Microstructure display method of metal ytterbium

Through the grinding, polishing and electrolytic coating of metal ytterbium samples, an interference film is formed to display its grain structure under a polarized light microscope, solving the problem that metal ytterbium microscope is difficult to truly manifest, and achieving efficient and simple microscopy Organizational analysis.

CN118961325APending Publication Date: 2024-11-15GUOBIAO BEIJING TESTING & CERTIFICATION CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410885825.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing material microstructure research techniques cannot effectively avoid deformation interference and oxidation caused by metal bblt samples during corrosion, resulting in the inability to obtain a clear and true microstructure structure.

Method used

Metal ytterbium was used as the experimental sample, and the grain structure was displayed under a silicon carbide sandpaper grinding, silicon oxide polishing and electrolytic coating of mixed solutions of methanol, ethylene glycol and nitric acid.

Benefits of technology

The clear display of metal yotterbium microstructure is achieved, the grain profile is obvious and different grain orientations show different colors, solving the technical difficulties of metal yotterbium microstructure characterization and providing an efficient and simple corrosion method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118961325A_ABST
    Figure CN118961325A_ABST
Patent Text Reader

Abstract

The invention discloses a microscopic structure display method of metal ytterbium, and belongs to the technical field of physical testing. According to the method, a mixed solution of methanol, ethylene glycol and nitric acid is used as an electrolyte, a metal ytterbium sample is used as an anode, a stainless steel plate is used as a cathode, the sample is coated with a film under the voltage of 1-6V, observation is carried out under a polarized light microscope, the prepared sample is obvious in grain boundary contour, and grains of different grain samples show different colors under polarized light. According to the method, the problem that the microscopic structure of the metal ytterbium sample is difficult to truly display is effectively solved, and a better technical support is provided for subsequently developing metal ytterbium microscopic technology research and product quality control. All formulas of the corrosive are common reagents in laboratories, and the corrosion method is simple, convenient, efficient, good in reproducibility, economical and practical.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of physical testing, and in particular relates to a method for displaying the microstructure of metal ytterbium. Background Art

[0002] Due to its unique properties, metallic ytterbium is widely used in pressure sensors, nuclear energy, conductive ceramics, modifiers, target materials and other fields.

[0003] The microstructure of ytterbium metal has a significant impact on the performance of the product. For high-purity ytterbium targets, the finer the target grains, the narrower the grain distribution, the higher the sputtering efficiency and the better the uniformity of the coating thickness. The clear and true display of the microstructure of ytterbium metal is the basis for studying its microstructure.

[0004] Due to its active chemical properties and soft texture, metallic ytterbium easily reacts with water, abrasive particles, air, etc. to produce an oxide layer, and is easily embedded in abrasives, polishing agents and other particles to produce a deformation interference layer. During the corrosion process, due to its active properties, it reacts more violently, is prone to over-corrosion, and it is difficult to obtain a clear and true microstructure.

[0005] So far, the existing material microstructure research technology at home and abroad has not yet involved the microstructure display of metal ytterbium. The samples prepared by the metallographic sample preparation method of other metal materials disclosed in the prior art inevitably have a deformation interference layer, and the material surface is severely oxidized and corroded, and the real structure cannot be obtained. Rare earth metals are key raw materials for the research and development of high-tech materials. Conducting research on the microstructure of metal ytterbium is in line with the development direction of high-end rare earth materials. The microstructure display method involved is a key technology to ensure the quality of rare earth metal ytterbium material products, and new research and exploration are needed. Summary of the invention

[0006] In view of the above problems, the purpose of the present invention is to provide an effective method for displaying the microstructure of metal ytterbium. The present invention uses metal ytterbium as an experimental sample, and after sampling, grinding, polishing, anodic coating and other steps, a metallographic sample for microstructure observation with obvious grains and clear grain boundaries can be obtained.

[0007] A method for displaying the microstructure of metal ytterbium mainly comprises the following steps:

[0008] 1) The sample is ground from coarse to fine on silicon carbide sandpaper of different meshes. Each time the sandpaper is changed, the sample needs to be rotated at a certain angle until the previous scratch is removed;

[0009] 2) Polish the ground sample with a silicon oxide polishing agent with a particle size less than 1 μm until the scratches on the sample surface are removed. During the polishing process, spray anhydrous ethanol to prevent oxidation of the sample.

[0010] 3) Using a mixed solution of methanol, ethylene glycol and nitric acid as the electrolyte, the sample as the anode and the stainless steel plate as the cathode, the sample is electrolytically coated;

[0011] 4) Rinse the coated sample in deionized water, blow dry it, and then observe it under a microscope with polarized light to analyze its microstructure.

[0012] Further, the silicon carbide sandpaper described in step 1) includes, but is not limited to, 500 mesh, 1000 mesh and 2400 mesh, 320 mesh, 800 mesh and 2500 mesh, and a combination of 240 mesh, 500 mesh, 1000 mesh and 2400 mesh from coarse to fine. Each time the sandpaper is changed, the sample is rotated 45°-135° until the previous scratch is removed.

[0013] Furthermore, the particle size of the silicon oxide polishing agent less than 1 μm in step 2) includes but is not limited to 0.2 μm, 0.05 μm, and 0.04 μm. The polishing time is 1 min to 3 min.

[0014] Furthermore, in the electrolyte described in step 3), the volume fractions of each raw material are: 10-25 parts of methanol, 20-50 parts of ethylene glycol, and 1-10 parts of nitric acid; that is, the volume ratio of methanol, ethylene glycol, and nitric acid is (10-25): (20-50): (1-10), wherein the purity of methanol is ≥ 99.0wt%, the purity of ethylene glycol is ≥ 99.0wt%, and the concentration of nitric acid is 40.0wt% to 60.0wt%. The voltage used for the electrolytic coating is 1V to 6V, and the electrolysis time is 5s to 40s.

[0015] Using the electrolyte described in step 3), under the action of electric current, the surface of the metal ytterbium reacts electrochemically with the mixed solution of methanol + ethylene glycol + nitric acid to form an interference film. Due to the different microstructures in the sample or the same structure but different grain orientations, the thickness of the interference film generated will be different, so that under a polarized light microscope, different microstructures or grains with different grain orientations in the same microstructure will show different colors, so that the microscopic structural characteristics such as the grain structure morphology of the metal ytterbium are clearly shown through the difference in color contrast.

[0016] The volume ratio of methanol, ethylene glycol and nitric acid in the electrolyte should be controlled within the range of (10-25):(20-50):(1-10). If it exceeds this range, chemical reaction and electrochemical reaction will occur simultaneously on the sample surface, and the chemical reaction will be dominant, so that the interference film cannot be effectively formed. Under a polarized light microscope, the grain structure morphology cannot be displayed.

[0017] The advantages of the present invention are as follows:

[0018] (1) The present invention innovatively discloses a method for displaying the microstructure of metal ytterbium, filling the technical gap in the field of metal ytterbium microstructure analysis.

[0019] (2) The metallographic sample of ytterbium prepared by the present invention has a clear microstructure, obvious grain outlines, and grains with different grain orientations show different colors, which effectively solves the technical problem of characterizing the microstructure of ytterbium.

[0020] (3) The present invention uses a mixed solution of methanol + ethylene glycol + nitric acid to perform anodic coating on metal ytterbium, and displays the real structure of metal ytterbium under polarized light. The formula of the etchant is a common laboratory reagent, and the etching method is simple, efficient, reproducible, economical and practical. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a microstructure picture of the metal ytterbium prepared in Example 1;

[0022] Figure 2 This is a microstructure picture of the metal ytterbium prepared in Example 2;

[0023] Figure 3 This is a microstructure picture of the metal ytterbium prepared in Example 3;

[0024] Figure 4 The microstructure picture of the metal ytterbium prepared in Comparative Example 1;

[0025] Figure 5 This is a microstructure picture of the metal ytterbium prepared in Comparative Example 2. DETAILED DESCRIPTION

[0026] The method for displaying the microstructure of metal ytterbium of the present invention comprises the following steps:

[0027] 1) The sample is ground on silicon carbide sandpaper of different meshes from coarse to fine. Each time the sandpaper is changed, the sample needs to be rotated at a certain angle (45°-135°) until the previous scratch is removed; silicon carbide sandpaper from coarse to fine includes but is not limited to 500 mesh, 1000 mesh and 2400 mesh, 320 mesh, 800 mesh, 2500 mesh and 240 mesh, 500 mesh, 1000 mesh and 2400 mesh.

[0028] 2) The ground sample is polished with a silicon oxide polishing agent with a particle size of less than 1 μm until the wear marks on the sample surface are removed. During the polishing process, anhydrous ethanol is sprayed to prevent the sample from oxidizing. The particle size of the silicon oxide polishing agent with a particle size of less than 1 μm includes but is not limited to 0.2 μm, 0.05 μm, and 0.04 μm.

[0029] 3) Prepare a mixed solution of methanol + ethylene glycol + nitric acid, where the volume ratio of methanol (≥99.0wt%), ethylene glycol (≥99.0wt%), and nitric acid (40.0wt% to 60.0wt%) is (10-25):(20-50):(1-10). Use the sample as the anode and perform anode coating in the prepared electrolyte at a voltage of 1V to 6V for a coating time of 5s to 40s.

[0030] 4) Rinse the coated sample in deionized water, blow dry it, and then observe it under a microscope with polarized light to analyze its microstructure.

[0031] Example 1

[0032] The metal ytterbium sample was subjected to 500 # -1000 # -2400 # After grinding with silicon carbide sandpaper of different mesh sizes, polish with 0.05μm silicon oxide polishing agent until the wear marks on the sample surface are removed. The polishing time is about 2min. During the polishing process, spray anhydrous ethanol to prevent the sample from oxidizing. Mix 10ml methanol (≥99.0wt%), 50ml ethylene glycol (≥99.0wt%), and 10ml nitric acid (40.0wt%) to prepare an electrolyte. Use the sample as the anode and the stainless steel plate as the cathode, adjust the voltage to 1V, and electrolyze for 40s.

[0033] Rinse the coated samples in deionized water, blow dry them, and then observe them under a polarized light microscope to analyze their microstructure. Figure 1 As shown, the grain boundaries are clearly delineated and grains sampled from different grains appear in different colors under polarized light.

[0034] Example 2

[0035] The metal ytterbium sample was heated at 320 # -800 # -2500 # After grinding with silicon carbide sandpaper of different mesh sizes, polish with 0.2μm silicon oxide polishing agent until the wear marks on the sample surface are removed. The polishing time is about 1min. During the polishing process, spray anhydrous ethanol to prevent the sample from oxidation. Mix 25ml methanol (≥99.0wt%), 20ml ethylene glycol (≥99.0wt%), and 1ml nitric acid (60.0wt%) to prepare an electrolyte. Use the sample as the anode and the stainless steel plate as the cathode, adjust the voltage to 6V, and electrolyze for 5s.

[0036] Rinse the coated samples in deionized water, blow dry them, and then observe them under a polarized light microscope to analyze their microstructure. Figure 2As shown, the grain boundaries are clearly delineated and grains sampled from different grains appear in different colors under polarized light.

[0037] Example 3

[0038] The metal ytterbium sample was subjected to 240 # -500 # -1000 # -2400 # After grinding with silicon carbide sandpaper of different mesh sizes, polish with 0.2μm silicon oxide polishing agent until the wear marks on the sample surface are removed. The polishing time is about 2.5min. During the polishing process, spray anhydrous ethanol to prevent the sample from oxidation. Mix 15ml methanol (≥99.0wt%), 40ml ethylene glycol (≥99.0wt%), and 5ml nitric acid (50.0wt%) to prepare an electrolyte. Use the sample as the anode and the stainless steel plate as the cathode, adjust the voltage to 3V, and electrolyze for 25s.

[0039] Rinse the coated samples in deionized water, blow dry them, and then observe them under a polarized light microscope to analyze their microstructure. Figure 3 As shown, the grain boundaries are clearly delineated and grains sampled from different grains appear in different colors under polarized light.

[0040] Comparative Example 1

[0041] In accordance with the method described in Example 1, the metal ytterbium is ground and polished, and then placed in a mixed solution of 10 ml methanol (≥99.0 wt%), 50 ml ethylene glycol (≥99.0 wt%), and 10 ml nitric acid (40.0 wt%). After corrosion at room temperature for 40 seconds, the sample is taken out, rinsed in deionized water, blown dry, and observed under a microscope with polarized light.

[0042] Comparative Example 1 Compared with Example 1, the same solution was used but no electrolytic coating was used. The microstructure of the Figure 4 As shown, the morphology of the sample grains is unclear, and grains with different orientations do not show obvious color contrast differences under polarized light.

[0043] Comparative Example 2

[0044] In accordance with the method described in Example 1, the metal ytterbium was ground and polished, and then placed in a mixed solution of 90 ml ethanol (≥99.0 wt%) and 4 ml nitric acid (40.0 wt%) for corrosion at room temperature for 10 s. The sample was then taken out, rinsed in deionized water, blown dry, and observed under a microscope with polarized light.

[0045] Comparative Example 2 adopts the conventional rare earth metal corrosion method, and the microstructure is as follows Figure 5The grain morphology of the sample is also unclear, and grains with different orientations do not show obvious color contrast differences under polarized light.

[0046] In summary, the present invention innovatively discloses a method for displaying the microstructure of metal ytterbium, which fills the technical gap in the field of metal ytterbium microstructure analysis. The present invention uses a mixed solution of methanol + ethylene glycol + nitric acid as an electrolyte, a metal ytterbium sample as an anode, and a stainless steel plate as a cathode. The sample is coated at a voltage of 1V to 6V, and the real structure of metal ytterbium is displayed under polarized light. The formulas of the etchants are all common laboratory reagents, and the corrosion method is simple, efficient, reproducible, economical and practical.

[0047] Under polarized light microscope, the sample prepared by the present invention has obvious grain boundary contours, and the grains sampled from different grains show different colors under polarized light. The present invention effectively solves the problem that the microstructure of metal ytterbium samples is difficult to truly display, and provides good technical support for subsequent research on metal ytterbium microscopy technology and product quality control. The etchant formulas of the present invention are all common laboratory reagents, and the corrosion method is simple, efficient, reproducible, economical and practical.

Claims

1. A method for displaying the microstructure of metal ytterbium, comprising the following steps: 1) The sample is ground from coarse to fine on silicon carbide sandpaper of different meshes. Each time the sandpaper is changed, the sample is rotated at a certain angle until the previous scratch is removed; 2) Polish the ground sample with a silicon oxide polishing agent with a particle size less than 1 μm until the scratches on the sample surface are removed. During the polishing process, spray anhydrous ethanol to prevent oxidation of the sample. 3) Using a mixed solution of methanol, ethylene glycol and nitric acid as the electrolyte, the sample as the anode and the stainless steel plate as the cathode, the sample is electrolytically coated; 4) Rinse the coated sample in deionized water, blow dry it, and then observe it under a microscope with polarized light to analyze its microstructure.

2. The method for displaying the microstructure of metal ytterbium according to claim 1, characterized in that: The silicon carbide sandpaper includes 500 mesh, 1000 mesh and 2400 mesh, 320 mesh, 800 mesh and 2500 mesh, and a combination of 240 mesh, 500 mesh, 1000 mesh and 2400 mesh from coarse to fine.

3. The method for displaying the microstructure of metal ytterbium according to claim 2, characterized in that: Each time the sandpaper is changed, the sample is rotated 45-135° until the previous scratch is removed.

4. The method for displaying the microstructure of metal ytterbium according to claim 1, characterized in that: The particle sizes of the silicon oxide polishing agent smaller than 1 μm include 0.2 μm, 0.05 μm and 0.04 μm.

5. The method for displaying the microstructure of metal ytterbium according to claim 4, characterized in that: The polishing time is 1min to 3min.

6. The method for displaying the microstructure of metal ytterbium according to claim 1, characterized in that: In the electrolyte, the volume proportions of the raw materials are: 10-25 parts of methanol, 20-50 parts of ethylene glycol, and 1-10 parts of nitric acid.

7. The method for displaying the microstructure of metal ytterbium according to claim 6, characterized in that: The purity of the methanol is ≥99.0wt%, the purity of the ethylene glycol is ≥99.0wt%, and the concentration of the nitric acid is 40.0wt% to 60.0wt%.

8. The method for displaying the microstructure of metal ytterbium according to claim 1, characterized in that: During the electrolytic coating, the voltage used is 1V to 6V and the electrolysis time is 5s to 40s.

Citation Information

Cited By

  • Macrostructure inspection method of high-activity and high-purity rare earth metal gadolinium target material

    CN121558455A