Modified lithium-rich manganese-based positive electrode material as well as preparation method and application thereof

By co-doping vanadium doping and vanadium cerium in lithium-rich manganese-based positive electrode material, the core-shell structure is formed, and the problems of insufficient coulomb efficiency and cycle stability of existing materials are solved, and efficient discharge capacity and cycle performance are achieved. , and simplifies the preparation process.

CN118970014APending Publication Date: 2024-11-15JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202411268159.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing lithium-rich manganese-based cathode materials have low Coulomb efficiency and insufficient cycle stability in practical applications, resulting in severe attenuation of voltage and capacity. The existing modification methods have problems with the difficulty of using and controlling materials.

Method used

By doping the core of the lithium-rich manganese-based positive electrode material and co-doping vanadium-cerium in the coating layer, a core-shell structure is formed, which inhibits material structure transformation, improves structural stability, and is blocked by a dense coating layer. Contact the electrolyte to avoid side reactions.

Benefits of technology

The discharge capacity and cyclic performance of the modified lithium-rich manganese-based positive electrode material are significantly improved, the structural stability and electrochemical properties of the material are ensured, the dissolution and side reaction of Mn are avoided, and the preparation process is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970014A_ABST
    Figure CN118970014A_ABST
Patent Text Reader

Abstract

The invention provides a modified lithium-rich manganese-based positive electrode material as well as a preparation method and application thereof. The modified lithium-rich manganese-based positive electrode material comprises an inner core and a coating layer coating the surface of the inner core, the inner core comprises a vanadium-doped lithium-rich manganese-based positive electrode material, and the coating layer comprises a vanadium-cerium co-doped lithium-rich manganese-based positive electrode material. Vanadium doping is carried out on the inner core of the modified lithium-rich manganese-based positive electrode material, and vanadium-cerium co-doping in the coating layer is cooperatively matched, so that the capacity and the cycle performance of the modified lithium-rich manganese-based positive electrode material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion batteries and relates to a modified lithium-rich manganese-based positive electrode material and a preparation method and application thereof. Background Art

[0002] Lithium-rich manganese-based cathode materials are a new type of lithium-ion battery cathode materials with the advantages of high capacity, high energy density and low cost. Although lithium-rich manganese-based cathode materials have many advantages, they still face some challenges in practical applications, such as low initial coulombic efficiency, insufficient cycle stability, and serious attenuation of voltage and capacity.

[0003] To overcome these challenges, researchers are using a variety of methods to improve the performance of lithium-rich manganese-based cathode materials, such as doping modification, surface coating and optimized preparation process, in order to achieve their widespread application in the next generation of high-energy density lithium-ion batteries; however, the above-mentioned modification methods still have defects to varying degrees.

[0004] CN113788500A discloses a surface modification method of a lithium-rich manganese-based positive electrode material and a lithium-rich manganese-based positive electrode material. The lithium-rich manganese-based material is mixed with a stannous salt solution to obtain a lithium-rich manganese-based material with a tin surface modification, and a higher discharge capacity and cycle performance are obtained. However, the stannous salt solution is harmful to the human body and will cause certain harm to operators during the production process. CN110890541A discloses a preparation method and a lithium-ion battery of a surface-modified lithium-rich manganese-based positive electrode material. The surface of the lithium-rich manganese-based material is modified by adding a fast ion conductor coating agent such as a phosphate solution, so that the total amount of residual alkali on the surface of the material is significantly reduced, and the first coulomb efficiency and rate performance are significantly improved. However, the surface modification of the fast ion conductor coating liquid is affected by the liquid concentration and the uniformity of ion dispersion, and the modification process is not easy to control.

[0005] Therefore, how to improve the capacity and cycle performance of lithium-rich manganese-based positive electrode materials is a technical problem that needs to be solved urgently. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a modified lithium-rich manganese-based positive electrode material and its preparation method and use. The present invention performs vanadium doping on the core of the modified lithium-rich manganese-based positive electrode material, and cooperates with the vanadium-cerium co-doping in the coating layer to improve the capacity and cycle performance of the modified lithium-rich manganese-based positive electrode material.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In the first aspect, the present invention provides a modified lithium-rich manganese-based positive electrode material, which comprises a core and a coating layer coated on the surface of the core; the core comprises a vanadium-doped lithium-rich manganese-based positive electrode material, and the coating layer comprises a vanadium-cerium co-doped lithium-rich manganese-based positive electrode material.

[0009] The modified lithium-rich manganese-based positive electrode material provided by the present invention is doped with vanadium in the core, and the vanadium exists in the form of a lithium vanadate (Li2VO3) phase structure, which can inhibit the transformation of the material from a layered structure to a spinel-like structure, is beneficial to stabilizing the material structure, and improving the structural stability of the positive electrode material; and the vanadium and cerium co-doping in the coating layer ensures that the coating layer formed by the outer shell has a high density, and the coating layer can also effectively block the contact between the material core and the electrolyte, avoiding the dissolution of Mn and reducing the occurrence of side reactions when the material contacts the electrolyte during the reaction process; the core and the coating layer cooperate with each other to jointly improve the discharge capacity and cycle performance of the modified lithium-rich manganese-based positive electrode material.

[0010] In the present invention, vanadium doping in the core and vanadium-cerium co-doping in the coating layer cooperate synergistically and are indispensable. If vanadium doping is not performed in the core, it is impossible to inhibit material phase transformation and stabilize the material structure. If vanadium-cerium co-doping is not performed in the coating layer, the rate performance and cycle performance of the lithium-rich manganese-based positive electrode material cannot be improved.

[0011] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0012] Preferably, the molar ratio of vanadium in the inner core is smaller than the molar ratio of vanadium in the coating layer.

[0013] In the present invention, the molar proportion of vanadium refers to the molar proportion of vanadium in the core or the molar proportion of vanadium in the coating layer, based on the total molar proportion of all metal elements in the core or the coating layer being 100%.

[0014] In the present invention, the vanadium content in the core is lower than that in the coating layer, which is more conducive to ensuring good electrochemical performance of nickel.

[0015] Preferably, the chemical formula of the core is Li x Ni a Mn b V c O2, where 1.1≤x≤1.6, 0.14≤a≤0.35, 0.6≤b≤0.85, 0.01≤c≤0.05.

[0016] For example, the x may be 1.1, 1.2, 1.3, 1.4, 1.5 or 1.6, etc.; the a may be 0.14, 0.15, 0.18, 0.2, 0.23, 0.25, 0.28, 0.3, 0.33 or 0.35, etc.; the b may be 0.6, 0.63, 0.65, 0.68, 0.7, 0.73, 0.75, 0.78, 0.8, 0.83 or 0.85, etc.; the c may be 0.01, 0.02, 0.03, 0.04 or 0.05, etc.

[0017] In the present invention, by regulating the stoichiometric ratio of vanadium in the inner core to 0.01≤c≤0.05, it is more conducive to inhibiting the transformation of the material from a layered structure to a spinel-like structure, thereby improving the structural stability of the positive electrode material.

[0018] Preferably, the chemical formula of the coating layer is Li y Mn k V m Ce n O2, where 1.1≤y≤1.6, 0.85≤k≤0.95, 0.02≤m≤0.06, 0.03≤n≤0.09.

[0019] For example, the x may be 1.1, 1.2, 1.3, 1.4, 1.5 or 1.6, etc.; the k may be 0.850.860.870.880.890.90.910.920.930.940.95, the m may be 0.02, 0.03, 0.04, 0.05 or 0.06, etc., and the n may be 0.03, 0.04, 0.05, 0.06, 0.07, 0.08 or 0.09, etc.

[0020] In the present invention, the stoichiometric ratio of vanadium in the coating layer is further regulated to be 0.02≤m≤0.06, and the stoichiometric ratio of cerium is 0.03≤n≤0.09, so that the outer shell can better form a high-density coating layer. The coating layer can effectively block the contact between the core of the material and the electrolyte, avoid the dissolution of manganese, and reduce the occurrence of side reactions when the material contacts the electrolyte during the reaction process, thereby improving the discharge capacity and rate performance of the lithium-rich manganese-based positive electrode material.

[0021] Preferably, the D50 of the lithium-rich manganese-based positive electrode material is 6 to 15 μm, for example, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm or 15 μm.

[0022] Preferably, the D50 of the inner core is 5 to 12 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm or 12 μm, and the shell thickness of the coating layer is 1 to 3 μm, for example, 1 μm, 2 μm or 3 μm.

[0023] In a second aspect, the present invention provides a method for preparing the modified lithium-rich manganese-based positive electrode material as described in the first aspect, the preparation method comprising the following steps:

[0024] Adding a first mixed metal salt solution, a first precipitant solution and a first complexing agent solution in parallel to perform a first coprecipitation reaction to obtain a precursor core;

[0025] After the precursor core is obtained, a second mixed metal salt solution, a second precipitant solution and a second complexing agent solution are added in parallel to perform a second coprecipitation reaction to obtain a precursor material;

[0026] Mixing the precursor material with a lithium source and sintering to obtain the modified lithium-rich manganese-based positive electrode material;

[0027] The first mixed metal salt solution includes vanadium ions and manganese ions, and the second mixed metal salt solution includes vanadium ions, cerium ions and manganese ions.

[0028] The preparation method provided by the present invention obtains a core-shell structure in the precursor preparation stage, and realizes the doping of vanadium in the core and the co-doping of vanadium and cerium in the coating layer in the precursor stage, thereby realizing the uniform doping of the doping elements in the bulk phase. After subsequent sintering treatment after mixing with a lithium source, a modified lithium-rich manganese-based positive electrode material with a stable structure and excellent performance is obtained. The preparation method is simple to operate and does not require additional preparation costs.

[0029] Preferably, the molar amount ratio of vanadium in the first mixed metal salt solution is smaller than the molar amount ratio of vanadium in the second mixed metal salt solution.

[0030] It should be noted that the molar ratio of vanadium in the mixed metal salt solution is the molar ratio of vanadium therein, taking the sum of the total molar ratios of metal elements in the mixed metal salt solution as 100%, which is consistent with the molar ratio of vanadium in the core and the coating layer in the final modified lithium-rich manganese-based positive electrode material.

[0031] Preferably, the chemical formula of the precursor core is Ni a Mn b V c (OH)2, wherein 0.14≤a≤0.35, 0.6≤b≤0.85, and 0.01≤c≤0.05.

[0032] Preferably, the chemical formula of the coating layer in the precursor material is Mn k V m Ce n (OH)2, wherein 0.85≤k≤0.95, 0.02≤m≤0.06, 0.03≤n≤0.09.

[0033] Preferably, the reaction temperatures of the first coprecipitation reaction and the second coprecipitation reaction are independently 45-70°C, such as 45°C, 50°C, 55°C, 60°C, 65°C or 70°C.

[0034] Preferably, the pH values ​​of the first coprecipitation reaction and the second coprecipitation reaction are each independently 9 to 12, for example, 9, 9.3, 9.5, 9.8, 10, 10.3, 10.5, 10.8, 11, 11.3, 11.5, 11.8 or 12, etc.

[0035] Preferably, the reaction time of the first coprecipitation reaction is 50 to 200 h, for example, 50 h, 60 h, 70 h, 80 h, 90 h, 100 h, 110 h, 120 h, 130 h, 140 h, 150 h, 160 h, 170 h, 180 h, 190 h or 200 h, etc.

[0036] Preferably, the reaction time of the second coprecipitation reaction is 8 to 30 h, for example, 8 h, 10 h, 13 h, 15 h, 18 h, 20 h, 23 h, 25 h, 28 h or 30 h.

[0037] Preferably, the stirring speeds of the first coprecipitation reaction and the second coprecipitation reaction are independently 200-400 rpm, such as 200 rpm, 250 rpm, 300 rpm, 350 rpm or 400 rpm.

[0038] It is understood that in the preparation process of the precursor provided by the present invention, the preparation process can be adaptively selected and adjusted under the premise of ensuring the limited stoichiometric ratio of each substance in the precursor;

[0039] 1) Specifically, during the first coprecipitation reaction, the preparation parameters can be adjusted as follows:

[0040] Optionally, the concentration of the first mixed metal salt solution is 50 to 200 g / L, such as 50 g / L, 75 g / L, 100 g / L, 125 g / L, 150 g / L, 175 g / L or 200 g / L, etc., and the specific salt type is selected from at least one of sulfate, chloride, nitrate or acetate;

[0041] Optionally, the mass concentration of the first precipitant solution is 15-45%, for example, 15%, 20%, 25%, 30%, 35%, 40% or 45%, etc., and the specific type of precipitant is selected from at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium sulfide or sodium acetate;

[0042] Optionally, the mass concentration of the first complexing agent solution is 10-30%, such as 10%, 15%, 20%, 25% or 30%, etc., and the specific type of complexing agent is selected from at least one of ammonia water, carbonic acid, lactic acid or triethanolamine;

[0043] Optionally, the feed flow rate of the first mixed metal salt solution is 20 to 40 L / h, such as 20 L / h, 25 L / h, 30 L / h, 35 L / h or 40 L / h;

[0044] Optionally, the feed flow rate of the first precipitant solution is 8 to 14 L / h, such as 8 L / h, 9 L / h, 10 L / h, 11 L / h, 12 L / h, 13 L / h or 14 L / h, etc.;

[0045] Optionally, the feed flow rate of the first complexing agent solution is 1 to 5 L / h, such as 1 L / h, 2 L / h, 3 L / h, 4 L / h or 5 L / h;

[0046] The particle size of the precursor core is the particle size of the core in the positive electrode material;

[0047] 2) Specifically, during the second coprecipitation reaction, the preparation parameters can be adjusted as follows:

[0048] Optionally, the concentration of the second mixed metal salt solution is 50 to 200 g / L, such as 50 g / L, 75 g / L, 100 g / L, 125 g / L, 150 g / L, 175 g / L or 200 g / L, etc., and the specific salt type is selected from at least one of sulfate, chloride, nitrate or acetate;

[0049] Optionally, the mass concentration of the second precipitant solution is 15-45%, for example, 15%, 20%, 25%, 30%, 35%, 40% or 45%, etc., and the specific type of precipitant is selected from at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium sulfide or sodium acetate;

[0050] Optionally, the mass concentration of the second complexing agent solution is 10-30%, such as 10%, 15%, 20%, 25% or 30%, etc., and the specific type of complexing agent is selected from at least one of ammonia water, carbonic acid, lactic acid or triethanolamine;

[0051] Optionally, the feed flow rate of the second mixed metal salt solution is 20 to 40 L / h, such as 20 L / h, 25 L / h, 30 L / h, 35 L / h or 40 L / h, etc.;

[0052] Optionally, the feed flow rate of the second precipitant solution is 8 to 14 L / h, such as 8 L / h, 9 L / h, 10 L / h, 11 L / h, 12 L / h, 13 L / h or 14 L / h, etc.;

[0053] Optionally, the feed flow rate of the second complexing agent solution is 1 to 5 L / h, such as 1 L / h, 2 L / h, 3 L / h, 4 L / h or 5 L / h;

[0054] The precursor material includes a precursor core and a coating layer on the surface of the precursor core, and the thickness of the coating layer in the precursor material is the thickness value of the coating layer in the positive electrode material;

[0055] Optionally, after the second coprecipitation reaction is completed, an aging treatment is performed, and after the aging treatment, alkali washing and water washing are performed in sequence, and drying is performed to obtain a precursor material;

[0056] Under the above-mentioned conditions of preparation raw materials and preparation parameters, those skilled in the art can make adaptive selections and adjustments according to specific needs.

[0057] Preferably, the sintering includes performing a first sintering and a second sintering in sequence.

[0058] In the present invention, by staged sintering, the temperature, atmosphere and time can be better controlled step by step, and the microstructure, grain size and composition uniformity of the positive electrode material can be better adjusted, thereby optimizing the electrochemical performance of the material.

[0059] Preferably, the heating rates of the first sintering and the second sintering are independently 2 to 10°C / min, for example, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, etc.

[0060] Preferably, the sintering temperature of the first sintering is 450-550°C, for example, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C or 550°C.

[0061] Preferably, the sintering time of the first sintering is 2 to 10 h, for example, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h.

[0062] Preferably, the sintering temperature of the second sintering is 600-800°C, for example, 600°C, 650°C, 700°C, 750°C or 800°C.

[0063] Preferably, the sintering time of the second sintering is 12 to 24 h, for example, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h, 20 h, 21 h, 22 h, 23 h or 24 h.

[0064] As a preferred technical solution, the preparation method comprises the following steps:

[0065] The first mixed metal salt solution, the first precipitant solution and the first complexing agent solution are added in parallel to perform a first coprecipitation reaction to obtain a precursor core Ni a Mn b V c (OH)2, 0.14≤a≤0.35, 0.6≤b≤0.85, 0.01≤c≤0.05;

[0066] After the precursor core is obtained, the second mixed metal salt solution, the second precipitant solution and the second complexing agent solution are added in parallel to perform a second coprecipitation reaction to obtain a precursor material. The chemical formula of the coating layer in the precursor material is Mn k V m Ce n (OH)2, where 0.85≤k≤0.95, 0.02≤m≤0.06, 0.03≤n≤0.09;

[0067] The precursor material is mixed with a lithium source, and the temperature is raised to 450-550° C. at a heating rate of 2-10° C. / min for a first sintering for 2-10 hours, and then the temperature is raised to 600-800° C. at a heating rate of 2-10° C. / min for a second sintering for 12-24 hours to obtain the modified lithium-rich manganese-based positive electrode material;

[0068] Among them, the first mixed metal salt solution includes vanadium ions and manganese ions, and the second mixed metal salt solution includes vanadium ions, cerium ions and manganese ions; the molar amount of vanadium in the first mixed metal salt solution is greater than the molar amount of vanadium in the second mixed metal salt solution.

[0069] It should also be noted that the specific type and amount of the lithium source, the mixing method of the lithium source and the precursor material, and the specific sintering atmosphere during the sintering process in the present invention are all conventional technical solutions in the art;

[0070] Optionally, the lithium source is selected from at least one of lithium carbonate, lithium sulfate, lithium hydroxide, lithium acetate or lithium chloride;

[0071] Optionally, the ratio of the total molar amount of lithium in the lithium source to all metal elements in the precursor material is (1.1-1.6):1, such as 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1 or 1.6:1, etc.;

[0072] Optionally, the sintering atmosphere is selected from at least one of a protective atmosphere, an oxygen-containing atmosphere or a hydrogen atmosphere, the protective atmosphere includes a nitrogen atmosphere or an inert gas atmosphere, and the oxygen-containing atmosphere includes an oxygen atmosphere or air gas.

[0073] In a third aspect, the present invention further provides a lithium-ion battery, comprising the modified lithium-rich manganese-based positive electrode material as described in the first aspect or the modified lithium-rich manganese-based positive electrode material prepared by the preparation method as described in the second aspect.

[0074] Due to space limitations and to avoid redundancy, the present invention does not exhaustively list all point values ​​within the above numerical range, but is not limited to the listed values, and other unlisted values ​​within the above numerical range are also applicable.

[0075] Compared with the prior art, the present invention has the following beneficial effects:

[0076] The modified lithium-rich manganese-based positive electrode material provided by the present invention is doped with vanadium in the core, and the vanadium exists in the form of a lithium vanadate (Li2VO3) phase structure, which can inhibit the transformation of the material from a layered structure to a spinel-like structure, is beneficial to stabilizing the material structure, and improving the structural stability of the positive electrode material; and the vanadium and cerium co-doping in the coating layer ensures that the coating layer formed by the outer shell has a high density, and the coating layer can also effectively block the contact between the material core and the electrolyte, avoiding the dissolution of Mn and reducing the occurrence of side reactions when the material contacts the electrolyte during the reaction process; the core and the coating layer cooperate with each other to jointly improve the discharge capacity and cycle performance of the modified lithium-rich manganese-based positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0077] Figure 1 This is an SEM image of the modified lithium-rich manganese-based positive electrode material provided in Example 1. DETAILED DESCRIPTION

[0078] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0079] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.

[0080] In the description of this application, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the quantity, specific order or primary and secondary relationship of the indicated technical features.

[0081] Example 1

[0082] This embodiment provides a modified lithium-rich manganese-based positive electrode material, wherein the modified lithium-rich manganese-based positive electrode comprises a core and a coating layer coated on the surface of the core;

[0083] The chemical formula of the core is Li 1.2 Ni 0.25 Mn 0.72 V 0.03 O2, D50 of the inner core is 8 μm;

[0084] The chemical formula of the coating layer is Li 1.2 Mn 0.89 V 0.06 Ce 0.05 O2, the coating thickness is 2 μm;

[0085] The preparation method of the modified lithium-rich manganese-based positive electrode material is as follows:

[0086] Step S1:

[0087] Accurately weigh nickel sulfate, manganese sulfate and ammonium vanadate in sequence to make the molar ratio of nickel, manganese and vanadium be n(Ni 2+ ):n(Mn 2+ ):n(V 2+ )=0.25:0.72:0.03, to prepare 100g / L metal salt solution A;

[0088] The first precipitant is sodium hydroxide, and solid sodium hydroxide is prepared into a sodium hydroxide solution with a mass fraction of 29%;

[0089] The first complexing agent is ammonia water, which is prepared into an ammonia water solution with a mass fraction of 15%;

[0090] At the same time, metal salt solution A is introduced into the reactor at a feed rate of 30 L / h, sodium hydroxide solution is introduced at a feed rate of 11 L / h, and ammonia solution is introduced at a feed rate of 3 L / h to perform a first coprecipitation reaction. During the first coprecipitation reaction, the temperature in the reactor is controlled to be 60° C., the pH is 9.9-10.1, the ammonia concentration is 5.5-5.7 g / L, the reactor speed is 300 rpm, and the reaction time is 120 h. When the core particle size D50 reaches 8 μm, the reaction solution is stopped to obtain the core of the lithium-rich manganese-based precursor;

[0091] Step S2:

[0092] Accurately weigh manganese sulfate, ammonium vanadate and cerium nitrate in sequence to make the molar ratio of manganese, vanadium and cerium equal to n(Mn 2+ ):n(V 2+ ):n(Ce 3+ )=0.89:0.06:0.05, to prepare 120g / L metal salt solution B;

[0093] The second precipitant is sodium hydroxide, and solid sodium hydroxide is prepared into a sodium hydroxide solution with a mass fraction of 32%;

[0094] The second complexing agent is lactic acid, which is prepared into a lactic acid solution with a mass fraction of 18%;

[0095] At the same time, metal salt solution A is introduced into the above-mentioned reactor at a feed rate of 24 L / h, sodium hydroxide solution is introduced at a feed rate of 10.5 L / h, and lactic acid solution is introduced at a feed rate of 2.5 L / h to carry out a second coprecipitation reaction. During the second coprecipitation reaction, the temperature in the reactor is controlled to be 60° C., the pH is 10.6-10.8, the lactic acid concentration is 6-6.2 g / L, the reactor speed is 250 rpm, and the reaction time is 18 h. When the thickness of the shell layer reaches 2 μm, the reaction solution is stopped to obtain the shell layer of the lithium-rich manganese-based precursor (i.e., the precursor coating layer), thereby obtaining the precursor material;

[0096] Step S3:

[0097] The precursor particles obtained in step S2 are aged for 7 hours at a temperature of 65° C. and a total alkali concentration of 30 g / L. After the aging, the particles are filtered and washed. The washing includes alkali washing and water washing in sequence. The particles are washed with a liquid alkali solution for 3 times and then washed with hot water for 3 times. The particles are dried at 150° C. for 24 hours and sieved to remove iron to obtain the lithium-rich manganese-based precursor material.

[0098] Step S4:

[0099] The above-mentioned precursor powder and lithium carbonate are evenly mixed according to the molar ratio of lithium content to transition metal of 1.2:1, and then sintered in an air atmosphere by gradient heating method, first heated to 500°C at a heating rate of 6°C / min and kept warm for 5 hours, then heated to 700°C at a heating rate of 6°C / min and kept warm for 18 hours, and naturally cooled at room temperature to obtain the modified lithium-rich manganese-based positive electrode material.

[0100] Figure 1 The SEM image of the modified lithium-rich manganese-based positive electrode material provided in Example 1 is shown. Figure 1 It can be seen that the positive electrode material provided by the present invention has a dense structure, uniform morphology, and uniform particle size.

[0101] Example 2

[0102] This embodiment provides a modified lithium-rich manganese-based positive electrode material, wherein the modified lithium-rich manganese-based positive electrode comprises a core and a coating layer coated on the surface of the core;

[0103] The chemical formula of the core is Li 1.6 Ni0.25 Mn 0.72 V 0.03 O2, D50 of the inner core is 10 μm;

[0104] The chemical formula of the coating layer is Li 1.6 Mn 0.89 V 0.06 Ce 0.05 O2, the coating thickness is 3 μm;

[0105] The preparation method of the modified lithium-rich manganese-based positive electrode material is as follows:

[0106] Step S1:

[0107] Accurately weigh nickel sulfate, manganese sulfate and ammonium vanadate in sequence to make the molar ratio of nickel, manganese and vanadium be n(Ni 2+ ):n(Mn 2+ ):n(V 2+ )=0.25:0.72:0.03, to prepare 200g / L metal salt solution A;

[0108] The first precipitant is sodium hydroxide, and solid sodium hydroxide is prepared into a sodium hydroxide solution with a mass fraction of 40%;

[0109] The first complexing agent is ammonia water, which is prepared into an ammonia water solution with a mass fraction of 20%;

[0110] At the same time, metal salt solution A is introduced into the reactor at a feed rate of 20 L / h, sodium hydroxide solution is introduced at a feed rate of 8 L / h, and ammonia solution is introduced at a feed rate of 1 L / h to perform a first coprecipitation reaction. During the first coprecipitation reaction, the temperature in the reactor is controlled to be 45° C., the pH is 11.1-11.3, the ammonia concentration is 5.5-5.7 g / L, the reactor speed is 400 rpm, and the reaction time is 150 h. When the core particle size D50 reaches 10 μm, the reaction solution is stopped to obtain the core of the lithium-rich manganese-based precursor;

[0111] Step S2:

[0112] Accurately weigh manganese sulfate, ammonium vanadate and cerium nitrate in sequence to make the molar ratio of manganese, vanadium and cerium equal to n(Mn 2+ ):n(V 2+ ):n(Ce 3+ )=0.89:0.06:0.05, to prepare 200g / L metal salt solution B;

[0113] The second precipitant is sodium hydroxide, and solid sodium hydroxide is prepared into a sodium hydroxide solution with a mass fraction of 40%;

[0114] The second complexing agent is lactic acid, which is prepared into a lactic acid solution with a mass fraction of 25%;

[0115] At the same time, metal salt solution A is introduced into the above-mentioned reactor at a feed rate of 40 L / h, sodium hydroxide solution is introduced at a feed rate of 14 L / h, and lactic acid solution is introduced at a feed rate of 5 L / h to carry out a second coprecipitation reaction. During the second coprecipitation reaction, the temperature in the reactor is controlled to be 70° C., the pH is 10.6-10.8, the lactic acid concentration is 6-6.2 g / L, the reactor speed is 350 rpm, and the reaction time is 30 h. When the thickness of the shell layer reaches 3 μm, the reaction solution is stopped to obtain the shell layer of the lithium-rich manganese-based precursor (i.e., the precursor coating layer), thereby obtaining the precursor material;

[0116] Step S3:

[0117] The precursor particles obtained in step S2 are aged for 7 hours at a temperature of 65° C. and a total alkali concentration of 30 g / L. After the aging, the particles are filtered and washed. The washing includes alkali washing and water washing in sequence. The particles are washed with a liquid alkali solution for 3 times and then washed with hot water for 3 times. The particles are dried at 150° C. for 24 hours and sieved to remove iron to obtain the lithium-rich manganese-based precursor material.

[0118] Step S4:

[0119] The above-mentioned precursor powder and lithium carbonate are evenly mixed according to the molar ratio of lithium content to transition metal of 1.6:1, and then sintered in an air atmosphere by gradient heating method, first heated to 450°C at a heating rate of 5°C / min and kept warm for 8 hours, then heated to 600°C at a heating rate of 5°C / min and kept warm for 20 hours, and naturally cooled at room temperature to obtain the modified lithium-rich manganese-based positive electrode material.

[0120] Example 3

[0121] The difference between this embodiment and embodiment 1 is that the chemical formula of the core in this embodiment is Li 1.2 Ni 0.25 Mn 0.70 V 0.05 O2;

[0122] In the preparation method, step S1 accurately weighs nickel sulfate, manganese sulfate and ammonium vanadate in sequence to make the molar ratio of nickel, manganese and vanadium be n(Ni 2+ ):n(Mn 2+ ):n(V 2+ )=0.25:0.70:0.05 to prepare 100g / L metal salt solution A.

[0123] The rest of the preparation methods and parameters were the same as those in Example 1.

[0124] Example 4

[0125] The difference between this embodiment and embodiment 1 is that the chemical formula of the core in this embodiment is Li 1.2 Ni 0.25 Mn 0.74 V 0.01 O2;

[0126] In the preparation method, step S1 accurately weighs nickel sulfate, manganese sulfate and ammonium vanadate in sequence to make the molar ratio of nickel, manganese and vanadium be n(Ni 2+ ):n(Mn 2+ ):n(V 2+ )=0.25:0.74:0.01 to prepare 100g / L metal salt solution A.

[0127] The rest of the preparation methods and parameters were the same as those in Example 1.

[0128] Example 5

[0129] The difference between this embodiment and embodiment 1 is that the chemical formula of the coating layer in this embodiment is Li 1.2 Mn 0.85 V 0.09 Ce 0.06 O2;

[0130] In the preparation method,

[0131] Step S2: accurately weigh manganese sulfate, ammonium vanadate and cerium nitrate in sequence to make the molar ratio of manganese, vanadium and cerium be n(Mn 2+ ):n(V 2+ ):n(Ce 3+ )=0.85:0.09:0.06, to prepare 120g / L metal salt solution B.

[0132] The rest of the preparation methods and parameters were the same as those in Example 1.

[0133] Example 6

[0134] The difference between this embodiment and embodiment 1 is that the chemical formula of the core in this embodiment is Li 1.2 Ni 0.25 Mn 0.73 V 0.02 O2, the chemical formula of the coating layer is Li 0.95 Mn 0.95 V 0.03 Ce 0.02 O2;

[0135] In the preparation method, step S1 accurately weighs nickel sulfate, manganese sulfate and ammonium vanadate in sequence to make the molar ratio of nickel, manganese and vanadium be n(Ni 2+):n(Mn 2+ ):n(V 2+ )=0.25:0.73:0.02, to prepare 100g / L metal salt solution A;

[0136] Step S2: accurately weigh manganese sulfate, ammonium vanadate and cerium nitrate in sequence to make the molar ratio of manganese, vanadium and cerium be n(Mn 2+ ):n(V 2+ ):n(Ce 3+ )=0.95:0.03:0.02, to prepare 120g / L metal salt solution B.

[0137] The rest of the preparation methods and parameters were the same as those in Example 1.

[0138] Example 7

[0139] The difference between this embodiment and embodiment 1 is that the chemical formula of the core in this embodiment is Li 1.2 Ni 0.25 Mn 0.65 V 0.1 O2;

[0140] In the preparation method, step S1 accurately weighs nickel sulfate, manganese sulfate and ammonium vanadate in sequence to make the molar ratio of nickel, manganese and vanadium be n(Ni 2+ ):n(Mn 2+ ):n(V 2+ )=0.25:0.65:0.1, to prepare 100g / L metal salt solution A.

[0141] The rest of the preparation methods and parameters were the same as those in Example 1.

[0142] Example 8

[0143] The difference between this embodiment and embodiment 1 is that the chemical formula of the coating layer in this embodiment is Li 1.2 Mn 0.92 V 0.03 Ce 0.05 O2;

[0144] In the preparation method, step S2 accurately weighs manganese sulfate, ammonium vanadate and cerium nitrate in sequence to make the molar ratio of manganese, vanadium and cerium be n(Mn 2+ ):n(V 2+ ):n(Ce 3+ )=0.92:0.03:0.05, to prepare 120g / L metal salt solution B.

[0145] The rest of the preparation methods and parameters were the same as those in Example 1.

[0146] Example 9

[0147] The difference between this embodiment and embodiment 1 is that the chemical formula of the coating layer in this embodiment is Li 1.2 Mn 0.8 V 0.15 Ce 0.05 O2;

[0148] In the preparation method, step S2 accurately weighs manganese sulfate, ammonium vanadate and cerium nitrate in sequence to make the molar ratio of manganese, vanadium and cerium be n(Mn 2+ ):n(V 2+ ):n(Ce 3+ )=0.80:0.15:0.05, to prepare 120g / L metal salt solution B.

[0149] The rest of the preparation methods and parameters were the same as those in Example 1.

[0150] Example 10

[0151] The difference between this embodiment and embodiment 1 is that the chemical formula of the coating layer in this embodiment is Li 1.2 Mn 0.84 V 0.06 Ce 0.1 O2;

[0152] In the preparation method, step S2 accurately weighs manganese sulfate, ammonium vanadate and cerium nitrate in sequence to make the molar ratio of manganese, vanadium and cerium be n(Mn 2+ ):n(V 2+ ):n(Ce 3+ )=0.84:0.06:0.1, and a metal salt solution B of 120 g / L was prepared.

[0153] The rest of the preparation methods and parameters were the same as those in Example 1.

[0154] Comparative Example 1

[0155] The difference between this comparative example and Example 1 is that in this comparative example, vanadium is not doped in the core, and the chemical formula of the core is Li 1.2 Ni 0.25 Mn 0.75 O2;

[0156] In the preparation method, step S1 accurately weighs nickel sulfate and manganese sulfate in sequence to make the molar ratio of nickel to manganese be n(Ni 2+ ):n(Mn 2+ )=0.25:0.75, to prepare 100g / L metal salt solution A.

[0157] The rest of the preparation methods and parameters were the same as those in Example 1.

[0158] Comparative Example 2

[0159] The difference between this comparative example and Example 1 is that the coating layer of this comparative example is not doped with vanadium, and the chemical formula of the coating layer is Li 1.2 Mn 0.95 Ce 0.05 O2;

[0160] In the preparation method, step S2 accurately weighs manganese sulfate and cerium nitrate in sequence to make the molar ratio of manganese to cerium be n(Mn 2+ ):n(Ce 3+ )=0.95:0.05, and a metal salt solution B of 120g / L is prepared.

[0161] The rest of the preparation methods and parameters were the same as those in Example 1.

[0162] Comparative Example 3

[0163] The difference between this comparative example and Example 1 is that the coating layer of this comparative example is not doped with cerium, and the chemical formula of the coating layer is Li 1.2 Mn 0.94 V 0.06 O2;

[0164] In the preparation method, step S2 accurately weighs manganese sulfate and ammonium vanadate in sequence to make the molar ratio of manganese to vanadium be n(Mn 2+ ):n(V 2+ )=0.94:0.06:, and make 120g / L metal salt solution B.

[0165] The rest of the preparation methods and parameters were the same as those in Example 1.

[0166] Comparative Example 4

[0167] The difference between this comparative example and Example 1 is that the coating layer of this comparative example is not doped with vanadium and cerium, and the chemical formula of the coating layer is Li 1.2 MnO2;

[0168] In the preparation method, step S2 is to accurately weigh manganese sulfate in sequence to prepare a metal salt solution B of 120 g / L.

[0169] The rest of the preparation methods and parameters were the same as those in Example 1.

[0170] Comparative Example 5

[0171] The difference between this comparative example and Example 1 is that the chemical formula of the core in this comparative example is Li 0.70 Ni 0.25 Mn 0.72 V 0.03 O2, the chemical formula of the coating layer is Li 0.70 Mn 0.89 V 0.06 Ce0.05 O2;

[0172] In the preparation method, in step S4, the molar ratio of the precursor powder to the lithium carbonate is 0.7:1 based on the lithium content to the transition metal.

[0173] The rest of the preparation methods and parameters were the same as those in Example 1.

[0174] The modified lithium-rich manganese-based positive electrode materials provided in Examples 1-10 and Comparative Examples 1-5 were weighed and dissolved in N-methylpyrrolidone (NMP) according to a mass ratio of 8:1:1 with acetylene black as a conductive agent and polyvinylidene fluoride (PVDF) as a binder, and then the slurry was applied to an aluminum foil with an applicator and dried in a vacuum drying oven at 80°C for 8h; finally, the aluminum foil was punched into 1.13 cm 2 The positive electrode is obtained by forming a circular shape;

[0175] The obtained electrode sheet was used as the positive electrode, the lithium metal sheet was used as the counter electrode, and a porous polypropylene membrane (Celgard2400) was used as a separator to separate the positive electrode and the counter electrode. The composition of the electrolyte was: a mixture of 1MLiPF6 and EC, DMC and EMC (EC:DMC:EMC volume ratio = 1:1:1); CR2032 button batteries were assembled in an argon glove box.

[0176] The prepared batteries of Examples 1-10 and Comparative Examples 1-5 were subjected to performance tests under the following test conditions: voltage range 2-4.8V, current density 1C, charge and discharge cycles, 200 cycles, and the test results are shown in Table 1.

[0177] Table 1

[0178]

[0179]

[0180] From Table 1, we can get:

[0181] From the data results of Examples 1-6, it can be seen that the lithium-rich manganese-based positive electrode material provided by the present invention, the vanadium doping in the core and the vanadium-cerium co-doping in the coating layer cooperate synergistically, and the vanadium content in the core is lower than that in the coating layer, which jointly improves the discharge capacity and cycle performance of the modified lithium-rich manganese-based positive electrode material;

[0182] It can be seen from the data results of Example 1 and Examples 7-10 that by adjusting the stoichiometric ratio of vanadium and cerium in the core and the coating layer, it is more conducive to improving the performance of the positive electrode material.

[0183] From the data results of Example 1 and Comparative Examples 1-5, it can be seen that in the modified lithium-rich manganese-based positive electrode material, vanadium core doping and co-doping of the vanadium-cerium coating layer must be carried out simultaneously, and the material must be lithium-rich in order to achieve improvements in discharge capacity and cycle performance.

[0184] In summary, in the modified lithium-rich manganese-based positive electrode material provided by the present invention, vanadium is doped in the core, and the vanadium exists in the form of lithium vanadate (Li2VO3) phase structure, which can inhibit the transformation of the material from a layered structure to a spinel-like structure, which is beneficial to stabilizing the material structure and improving the structural stability of the positive electrode material; and the vanadium and cerium co-doping in the coating layer ensures that the coating layer formed by the outer shell has a high density, and the coating layer can also effectively block the contact between the material core and the electrolyte, avoiding the dissolution of Mn and reducing the occurrence of side reactions when the material contacts the electrolyte during the reaction process; the core and the coating layer cooperate with each other to jointly improve the discharge capacity and cycle performance of the modified lithium-rich manganese-based positive electrode material.

[0185] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A modified lithium-rich manganese-based positive electrode material, characterized in that: The modified lithium-rich manganese-based positive electrode material includes a core and a coating layer coated on the surface of the core; the core includes a vanadium-doped lithium-rich manganese-based positive electrode material, and the coating layer includes a vanadium-cerium co-doped lithium-rich manganese-based positive electrode material.

2. The modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The molar ratio of vanadium in the core is smaller than the molar ratio of vanadium in the coating layer.

3. The modified lithium-rich manganese-based positive electrode material according to claim 1 or 2, characterized in that: The chemical formula of the core is Li x Ni a Mn b V c O2, where 1.1≤x≤1.6, 0.14≤a≤0.35, 0.6≤b≤0.85, 0.01≤c≤0.05; Preferably, the chemical formula of the coating layer is Li y Mn k V m Ce n O2, where 1.1≤y≤1.6, 0.85≤k≤0.95, 0.02≤m≤0.06, 0.03≤n≤0.

09.

4. The modified lithium-rich manganese-based positive electrode material according to any one of claims 1 to 3, characterized in that: The D50 of the lithium-rich manganese-based positive electrode material is 6 to 15 μm; Preferably, the D50 of the inner core is 5 to 12 μm, and the shell thickness of the coating layer is 1 to 3 μm.

5. A method for preparing a modified lithium-rich manganese-based positive electrode material according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: Adding a first mixed metal salt solution, a first precipitant solution and a first complexing agent solution in parallel to perform a first coprecipitation reaction to obtain a precursor core; After the precursor core is obtained, a second mixed metal salt solution, a second precipitant solution and a second complexing agent solution are added in parallel to perform a second coprecipitation reaction to obtain a precursor material; Mixing the precursor material with a lithium source and sintering to obtain the modified lithium-rich manganese-based positive electrode material; The first mixed metal salt solution includes vanadium ions and manganese ions, and the second mixed metal salt solution includes vanadium ions, cerium ions and manganese ions.

6. The preparation method according to claim 5, characterized in that: The molar amount ratio of vanadium in the first mixed metal salt solution is less than the molar amount ratio of vanadium in the second mixed metal salt solution; Preferably, the chemical formula of the precursor core is Ni a Mn b V c (OH)2, where 0.14≤a≤0.35, 0.6≤b≤0.85, 0.01≤c≤0.05; Preferably, the chemical formula of the coating layer in the precursor material is Mn k V m Ce n (OH)2, wherein 0.85≤k≤0.95, 0.02≤m≤0.06, 0.03≤n≤0.

09.

7. The preparation method according to claim 5 or 6, characterized in that: The reaction temperatures of the first coprecipitation reaction and the second coprecipitation reaction are each independently 45 to 70° C.; Preferably, the pH values ​​of the first coprecipitation reaction and the second coprecipitation reaction are independently 9 to 12; Preferably, the reaction time of the first coprecipitation reaction is 50 to 200 hours; Preferably, the reaction time of the second coprecipitation reaction is 8 to 30 hours.

8. The preparation method according to any one of claims 5 to 7, characterized in that: The sintering includes sequentially performing a first sintering and a second sintering; Preferably, the heating rates of the first sintering and the second sintering are independently 2 to 10°C / min; Preferably, the sintering temperature of the first sintering is 450-550° C., and the sintering time of the first sintering is 2-10 hours; Preferably, the sintering temperature of the second sintering is 600-800° C., and the sintering time of the second sintering is 12-24 hours.

9. The preparation method according to any one of claims 5 to 8, characterized in that: The preparation method comprises the following steps: The first mixed metal salt solution, the first precipitant solution and the first complexing agent solution are added in parallel to perform a first coprecipitation reaction to obtain a precursor core Ni a Mn b V c (OH)2, 0.14≤a≤0.35, 0.6≤b≤0.85, 0.01≤c≤0.05; After the precursor core is obtained, the second mixed metal salt solution, the second precipitant solution and the second complexing agent solution are added in parallel to perform a second coprecipitation reaction to obtain a precursor material. The chemical formula of the coating layer in the precursor material is Mn k V m Ce n (OH)2, where 0.85≤k≤0.95, 0.02≤m≤0.06, 0.03≤n≤0.09; The precursor material is mixed with a lithium source, and the temperature is raised to 450-550° C. at a heating rate of 2-10° C. / min for a first sintering for 2-10 hours, and then the temperature is raised to 600-800° C. at a heating rate of 2-10° C. / min for a second sintering for 12-24 hours to obtain the modified lithium-rich manganese-based positive electrode material; Among them, the first mixed metal salt solution includes vanadium ions and manganese ions, and the second mixed metal salt solution includes vanadium ions, cerium ions and manganese ions; the molar amount of vanadium in the first mixed metal salt solution is less than the molar amount of vanadium in the second mixed metal salt solution.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the modified lithium-rich manganese-based positive electrode material as described in any one of claims 1 to 4 or the modified lithium-rich manganese-based positive electrode material prepared by the preparation method as described in any one of claims 5 to 9.

Citation Information

Cited By

  • Nickel-rich positive electrode material and preparation method thereof, positive electrode plate, lithium ion battery and electric equipment

    CN119340379A

  • Modified lithium-rich positive electrode material as well as preparation method and application thereof

    CN120545342A

  • Modified lithium-rich cathode material, and preparation method and application thereof

    CN120545342B

  • Doped and coated lithium-rich manganese-based positive electrode material and preparation method thereof, lithium ion battery and electric equipment

    CN121035192A

  • Doped-coated lithium-rich manganese-based positive electrode material, preparation method thereof, lithium ion battery and electric device

    CN121035192B