on the OER activity of the composite material.
[0074] This comparative example refers to the synthesis method of Example 1. Compared with Example 1, step (2) is omitted, and Ni(oxy)hydroxide nanosheets are directly modified with L-cysteine. The composite material finally obtained is named cys-Ni(oxy)hydroxide.
[0075] like Fig. 9 As shown, the activity of cys-Ni(oxy)hydroxide is higher than that of Ni(oxy)hydroxide in the entire test range, indicating that the morphology of the magnetic material does not affect the synergy between the chirality-induced spin selection effect and the magnetic effect generated by the magnetic unit.
[0076] But from Fig. 9It can also be seen that although there are differences in the activities of cys-Ni(oxy)hydroxide and Ni(oxy)hydroxide, the differences are not obvious. This is mainly because the surface of Ni(oxy)hydroxide is smoother than that of CNT@Ni, which is not conducive to the adsorption of more chiral molecules and produces fewer synergistic sites. Therefore, in the actual process, the activity can be further optimized by regulating the surface and interfacial properties of the magnetic unit.
[0077] Comparative Example 4
[0078] In this comparative example, metallic nickel was replaced with metallic iron, and iron-catalyzed carbon nanotubes were produced to explore whether different types of metals can also synergize with chiral small molecules to enhance OER activity.
[0079] The synthesis method is as follows:
[0080] FeCl3·6H2O (0.4 g) and Na2SO4 (0.24 g) were dissolved in 35 mL of aqueous solution and then transferred to a 50 mL stainless steel autoclave lined with polytetrafluoroethylene. A 2 cm*2 cm carbon cloth was immersed in the solution, hydrothermally treated at 120°C for 4 h and then cooled to room temperature to obtain iron-based nanowires. Then, the iron-based magnetic unit (CNT@Fe) and chiral-iron-based magnetic composite material (cys-CNT@Fe) were synthesized according to Example 1.
[0081] like Fig.10 As shown in Figure A, CNT@Fe has a nanotube morphology similar to that of CNT@Ni, where Fe particles are embedded inside the carbon nanotubes. Fig.10 As shown in Figure B, the OER activity of cys-CNT@Fe is also better than that of CNT@Fe, indicating that the synergistic effect of the chiral unit and the magnetic unit is not affected by the composition of the magnetic material and can also improve the OER activity.
[0082] It can be seen from Comparative Examples 1 to 4 that the chirality-induced spin selection effect and the magnetic effect generated by the magnetic unit can synergistically enhance the OER activity. The synergistic effect will not disappear due to changes in the composition, morphology, structure and concentration of the magnetic unit, but there are slight differences in its strength, which shows that the chiral-magnetic synergy has good universality.
[0083] In addition, the present invention also discusses the effect of the modification process on the OER activity of the composite material when the chiral molecule modifies the magnetic unit in Example 1, including the length of the oscillation time, whether the oscillation process is heated, and whether there is oscillation or not.
[0084] Comparative Example 5
[0085] Compared with Example 1, this comparative example only changed the shaking time in step (3). This comparative example explored the activity of samples prepared with shaking times of 0.5 h and 2 h.
[0086] As shown in Table 1, when the shaking time is 0.5 h, the activity of the synthesized composite material is lower than that of the sample shaken for 1 h in Example 1; but as the shaking time increases to 2 h, the activity of the obtained composite material is not significantly better than that of Example 1. The results of this comparative example prove that without changing the other experimental steps of Example 1, the performance-time cost of the composite material obtained when the shaking time is 1 h in step (3) is optimal.
[0087] Comparative Example 6
[0088] Compared with Example 1, in this comparative example, only in step (3), the external temperature was kept constant at 40° C. and 50° C. during the oscillation modification process.
[0089] As shown in Table 1, under the premise of maintaining the oscillation time at 1 h, the added temperature did not significantly improve the activity of the composite material, and even the activity was attenuated when oscillating at 50 ° C. This may be because when the temperature is too high, the adsorption rate of the chiral molecules on the magnetic unit is accelerated and the desorption rate is also increased.
[0090] Comparative Example 7
[0091] Compared with Example 1, in this comparative example, only in step (3), the modification process was not assisted by shaking, and the modification time was maintained at 1 hour.
[0092] Table 1 shows comparative examples 5, 6 and 7 of the present invention. The composite materials obtained by adjusting the oscillation time, oscillation temperature and whether to oscillate in step (3) of Example 1 reach 100 mA / cm in 1.0 M KOH electrolyte. 2 The overvoltage value required for the current density.
[0093] Table 1 Overpotentials of different preparation conditions
[0094]
[0095] It can be seen from Table 1 that the activity of the composite material synthesized without oscillation is lower than that of the sample synthesized with the assistance of oscillation. Therefore, when conditions permit, auxiliary methods including oscillation can be given priority to improve the modification effect of the chiral unit on the magnetic unit.
[0096] In general, the present invention utilizes the synergistic effect between the spin synergy effect induced by chiral molecules and the magnetic effect generated by magnetic materials to enhance the activity of the anode OER reaction of water electrolysis. The present invention has excellent universality, and its synergistic effect will not disappear due to changes in the composition, morphology, structure, concentration and other conditions of the magnetic material, but the strength of its synergistic effect will have a certain impact. The good universality of the chiral-magnetic material combination form of the present experimental invention increases the flexibility of the enterprise, and the structure and composition of the chiral-magnetic material can be reasonably selected according to the equipment, cost requirements and other conditions of the enterprise to achieve the greatest economic value and social value.
[0097] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A chiral-magnetic composite material, characterized in that: The composite material is a magnetic material with a chiral material loaded on its surface.
2. The chiral-magnetic composite material according to claim 1, characterized in that: The magnetic material is supported on a conductive base material.
3. The chiral-magnetic composite material according to claim 1, characterized in that: The magnetic material is a nickel-based magnetic material or an iron-based magnetic material.
4. The chiral-magnetic composite material according to claim 1, characterized in that: The morphology of the magnetic material is nanotube or nanosheet.
5. The chiral-magnetic composite material according to claim 1, characterized in that: The chiral material is a chiral small molecule, or an inorganic nanoparticle with a chiral group or a chiral morphology which is independently constructed by the chiral small molecule.
6. The chiral-magnetic composite material according to claim 5, characterized in that: The chiral small molecule is selected from at least one of tartaric acid, L-cysteine, L-tryptophan and L-ascorbic acid.
7. The method for preparing the chiral-magnetic composite material according to any one of claims 1 to 6, characterized in that: The steps include: (1) Preparation of magnetic materials; (2) Loading chiral materials on the surface of magnetic materials to obtain chiral-magnetic composite materials.
8. The method according to claim 7, characterized in that In step (1), the synthesis method of the magnetic material includes but is not limited to hydrothermal and high-temperature calcination, or a combination of these.
9. The method according to claim 7, characterized in that: In step (2), the chiral material is modified onto the surface of the magnetic material by means of ultrasound, vibration, and stirring.
10. Use of the chiral-magnetic composite material according to any one of claims 1 to 6 as an electrocatalyst for oxygen evolution reaction, characterized in that: The electrolyte for the oxygen evolution reaction is selected from an alkaline electrolyte.