Insulation protection layer and high-voltage motor insulation system
By using a single-sided reinforced multi-glue mica tape and VPI resin vacuum pressure immersion process in the high-voltage motor insulation system, combined with the epoxy mixture, the contradiction between volume and insulation performance of the high-voltage motor insulation system is solved, and efficient insulation performance and reduction are achieved Thin effect.
Patent Information
- Application Number
- CN202411085480.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
AI Technical Summary
The existing high-voltage motor insulation system is difficult to maintain sufficient insulation performance while reducing the motor size, resulting in a large overall volume and cannot meet the volume requirements of 10kV high-voltage motors.
Using a single-sided reinforced multi-glue mica tape and VPI resin vacuum pressure impregnation process, the glue content and mica content are increased, the second bonding layer is set to improve integrity and mechanical strength, and mica powder is added to the VPI resin to fill it voids, combined with epoxy mixture to improve insulation properties.
A lower thickness of insulating protective layer is realized, which improves insulation performance and integrity, reduces pores, enhances mechanical strength and sealing, meets the insulation performance requirements of high-voltage motors, and realizes thinning of the insulation system.
Smart Images

Figure CN118971452A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of motor insulation, and in particular to an insulating protective layer and a high-voltage motor insulation system. Background Art
[0002] With the development of 10kV high-voltage motors, their application market requires that the size of motors continue to decrease. The insulation performance of the motor insulation system will directly affect the operating reliability and service life of the high-voltage motor. Therefore, it is very important to maintain the reliability of the motor insulation system while adapting to the motor size requirements.
[0003] In the prior art, a mica tape with little rubber is usually used to wind the coil to form a main insulation layer. When winding with the existing mica tape with little rubber, it usually requires multiple layers of winding to meet the insulation performance requirements of the high-voltage motor. When applied to a 10kV high-voltage motor, in order to meet the insulation performance requirements, the mica tape with little rubber has a large number of winding layers, and the thickness of the main insulation layer is large, resulting in a larger overall volume of the motor, which is difficult to meet the volume requirements of the 10kV high-voltage motor. Summary of the invention
[0004] The object of the present invention is to provide an insulating protective layer and a high-voltage motor insulation system which can achieve a higher insulation effect with a lower thickness.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] An insulating protective layer is obtained by wrapping a single-sided reinforced multi-resin mica tape and then vacuum pressure impregnating it with a VPI resin. The single-sided reinforced multi-resin mica tape comprises a polyester film, a first adhesive layer, mica paper, and a second adhesive layer. The first adhesive layer is used for bonding and compounding the polyester film and the mica paper. The second adhesive layer is formed on the side of the mica paper away from the first adhesive layer. The adhesive content of the single-sided reinforced multi-resin mica tape is 70g / m 2 ~90g / m 2 Any value in, the mass of the mica paper is 117g / m 2 ~143g / m 2 Any value in .
[0007] Optionally, the VPI resin is obtained by doping mica powder with epoxy or epoxy-modified unsaturated polyester VPI resin, the particle size of the mica powder is any value between 0.5um and 10um, the added mass ratio is any value between 10% and 20%, and the breakdown field strength of the VPI resin is greater than or equal to 33kV / mm.
[0008] Optionally, the thickness of the polyester film is any value between 0.02mm and 0.04mm, the mica paper is calcined mica paper, the first bonding layer is formed by drying a first adhesive coated on the polyester film at a baking temperature, the second bonding layer is formed by drying a second adhesive coated on the mica paper at the baking temperature, the first adhesive and the second adhesive are both prepared by dissolving an epoxy mixture in a mixed solvent of toluene and acetone, the ratio of the toluene and the acetone in the mixed solvent is any ratio of 1:(0.9 to 1.1), and the thickness of the single-sided reinforced multi-glue mica tape is any value between 0.14mm and 0.18mm.
[0009] Optionally, the first adhesive is coated on the polyester film and then dried at the baking temperature, the mica paper is compounded, and the second adhesive is coated and then dried again at the baking temperature, the solid content of the first adhesive is any value between 45% and 55%, the solid content of the second adhesive is any value between 15% and 25%, and the baking temperature is any value between 100°C and 120°C.
[0010] Optionally, the epoxy mixture includes bisphenol A epoxy resin, novolac epoxy resin, epoxy ester and epoxy resin curing agent, and the mass ratio of the bisphenol A epoxy resin, the novolac epoxy resin, the epoxy ester and the epoxy resin curing agent is any ratio of 1:(2-3):(1-2):(0.2-1).
[0011] Optionally, the epoxy ester is obtained by an esterification reaction between a bisphenol epoxy resin and an acidic substance under the catalysis of zinc acetate, the acidic substance is one or more of methacrylic acid, maleic anhydride and methyltetrahydrophthalic anhydride, the bisphenol epoxy resin is epoxy resin 6101 or epoxy resin 128, the mass ratio of the bisphenol epoxy resin, the acidic substance and the zinc acetate is any ratio of (8.5 to 9.5): 1: (0.009 to 0.011), the reaction temperature of the esterification reaction is any value of 120°C to 140°C, and the acid value of the epoxy ester is less than or equal to 2 mgKOH / g.
[0012] Optionally, the bisphenol A epoxy resin is epoxy resin 6101 or epoxy resin 128, the novolac epoxy resin is novolac epoxy resin F51 or novolac epoxy resin F44, and the epoxy resin curing agent is zinc isooctanoate.
[0013] In the second aspect, the present invention also provides a high-voltage motor insulation system, comprising an inter-turn insulation layer wrapped around the surface of a wire core, a main insulation layer wrapped around the outside of a plurality of turns of a coil composed of the wire core and the inter-turn insulation layer, and an anti-corona layer wrapped around the main insulation layer, the thickness of the inter-turn insulation layer being any value between 0.35 mm and 0.40 mm, being obtained by wrapping with a first low-resistance mica tape, and being obtained by wrapping with the above-mentioned single-sided reinforced multi-resistance mica tape, the anti-corona layer comprising a low-resistance anti-corona tape, a high-resistance anti-corona tape and a second low-resistance mica tape reinforced with glass cloth, the total single-side thickness of the main insulation layer and the anti-corona layer being any value between 1.6 mm and 1.8 mm, and after the inter-turn insulation layer, the main insulation layer and the anti-corona layer are wrapped, they are vacuum pressure impregnated and cured by the above-mentioned VPI resin.
[0014] Optionally, the inter-turn insulation layer includes several types of the first low-resistance mica tapes, the thickness of the first low-resistance mica tapes is any value between 0.05 mm and 0.09 mm, and the first low-resistance mica tapes are reinforced with polyester film or polyimide film.
[0015] According to the first aspect of the present invention, by adopting single-sided reinforcement and increasing the glue content, the mica tape has higher flexibility and fit, thereby improving the integrity of the insulating protective layer and reducing pores. The single-sided reinforced multi-glue mica tape of the same thickness has a higher mica content than the double-sided reinforced multi-glue mica tape, which helps to improve the insulation performance. By providing a second adhesive layer, the single-sided reinforced multi-glue mica tape has a higher integrity with the single-sided reinforced multi-glue mica tape of other layers after wrapping, thereby improving the mechanical strength and preventing the uniformity and sealing of the insulating layer from decreasing due to loosening of the inner layer. By vacuum pressure impregnation, the VPI resin is impregnated into the single-sided reinforced multi-glue mica tape. Due to the high glue content in the mica tape, the cured insulating protective layer has a high degree of integrity, thereby improving its insulation performance.
[0016] Furthermore, adding mica powder to the VPI resin helps to fill the gaps between multiple layers of single-sided reinforced multi-resin mica tapes during the impregnation process while maintaining the penetration ability and fluidity of the VPI resin, thereby improving the overall insulation performance of the insulating protective layer.
[0017] Furthermore, the calcined mica paper has good plasticity and high temperature resistance, which facilitates the wrapping and curing of the mica tape, so that the epoxy mixture is dissolved in the mixed solvent to form an adhesive, and the mixed solvent in the adhesive is evaporated by drying, which helps the epoxy mixture to be evenly mixed and evenly coated on the surface of the polyester film or mica paper, thereby improving the uniformity of the mica tape.
[0018] Furthermore, the solid content of the first adhesive is made higher and is dried twice to improve the composite strength of the polyester film and the mica paper, prevent the polyester film from separating from the mica paper, and make the solid content of the first adhesive lower to prevent the mica tape that is rolled up and stored after production from being difficult to peel off.
[0019] Furthermore, bisphenol A epoxy resin has high transparency and good physical and mechanical properties, and has excellent adhesion, chemical corrosion resistance and electrical insulation after curing. It has good processability, small volume shrinkage during curing, can be dissolved in a variety of solvents, and is suitable for a variety of coating and bonding applications. Phenolic epoxy resin is superior to bisphenol A epoxy resin in terms of heat resistance. It combines the high temperature resistance of phenolic resin and the good processability of epoxy resin, allowing mica tape to maintain excellent insulation properties at higher temperatures. The combination of these two epoxy resins can take into account high adhesion and high heat resistance, meet the needs of vacuum pressure impregnation process, and improve the flexibility and mechanical strength of mica tape, so that it can withstand greater tension during the wrapping process and avoid damage. The addition of epoxy ester helps to further improve the mechanical properties, flexibility and insulation properties, and is well compatible with other resins such as polyester and polyimide, which improves the applicability of mica tape in vacuum pressure impregnation process. Epoxy curing agent helps to promote the curing of epoxy resin, increase crosslinking density, optimize thermal stability, and also helps to control shrinkage, reduce internal stress of mica tape, avoid cracking and deformation, and maintain the dimensional stability of mica tape. This epoxy mixture system ensures excellent integrity, thermal performance and long insulation life of low-resistance mica tape at high temperatures.
[0020] Furthermore, the epoxy ester is prepared immediately before use, which helps to ensure its optimal performance. By adjusting the raw material ratio and reaction conditions, it helps to promote the reaction to proceed fully, improve the yield, and reduce the presence of impurities in the epoxy ester.
[0021] According to the second aspect of the present invention, a coil is formed by wrapping a wire core with a mica tape with less glue, and a mica tape with more glue is wrapped around the outside of a multi-turn coil to form a main insulating layer. Since the mica tape with more glue has a high plasticity, the main insulating layer and the inter-turn insulating layer are connected more closely, which helps to improve the overall insulation performance. A low-resistance anti-corona tape, a high-resistance anti-corona tape and a second mica tape with less glue reinforced with glass cloth are sequentially wrapped around the outside of the main insulating layer to form an anti-corona layer. By wrapping the mica tape with glass cloth around the outside of the anti-corona tape, it helps to improve the anti-corona performance of the motor insulation system, increase the corona inception voltage, and help improve the insulation performance of the mica tape. The VPI resin is used for vacuum pressure impregnation curing, so that the main insulating layer and the anti-corona layer are fully impregnated with the VPI resin, the gaps are filled, the integrity and insulation capacity are improved, and the thinning of the high-voltage motor insulation system is achieved.
[0022] Furthermore, the low-resin mica tape reinforced with polyester film or polyimide film has a stronger insulation capability, which helps to reduce the thickness of the insulation system.
[0023] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic structural diagram of a single-sided reinforced multi-resin mica tape shown in Example 1 of the present invention.
[0025] Legend: 1-polyester film, 2-first adhesive layer, 3-mica paper, 4-second adhesive layer. DETAILED DESCRIPTION
[0026] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0028] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0029] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0030] 10kV high-voltage motors are widely used in high-power fields such as wind energy, underground oil pumping, urban water supply, air compressors, mining, generator sets and ships, and their reliability has high requirements. The insulation system is an important component of the motor and is closely related to the safety and life of the motor. In the prior art, the insulation of the coil is often achieved by winding and curing mica tape. The thickness of the mica tape with less glue is relatively small, and the insulating protective layer obtained after curing with the vacuum pressure impregnation process has good insulation performance. Therefore, it is often used for insulation protection of high-voltage motors. However, the existing insulating protective layer is still difficult to meet the thickness requirements of the insulation system of high-voltage motors.
[0031] The inventor discovered in an accidental operation that the multi-resin mica tape combined with the vacuum pressure impregnation process helps to improve the insulation performance of the insulation protective layer per unit thickness. Based on this discovery, the inventor improved the structure of the conventional multi-resin mica tape, improved the compatibility of the multi-resin mica tape with the vacuum pressure impregnation process, and formed a new insulation protective layer that overcomes the technical prejudice in this field.
[0032] See also Figure 1 The insulating protective layer protected by the present invention is obtained by vacuum pressure impregnation with VPI resin after being wrapped with a single-sided reinforced multi-glue mica tape, wherein the single-sided reinforced multi-glue mica tape includes a polyester film, a first adhesive layer, mica paper and a second adhesive layer, wherein the first adhesive layer is arranged between the polyester film and the mica paper, and the second adhesive layer is formed on the side of the mica paper away from the first adhesive layer, and both the first adhesive layer and the second adhesive layer have adhesion ability. The adhesive content of the single-sided reinforced multi-glue mica tape is 70g / m 2 ~90g / m 2 Any value in, for example, 70g / m 2 , 75g / m 2 , 80g / m 2 , 85g / m 2 and 90g / m 2 For any value in the range, the mass of mica paper is 117 g / m 2 ~143g / m 2 Any value, for example, 117g / m 2 , 120g / m 2 , 125g / m 2 , 130g / m 2 , 135g / m 2 , 140g / m 2 and 143g / m 2 Any value in .
[0033] By adopting a single-sided reinforced structure and increasing the glue content, the mica tape has higher flexibility and fit, thereby improving the integrity of the insulating protective layer and reducing air holes. The single-sided reinforced multi-glue mica tape of the same thickness has a higher mica content than the double-sided reinforced multi-glue mica tape, which helps to improve the insulation performance. By setting a second bonding layer, the single-sided reinforced multi-glue mica tape has a higher integrity with the other layers of single-sided reinforced multi-glue mica tape after wrapping, thereby improving the mechanical strength and preventing the uniformity and sealing of the insulating layer from decreasing due to loosening of the inner layer. Through vacuum pressure impregnation, the VPI resin is impregnated into the single-sided reinforced multi-glue mica tape. Due to the high glue content in the mica tape, the cured insulating protective layer has a high degree of integrity, thereby improving its insulation performance.
[0034] In some embodiments, the VPI resin is obtained by doping mica powder with epoxy or epoxy-modified unsaturated polyester VPI resin, wherein the particle size of the mica powder is any value between 0.5um and 10um, for example, it can be any value between 0.5um, 1um, 3um, 5um, 7um, 8um, 9um and 10um, the added mass proportion of mica powder is any value between 10% and 20%, for example, it can be any value between 10%, 12%, 14%, 16%, 18% and 20%, and the breakdown field strength value of the VPI resin is greater than or equal to 33kV / mm, for example, it can be any value between 33kV / mm, 35kV / mm, 37kV / mm, 39kV / mm and 41kV / mm.
[0035] In some embodiments, the thickness of the polyester film is any value in the range of 0.02 mm to 0.04 mm, for example, any value in the range of 0.02 mm, 0.025 mm, 0.03 mm, 0.035 mm and 0.04 mm. The mica paper is a calcined mica paper, the first adhesive layer is formed by drying the first adhesive applied to the polyester film at a baking temperature, the second adhesive layer is formed by drying the second adhesive applied to the mica paper at a baking temperature, the first adhesive and the second adhesive are both prepared by dissolving an epoxy mixture in a mixed solvent of toluene and acetone, the ratio of toluene to acetone in the mixed solvent is any ratio in the range of 1: (0.9 to 1.1), for example, any ratio in the range of (1: 0.9), (1: 0.95), (1: 1), (1: 1.05) and (1: 1.1). The thickness of the single-sided reinforced multi-resin mica tape is any value between 0.14 mm and 0.18 mm, for example, it can be any value between 0.14 mm, 0.15 mm, 0.16 mm, 0.17 mm and 0.18 mm.
[0036] In some embodiments, a first adhesive is coated on a polyester film and then dried at a baking temperature, and then composited with mica paper, and then coated with a second adhesive and dried again at a baking temperature, the solid content of the first adhesive is any value between 45% and 55%, for example, it can be any value between 45%, 47%, 49%, 51%, 53% and 55%, the solid content of the second adhesive is any value between 15% and 25%, for example, it can be any value between 15%, 17%, 19%, 21%, 23% and 25%, and the baking temperature is any value between 100°C and 120°C, for example, it can be any value between 100°C, 105°C, 110°C, 115°C and 120°C.
[0037] In some embodiments, the epoxy mixture includes bisphenol A epoxy resin, novolac epoxy resin, epoxy ester and epoxy resin curing agent, and the mass ratio of bisphenol A epoxy resin, novolac epoxy resin, epoxy ester and epoxy resin curing agent is any ratio of 1:(2-3):(1-2):(0.2-1).
[0038] In some embodiments, epoxy ester is obtained by esterification reaction of bisphenol epoxy resin and acidic substance under the catalysis of zinc acetate, the acidic substance is one or more of methacrylic acid, maleic anhydride and methyltetrahydrophthalic anhydride, the bisphenol epoxy resin is epoxy resin 6101 or epoxy resin 128, and the mass ratio of bisphenol epoxy resin, acidic substance and zinc acetate is any ratio in (8.5-9.5):1:(0.009-0.011), for example, it can be any ratio in (8.5:1:0.009), (8.5:1:0.01), (9:1:0.009) and (9.5:1:0.011). The reaction temperature of the esterification reaction is any value in 120°C-140°C, for example, it can be any value in 120°C, 125°C, 130°C, 135°C and 140°C. The acid value of the epoxy ester is less than or equal to 2 mgKOH / g, for example, it may be any one of 2 mgKOH / g, 1.8 mgKOH / g, 1.6 mgKOH / g, 1.4 mgKOH / g and 1.2 mgKOH / g.
[0039] The present invention also applies to protect a high-voltage motor insulation system, including an inter-turn insulation layer wrapped around the surface of the core, a main insulation layer wrapped around the outside of a coil consisting of multiple turns of the core and the inter-turn insulation layer, and an anti-corona layer wrapped around the main insulation layer, the thickness of the inter-turn insulation layer is any value in the range of 0.35 mm to 0.40 mm, for example, it can be any value in the range of 0.35 mm, 0.36 mm, 0.37 mm, 0.38 mm, 0.39 mm and 0.40 mm, and is wrapped by a first low-resistance mica tape The anti-corona layer is obtained by wrapping the above-mentioned single-sided reinforced multi-glue mica tape, and the anti-corona layer includes a low-resistance anti-corona tape, a high-resistance anti-corona tape and a second low-glue mica tape reinforced with glass cloth. The total single-side thickness of the main insulating layer and the anti-corona layer is any value between 1.6mm and 1.8mm, for example, it can be any value between 1.6mm, 1.65mm, 1.7mm, 1.75mm and 1.8mm. After the inter-turn insulation layer, the main insulating layer and the anti-corona layer are wrapped, they are vacuum pressure impregnated and cured with the above-mentioned VPI resin.
[0040] The wire core is wrapped with low-resistance mica tape to form a coil, and high-resistance mica tape is wrapped around the outside of the multi-turn coil to form the main insulation layer. Since the high-resistance mica tape has high plasticity, the connection between the main insulation layer and the inter-turn insulation layer is relatively tight, which helps to improve the overall insulation performance. The low-resistance anti-corona tape, high-resistance anti-corona tape and the second low-resistance mica tape reinforced with glass cloth are sequentially wrapped around the outside of the main insulation layer to form an anti-corona layer. By wrapping the mica tape with glass cloth around the outside of the anti-corona tape, it helps to improve the anti-corona performance of the motor insulation system, increase the corona inception voltage, and help improve the insulation performance of the mica tape. The VPI resin is vacuum pressure impregnated and cured to fully impregnate the main insulation layer and the anti-corona layer with VPI resin, fill the gaps, improve the integrity and insulation capacity, and thus achieve the thinning of the high-voltage motor insulation system.
[0041] In some embodiments, the inter-turn insulation layer includes several types of first low-resistance mica tapes, the thickness of the first low-resistance mica tapes is any value between 0.05 mm and 0.09 mm, for example, it can be any value between 0.05 mm, 0.06 mm, 0.07 mm, 0.08 mm and 0.09 mm, and the first low-resistance mica tapes are reinforced by polyester film or polyimide film.
[0042] Please refer to the following examples and comparative examples for details.
[0043] Embodiment 1:
[0044] The high-voltage motor insulation system shown in a preferred embodiment of the present application includes an inter-turn insulation layer, a main insulation layer and an anti-corona layer, wherein the inter-turn insulation layer is formed by a low-resistance mica tape wrapped around the wire core, the wire core winding under the protection of the inter-turn insulation layer forms a multi-turn coil, the main insulation layer is obtained by wrapping a single-sided reinforced multi-resistance mica tape wrapped around the outside of the multi-turn coil, and the outside of the main insulation layer is wrapped with a low-resistance anti-corona tape, a high-resistance anti-corona tape and a second low-resistance mica tape reinforced with glass cloth to form an anti-corona layer. This embodiment also includes a VPI resin that penetrates into the main insulation layer through a vacuum pressure impregnation process.
[0045] The method for constructing the high-voltage motor insulation system in this embodiment includes:
[0046] S1. Use a polyester film reinforced mica tape with a thickness of 0.051 mm to wrap the electromagnetic wire in two layers in a half-lap manner to form a 0.40 mm thick inter-turn insulation layer, and use the electromagnetic wire wrapped with the polyester film reinforced mica tape to prepare a shuttle coil and expand it into a coil. The polyester film reinforced mica tape is 50g / m 2 Calcined mica paper.
[0047] S2. Wrap 6 layers of single-sided reinforced multi-resin mica tape with a thickness of 0.148 mm on the surface of the coil in a half-lapped form to form the main insulation layer.
[0048] S3. Wrap a 0.08mm thick low-resistance anti-corona tape in a half-lapped form on the outside of the main insulation layer of the straight part of the coil, and wrap a 0.2mm thick high-resistance anti-corona tape in a half-lapped form from the end of the low-resistance anti-corona tape to the bend of the coil, with the high and low tapes overlapping by 2cm. Wrap a 0.13mm thick second low-resistance mica tape reinforced with glass cloth on the surface of the high-resistance anti-corona tape to form an anti-corona layer.
[0049] S4. The whole is impregnated with VPI resin through vacuum pressure impregnation process to prepare a thinned insulation system suitable for 10kV high-voltage motors. The total single-side thickness of the main insulation layer and the anti-corona layer is 1.78mm.
[0050] In the above experimental steps, polyester film reinforced low-resistance mica tape, low-resistance anti-corona tape, high-resistance anti-corona tape and glass cloth reinforced low-resistance mica tape were all purchased.
[0051] In step S2, the single-sided reinforced multi-glue mica tape includes a polyester film, a first adhesive layer, a mica paper and a second adhesive layer arranged in sequence, and its thickness is 0.148 mm, and the mica content is 119 g / m 2 , glue content is 81.5g / m 2 The preparation method thereof comprises:
[0052] S210. On a mica tape production line, unwind a polyester film having a thickness of 0.03 mm, and evenly apply a first adhesive on its upper surface.
[0053] S220, using the first adhesive to bond 125g / m 2 The calcined mica paper is passed through a drying oven at a temperature of 110°C, and the first adhesive removes the solvent to form a first bonding layer, so that the polyester film and the mica paper are tightly compounded under the action of the first adhesive.
[0054] S230, then evenly apply a second adhesive on the surface of the mica paper away from the first adhesive layer, pass through a drying oven at a temperature of 110° C., remove the solvent from the second adhesive to form a second adhesive layer, and roll and slit to obtain a single-sided reinforced multi-adhesive mica tape.
[0055] In steps S210, S220 and S230, the first adhesive and the second adhesive are both prepared by dissolving the epoxy mixture in a mixed solvent, and the preparation method includes:
[0056] S201. Evenly mix toluene and acetone in a ratio of 1:1 to obtain a mixed solvent.
[0057] S202, weigh 5 kg of epoxy resin 6101, 11.5 kg of phenolic epoxy resin F51, 8 kg of epoxy ester and 1.3 kg of zinc isooctanoate respectively, mix well, and obtain an epoxy mixture.
[0058] S203, dissolving the epoxy mixture in a mixed solvent respectively to obtain a first adhesive having a solid content of 50% and a second adhesive having a solid content of about 20%, respectively.
[0059] The epoxy resin 6101, epoxy resin F51 and zinc isooctanoate in step S202 are all purchased, and the epoxy ester is obtained by esterification reaction of epoxy 128, methacrylic acid and zinc acetate in a mass ratio of (9:1:0.01) at 120°C, and is prepared on the spot. In this embodiment, the acid value of the epoxy ester is 1.9 mgKOH / g.
[0060] In step S4, the VPI resin has a relatively high breakdown field strength. The breakdown field strength of the VPI resin in this embodiment is 36 kV / mm. The preparation method thereof includes:
[0061] S410, weigh 50kg of viscosity 35s (23℃, 4 # To the JF-9965 modified epoxy VPI impregnating resin (viscosity cup), 6 kg of mica powder with an average particle size of 1 um was added, and then 0.12 g of BYK110 wetting and dispersing agent, 0.06 g of 5600 defoaming agent and 0.05 g of BYK333 leveling agent were added, and the mixture was stirred and mixed to obtain a mixed VPI impregnating resin.
[0062] S420, grinding and dispersing the mixed VPI impregnation resin for 3 hours, and introducing cooling water during the grinding process to keep the temperature below 50° C. After grinding, filtering is performed using a 500-mesh filter to obtain the VPI resin used for vacuum pressure impregnation in this embodiment.
[0063] Embodiment 2:
[0064] The difference between this embodiment and the first embodiment is that the thickness of the first less-resin mica tape in this embodiment is 0.050 mm, the thickness of the inter-turn insulation layer is 0.38 mm, the thickness of the single-sided reinforced more-resin mica tape is 0.163 mm, and the mica content is 128 g / m 2 , the glue content is 83.6g / m 2 The total thickness of the main insulating layer and the anti-corona layer on one side is 1.63 mm. The breakdown field strength of the VPI resin in this embodiment is 34 kV / mm.
[0065] In step S202, 7.5 kg of epoxy resin 6101, 16 kg of phenolic epoxy resin F44, 9 kg of epoxy ester and 1.8 kg of zinc isooctanoate are weighed and mixed evenly to obtain an epoxy mixture. In the epoxy ester, maleic anhydride of equal mass is used to replace methacrylic acid to participate in the esterification reaction, and the reaction temperature is 135° C. The acid value of the epoxy ester in this embodiment is 1.7 mgKOH / g.
[0066] In step S410, 62 kg of a 36 s (23 ° C, 4 # To the JF-9965-3E modified epoxy VPI impregnating resin (viscosity cup), 7 kg of mica powder with an average particle size of 1 um was added, and then 0.23 g of BYK110 wetting and dispersing agent, 0.09 g of 5600 defoaming agent and 0.1 g of BYK333 leveling agent were added, and the mixture was stirred and mixed to obtain a mixed VPI impregnating resin.
[0067] Embodiment three:
[0068] The difference between this embodiment and the first embodiment is that the thickness of the first low-resin mica tape in this embodiment is 0.050 mm, it is reinforced with polyimide film, the thickness of the inter-turn insulation layer is 0.38 mm, and the breakdown field strength of the VPI resin in this embodiment is 34 kV / mm.
[0069] In step S410, 62 kg of a 36 s (23 ° C, 4 # To the JF-9965-3E modified epoxy VPI impregnating resin (viscosity cup), 7 kg of mica powder with an average particle size of 1 um was added, and then 0.23 g of BYK110 wetting and dispersing agent, 0.09 g of 5600 defoaming agent and 0.1 g of BYK333 leveling agent were added, and the mixture was stirred and mixed to obtain a mixed VPI impregnating resin.
[0070] The thickness of the low-resistance anti-corona tape in the anti-corona layer is 0.1mm, the thickness of the high-resistance anti-corona tape is 0.18mm, and the thickness of the second low-resistance mica tape reinforced with glass cloth is 0.12mm.
[0071] Embodiment 4:
[0072] The difference between this embodiment and the first embodiment is that the thickness of the first low-resistance mica tape in this embodiment is 0.09 mm, and it is reinforced with a polyimide film and uses a 75 g / m 2 Calcined mica paper production, the thickness of the inter-turn insulation layer obtained after one and a half layers of stacking is 0.35mm, the thickness of the single-sided reinforced multi-resin mica tape is 0.145mm, and the mica content is 118g / m 2 , glue content is 78.5g / m 2 The total thickness of the main insulating layer and the anti-corona layer on one side is 1.63 mm. The breakdown field strength of the VPI resin in this embodiment is 37 kV / mm.
[0073] In step S202, 10.5 kg of epoxy resin 128, 23 kg of novolac epoxy resin F44, 13 kg of epoxy ester and 2.3 kg of zinc isooctanoate are weighed and mixed uniformly to obtain an epoxy mixture. In the epoxy ester, methyltetrahydrophthalic anhydride of equal mass is used instead of methacrylic acid to participate in the esterification reaction, and the reaction temperature is 135° C. The acid value of the epoxy ester in this embodiment is 1.8 mgKOH / g.
[0074] In step S410, 50 kg of a 32 s (23 ° C, 4 # To the JF-9965 modified epoxy VPI impregnating resin (viscosity cup), 6 kg of mica powder with an average particle size of 1 um was added, and then 0.12 g of BYK110 wetting and dispersing agent, 0.06 g of 5600 defoaming agent and 0.05 g of BYK333 leveling agent were added, and the mixture was stirred and mixed to obtain a mixed VPI impregnating resin.
[0075] Comparative Example 1:
[0076] The inter-turn insulation layer in this comparative example is made of 2 and a half layers of polyimide film with a thickness of 0.025 mm, and is wound with 1 and a half layers of 5442-1D polyester film low-glue mica tape produced by Wuhan Changfeng Mica Insulation Material Co., Ltd. The thickness of the WD5446-2 polyester film single-sided reinforced low-glue mica tape is 0.10 mm, and the total thickness of the inter-turn insulation layer is about 0.50 mm.
[0077] The main insulation layer in this comparative example is composed of the second low-glue mica tape reinforced with glass cloth in Example 1 and the 5442-1P polyester film low-glue powder mica tape produced by Wuhan Changfeng Mica Insulation Material Co., Ltd. in a 4 plus 4 half-fold package, wherein the thickness of the 5442-1P polyester film low-glue powder mica tape is 0.14mm. The arrangement of the low-resistance anti-corona tape and the high-resistance anti-corona tape is the same as in Example 1, and a 0.1mm commercially available glass ribbon is half-folded on the outer side of the high-resistance anti-corona tape. The overall VPI is impregnated with epoxy-modified unsaturated polyesterimide VPI resin to prepare a motor insulation system, and the single-sided main insulation thickness of the motor insulation system is about 2.08mm.
[0078] Comparative Example 2:
[0079] The only difference between this comparative example and comparative example 1 is that the main insulating layer in this comparative example is obtained by half-wrapping 8 layers of 5442-1P polyester film low-glue mica tape in comparative example 1, wrapping anti-corona tape and glass ribbon and vacuum impregnating.
[0080] Performance test:
[0081] The insulation properties of Examples 1 to 4 and Comparative Examples 1 and 2 were tested and recorded. The results are shown in Table 1.
[0082] Table 1: Insulation performance comparison table
[0083]
[0084]
[0085] Among them, the methods for dielectric loss, breakdown voltage strength, 2.53UN electrical aging life and corona inception voltage testing refer to the industry standard "Technical Conditions for High Voltage Motor Stator Coils" issued by the Ministry of Industry and Information Technology of the People's Republic of China, with the standard number JB / T 12685-2016 and the release date January 15, 2016. The partial discharge test refers to the national standard "High Voltage Test Technology Partial Discharge Measurement" issued by the State Administration for Market Regulation and the Standardization Administration of China, with the standard number GB / T 7354-2018 and the release date September 17, 2018.
[0086] By comparing Examples 1 to 4 with Comparative Examples 1 and 2, and referring to the data in Table 1, it can be seen that the single-sided reinforced multi-resin mica tape of the present invention has better dielectric loss, breakdown voltage strength, partial discharge, corona inception voltage and other properties than the existing glass cloth reinforced low-resin mica tape. And the use of a low-volatile, high-breakdown voltage epoxy VPI resin system for vacuum impregnation helps to reduce dielectric loss. The motor insulation system of the present invention can effectively reduce the thickness of the insulation layer and increase the service life of the insulation layer.
[0087] The beneficial effect of the present invention is that by combining the single-sided reinforced multi-resin mica tape with the vacuum pressure impregnation process using high-breakdown VPI resin doped with mica powder, the insulation performance of the insulation protection layer is improved, and the thinning of the high-voltage motor insulation system is achieved.
[0088] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0089] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An insulating protective layer, characterized in that: The single-sided reinforced multi-glue mica tape is wrapped and then vacuum pressure impregnated with VPI resin. The single-sided reinforced multi-glue mica tape includes a polyester film, a first adhesive layer, mica paper, and a second adhesive layer. The first adhesive layer is used for bonding and compounding the polyester film and the mica paper. The second adhesive layer is formed on the side of the mica paper away from the first adhesive layer. The adhesive content of the single-sided reinforced multi-glue mica tape is 70g / m 2 ~90g / m 2 Any value in, the mass of the mica paper is 117g / m 2 ~143g / m 2 Any value in .
2. The insulating protective layer according to claim 1, characterized in that: The VPI resin is obtained by doping mica powder with epoxy or epoxy-modified unsaturated polyester VPI resin, the particle size of the mica powder is any value between 0.5um and 10um, the added mass ratio is any value between 10% and 20%, and the breakdown field strength value of the VPI resin is greater than or equal to 33kV / mm.
3. The insulating protective layer according to claim 2, characterized in that: The thickness of the polyester film is any value between 0.02 mm and 0.04 mm, the mica paper is a calcined mica paper, the first bonding layer is formed by drying a first adhesive coated on the polyester film at a baking temperature, the second bonding layer is formed by drying a second adhesive coated on the mica paper at the baking temperature, the first adhesive and the second adhesive are both prepared by dissolving an epoxy mixture in a mixed solvent of toluene and acetone, the ratio of the toluene to the acetone in the mixed solvent is any ratio between 1:(0.9 and 1.1), and the thickness of the single-sided reinforced multi-glue mica tape is any value between 0.14 mm and 0.18 mm.
4. The insulating protective layer according to claim 3, characterized in that: The first adhesive is applied to the polyester film and then dried at the baking temperature, the mica paper is compounded, and the second adhesive is applied and then dried again at the baking temperature, the solid content of the first adhesive is any value between 45% and 55%, the solid content of the second adhesive is any value between 15% and 25%, and the baking temperature is any value between 100°C and 120°C.
5. The insulating protective layer according to claim 3, characterized in that: The epoxy mixture includes bisphenol A epoxy resin, novolac epoxy resin, epoxy ester and epoxy resin curing agent, and the mass ratio of the bisphenol A epoxy resin, the novolac epoxy resin, the epoxy ester and the epoxy resin curing agent is any ratio of 1:(2-3):(1-2):(0.2-1).
6. The insulating protective layer according to claim 5, characterized in that: The epoxy ester is obtained by an esterification reaction between a bisphenol epoxy resin and an acidic substance under the catalysis of zinc acetate, wherein the acidic substance is one or more of methacrylic acid, maleic anhydride and methyltetrahydrophthalic anhydride. The bisphenol epoxy resin is epoxy resin 6101 or epoxy resin 128. The mass ratio of the bisphenol epoxy resin, the acidic substance and the zinc acetate is any ratio between (8.5 and 9.5):1:(0.009 and 0.011). The reaction temperature of the esterification reaction is any value between 120°C and 140°C. The acid value of the epoxy ester is less than or equal to 2 mgKOH / g.
7. The insulating protective layer according to claim 5, characterized in that: The bisphenol A type epoxy resin is epoxy resin 6101 or epoxy resin 128, the novolac epoxy resin is novolac epoxy resin F51 or novolac epoxy resin F44, and the epoxy resin curing agent is zinc isooctanoate.
8. A high voltage motor insulation system, characterized in that: It includes an inter-turn insulation layer wrapped around the surface of the wire core, a main insulation layer wrapped around the outside of a plurality of turns of a coil consisting of the wire core and the inter-turn insulation layer, and an anti-corona layer wrapped around the main insulation layer, the thickness of the inter-turn insulation layer is any value between 0.35 mm and 0.40 mm, and is obtained by winding a first low-resistance mica tape, and is obtained by winding a single-sided reinforced multi-resistance mica tape as described in any one of claims 1 to 6, the anti-corona layer includes a low-resistance anti-corona tape, a high-resistance anti-corona tape and a second low-resistance mica tape reinforced with glass cloth, the total single-side thickness of the main insulation layer and the anti-corona layer is any value between 1.6 mm and 1.8 mm, and after the inter-turn insulation layer, the main insulation layer and the anti-corona layer are wound, they are vacuum pressure impregnated and cured with the VPI resin as described in any one of claims 1 to 6.
9. The high voltage motor insulation system according to claim 8, characterized in that: The inter-turn insulation layer includes several types of the first low-resistance mica tapes, the thickness of the first low-resistance mica tapes is any value between 0.05 mm and 0.09 mm, and the first low-resistance mica tapes are reinforced by polyester films or polyimide films.
Citation Information
Cited By
Motor insulation system with environmental adaptability and heat dissipation optimization
CN120638717A