Preparation method of porous nitrogen-doped carbon-loaded noble metal catalyst and application of porous nitrogen-doped carbon-loaded noble metal catalyst in synthesis of o-chloroaniline
Through the preparation of porous nitrogen-doped carbon-supported precious metal catalysts, the problem of dechlorination side reaction of precious metal catalysts in hydrogenation synthesis is solved, and a high selectivity and stable catalytic effect is achieved, which simplifies the preparation process and reduces costs.
Patent Information
- Application Number
- CN202411048793.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
The existing precious metal catalysts have side reactions in the process of catalytic hydrogenation of ortho-chloroaniline, resulting in low selectivity, complex preparation methods and high cost, which limits their widespread application in industry.
The preparation method of porous nitrogen-doped carbon-supported precious metal catalyst is adopted, and aged by mixing and stirring of carbon source, metal source and nitrogen source, followed by calcining in a nitrogen atmosphere and washing with acidic liquid to form a porous nitrogen-doped carbon support, and then through impregnation The noble metal salt forms a catalyst, achieving uniform dispersion of the catalyst and electronic structure regulation.
The catalyst has a high specific surface area and multi-stage pore structure. The nitrogen in the support interacts with precious metal nanoparticles, inhibits the side reaction of dechlorination, improves catalytic activity and selectivity, reduces the amount of dechlorination during hydrogenation, and does not Additional dechlorination inhibitors are required, and the catalyst activity is stable.
Smart Images

Figure CN118976525A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical catalysts, and in particular to a method for preparing a porous nitrogen-doped carbon-supported noble metal catalyst and application of the catalyst in the synthesis of o-chloroaniline. Background Art
[0002] Chloroaniline (CAN) is an important chemical intermediate, widely used in medicine, dyes, pesticides and organic synthesis. Catalytic hydrogenation of chloronitrobenzene (CNB) is a common method for synthesizing CAN, but this process has a dechlorination side reaction, that is, when CAN is hydrogenated, dechlorination byproducts may be produced. Therefore, how to improve the selectivity of CAN and avoid or reduce the dechlorination side reaction is the focus and difficulty of research in this field.
[0003] At present, in order to improve the selectivity of catalytic hydrogenation, researchers have developed a variety of catalysts, including precious metal catalysts, skeleton nickel and amorphous alloys. Precious metal catalysts have attracted attention due to their high activity and good selectivity. In recent years, researchers have also explored catalysts based on transition metal nitrides, such as CoMoNx / CNTs (cobalt molybdenum nitride supported on carbon nanotubes). These catalysts improve catalytic activity and selectivity by adjusting the interaction between metal components and carriers, preparing bi / multi-metal catalysts, amorphous alloys and other methods.
[0004] The invention patent application with publication number CN106732549A discloses a porous carbon-supported composite material catalyst, which uses carbon quantum dots to modulate the outer electron distribution characteristics of the active component particles to improve the dechlorination inhibition effect. Although the selectivity of o-chloroaniline can reach 100%, the preparation method is complicated, and the active component needs two or more species to cooperate, and the cost is relatively high. The invention patent application with publication number CN116722160A discloses a preparation method for a composite carbon carrier for loading platinum-based precious metal particles, in which carbon black is coated with a polymer material as a carbon carrier, and its main function is to enhance conductivity and stability. The invention patent application with publication number CN114438536A discloses a porous carbon-supported precious metal catalyst and its preparation method, but the catalyst prepared therein has a specific carbonization structure, and it is used in the process of electrolysis of water to produce hydrogen, does not have o-chloroaniline selectivity, and cannot inhibit dechlorination.
[0005] Although precious metal catalysts have many advantages, their high cost and resource scarcity also limit their widespread application in industry. Therefore, researchers are also exploring how to further improve the catalytic performance of precious metal catalysts and improve their effect in inhibiting dechlorination. Summary of the invention
[0006] The present invention provides a method for preparing a porous nitrogen-doped carbon-supported noble metal catalyst and application of the catalyst in the synthesis of o-chloroaniline.
[0007] To achieve the above-mentioned purpose and other related purposes, the technical solution provided by the present invention is: a method for preparing a porous nitrogen-doped carbon-supported noble metal catalyst, comprising the following steps:
[0008] Step 1: Add a carbon source and a metal source to distilled water and stir to mix, add an alkaline solution under stirring, continue stirring for 2 to 3 hours after mixing, and then age in an oil bath at 80 to 120° C. for 5 to 8 hours; then add a nitrogen source, continue stirring and aging for 5 to 8 hours, cool to 30 to 50° C. after aging, stir and dry to obtain a carrier precursor; calcine the carrier precursor at 750 to 950° C. under a nitrogen atmosphere, soak it in an acidic liquid after calcination, filter and wash until the upper clear liquid is pH neutral, and dry to obtain a porous nitrogen-doped carbon carrier;
[0009] Step 2: Immerse the porous nitrogen-doped carbon support obtained in step 1 in a H2O2 aqueous solution or a citric acid aqueous solution for 40 to 50 hours, filter, wash, and dry to obtain a modified porous nitrogen-doped carbon support;
[0010] Step 3: The modified porous nitrogen-doped carbon support obtained in step 2 is impregnated into an aqueous solution containing at least one of palladium salt, platinum salt and ruthenium salt, and then dried at 100-140° C. to obtain a porous nitrogen-doped carbon-loaded precious metal catalyst.
[0011] The preferred technical solution is: the carbon source is at least one of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, gluconic acid and aminotriacetic acid.
[0012] The preferred technical solution is: the metal source is at least one of MgCl2, CaCl2 and ZnCl2.
[0013] The preferred technical solution is: the nitrogen source is at least one of dicyanamide and melamine urea.
[0014] The preferred technical solution is: the molar ratio of the carbon source to the metal source is 1:1 to 1:4, and the mass ratio of the carbon source to the nitrogen source is 1:0.5 to 1:2.
[0015] The preferred technical solution is: the mass percentage of the H2O2 aqueous solution is 10-15wt%; the mass percentage of the citric acid aqueous solution is 20-25wt%.
[0016] The preferred technical solution is: the alkaline solution is a NaOH aqueous solution or a KOH aqueous solution; the acidic liquid is hydrochloric acid or nitric acid.
[0017] To achieve the above purpose and other related purposes, the technical solution provided by the present invention is: the use of the porous nitrogen-doped carbon-supported precious metal catalyst in the synthesis of o-chloroaniline, characterized in that the porous nitrogen-doped carbon-supported precious metal catalyst is added to an organic solvent containing o-chloronitrobenzene, reacted with hydrogen at 60°C to 120°C and a pressure of 0.2MPa to 2.0MPa, and after the catalytic reaction is completed, o-chloroaniline is obtained by treatment.
[0018] The preferred technical solution is: the organic solvent is at least one of methanol, ethanol, isopropanol and n-propanol.
[0019] The preferred technical solution is: the mass ratio of the porous nitrogen-doped carbon-supported noble metal catalyst to o-chloronitrobenzene is 1:10 to 1:20.
[0020] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0021] The main advantages of the catalyst prepared in this application are: (1) the catalyst carrier preparation method is simple and easy to prepare in batches, and has a multi-level pore structure; (2) the specific surface area of the catalyst is 800m 2 / g or more; (3) the nitrogen in the catalyst carrier interacts with the precious metal nanoparticles, which is beneficial to the dispersion of the active components; (4) the surface modification of the catalyst carrier is beneficial to the uniform dispersion of the precious metal particles; (5) the catalyst is used to catalyze the hydrogenation of o-chloronitrobenzene to prepare o-chloroaniline without the need to add a dechlorination inhibitor; (6) nitrogen regulates the electronic structure of the precious metal active components, inhibits the catalytic hydrogenation dechlorination side reaction, stabilizes the catalyst activity, and reduces the amount of dechlorination during the hydrogenation process. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Nitrogen adsorption and desorption curves and pore size distribution of porous nitrogen-doped carbon carriers.
[0023] Figure 2 SEM image of porous nitrogen-doped carbon-supported platinum nanoparticles. DETAILED DESCRIPTION
[0024] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in the embodiments.
[0025] See also Figure 1-2. It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions under which the present invention can be implemented. Therefore, they have no substantive technical significance, and any structural modification, change in proportional relationship or adjustment of size. The following examples are provided to better understand the present invention, but are not intended to limit the present invention. The experimental methods in the following examples are all conventional methods unless otherwise specified. The experimental materials used in the following examples are all purchased from conventional biochemical reagent stores unless otherwise specified.
[0026] Example 1: Preparation method of porous nitrogen-doped carbon-supported noble metal catalyst and its application in the synthesis of o-chloroaniline
[0027] (1) Preparation of porous nitrogen-doped carbon
[0028] The carbon source ethylenediaminetetraacetic acid and the metal source MgCl2 are added to distilled water in a molar ratio of 1:4, stirred and dissolved, and NaOH solution is added dropwise under stirring. After sufficient mixing, stirring is continued for 3 hours, and then oil bath aging is performed at 100°C for 6 hours; then, nitrogen source melamine is added in a mass ratio of carbon source to nitrogen source of 1:1, and stirring and aging are continued for 6 hours. After aging, the temperature is lowered to 40°C and stirred and dried to obtain a carrier precursor; the carrier precursor is calcined at 950°C under a nitrogen atmosphere, and after calcination, it is soaked and washed with hydrochloric acid, filtered and washed until the upper clear liquid is pH neutral, and dried to obtain a porous nitrogen-doped carbon carrier.
[0029] (2) Modification of porous nitrogen-doped carbon supports
[0030] The porous nitrogen-doped carbon prepared in step (1) was immersed in a 12 wt% H2O2 aqueous solution for 48 hours, filtered, washed, and dried to obtain a modified porous nitrogen-doped carbon carrier.
[0031] (3) Catalyst loading
[0032] The modified porous nitrogen-doped carbon support described in step (2) is immersed in a platinum salt aqueous solution with a theoretical platinum loading of 1 wt.%, and dried at 120° C. to obtain the porous nitrogen-doped carbon-loaded noble metal catalyst.
[0033] Figure 1 The nitrogen adsorption and desorption curves and pore size distribution of porous nitrogen-doped carbon carriers. Figure 1 It can be seen that the pores of the nitrogen-doped carbon support are mainly mesopores, and the main pore size is concentrated between 2 and 4 nm. The nitrogen adsorption and desorption test shows that the pore volume of the support is 1.47 cm 3 / g, average pore size 7.2nm, specific surface area 891.7m 2 / g.
[0034] Figure 2 This is a SEM image of porous nitrogen-doped carbon supported platinum nanoparticles. Figure 2 It can be seen that the rough small nano-particles of Pt particles are evenly dispersed on the carrier, proving that the carrier has a strong interaction with the noble metal, which is conducive to the dispersion of the noble metal.
[0035] In the present invention, the porous structure and the oxygen-containing functional groups modified on the carbon surface are beneficial to the dispersion of the precious metals, and the nitrogen doping is beneficial to the dispersion of the precious metals, and the electronic structure is regulated by the interaction with the precious metals to inhibit dechlorination.
[0036] Example 2: Preparation method of porous nitrogen-doped carbon-supported noble metal catalyst and its application in the synthesis of o-chloroaniline
[0037] (1) Preparation of porous nitrogen-doped carbon
[0038] The carbon source ethylenediaminetetraacetic acid and the metal source MgCl2 are added to distilled water in a molar ratio of 1:4, stirred and dissolved, and NaOH solution is added dropwise under stirring. After sufficient mixing, stirring is continued for 3 hours, and then oil bath aging is performed at 100°C for 6 hours; then, nitrogen source melamine is added in a mass ratio of carbon source to nitrogen source of 1:1, and stirring and aging are continued for 6 hours. After aging, the temperature is lowered to 40°C and stirred and dried to obtain a carrier precursor; the carrier precursor is calcined at 750°C under a nitrogen atmosphere, and after calcination, it is soaked and washed with hydrochloric acid, filtered and washed until the upper clear liquid is pH neutral, and dried to obtain a porous nitrogen-doped carbon carrier.
[0039] (2) Modification of porous nitrogen-doped carbon supports
[0040] The porous nitrogen-doped carbon prepared in step (1) was immersed in a 12 wt% H2O2 aqueous solution for 48 hours, filtered, washed, and dried to obtain a modified porous nitrogen-doped carbon carrier.
[0041] (3) Catalyst loading
[0042] The modified porous nitrogen-doped carbon support described in step (2) is immersed in a platinum salt aqueous solution with a theoretical platinum loading of 1 wt.%, and dried at 120° C. to obtain the porous nitrogen-doped carbon-loaded noble metal catalyst.
[0043] Example 3: Preparation method of porous nitrogen-doped carbon-supported noble metal catalyst and its application in the synthesis of o-chloroaniline
[0044] (1) Preparation of porous nitrogen-doped carbon
[0045] The carbon source gluconic acid and the metal source MgCl2 are added to distilled water in a molar ratio of 1:1, stirred and dissolved, and NaOH solution is added dropwise under stirring conditions. After sufficient mixing, stirring is continued for 3 hours, and then oil bath aging is performed at 100°C for 6 hours; then, nitrogen source melamine is added in a mass ratio of carbon source to nitrogen source of 1:1, and stirring and aging is continued for 6 hours. After aging, the temperature is lowered to 40°C and stirred and dried to obtain a carrier precursor; the carrier precursor is calcined at 950°C under a nitrogen atmosphere, and after calcination, it is soaked and washed with hydrochloric acid, filtered and washed until the upper clear liquid is pH neutral, and dried to obtain a porous nitrogen-doped carbon carrier.
[0046] (2) Modification of porous nitrogen-doped carbon supports
[0047] The porous nitrogen-doped carbon prepared in step (1) was immersed in a 12 wt% H2O2 aqueous solution for 48 hours, filtered, washed, and dried to obtain a modified porous nitrogen-doped carbon carrier.
[0048] (3) Catalyst loading
[0049] The modified porous nitrogen-doped carbon support described in step (2) is immersed in a platinum salt aqueous solution with a theoretical platinum loading of 1 wt.%, and dried at 120° C. to obtain the porous nitrogen-doped carbon-loaded noble metal catalyst.
[0050] Example 4: Preparation method of porous nitrogen-doped carbon-supported noble metal catalyst and its application in the synthesis of o-chloroaniline
[0051] (1) Preparation of porous nitrogen-doped carbon
[0052] The carbon source gluconic acid and the metal source MgCl2 are added to distilled water in a molar ratio of 1:4, stirred and dissolved, and NaOH solution is added dropwise under stirring conditions. After sufficient mixing, stirring is continued for 3 hours, and then oil bath aging is performed at 100°C for 6 hours; then, the nitrogen source dinitrile amide is added in a mass ratio of carbon source to nitrogen source of 1:2, and stirring and aging are continued for 6 hours. After aging, the temperature is lowered to 40°C and stirred and dried to obtain a carrier precursor; the carrier precursor is calcined at 950°C under a nitrogen atmosphere, and after calcination, it is soaked and washed with hydrochloric acid, filtered and washed until the upper clear liquid is pH neutral, and dried to obtain a porous nitrogen-doped carbon carrier.
[0053] (2) Modification of porous nitrogen-doped carbon supports
[0054] The porous nitrogen-doped carbon prepared in step (1) was immersed in a 12 wt% H2O2 aqueous solution for 48 hours, filtered, washed, and dried to obtain a modified porous nitrogen-doped carbon carrier.
[0055] (3) Catalyst loading
[0056] The modified porous nitrogen-doped carbon support described in step (2) is immersed in a palladium salt aqueous solution with a theoretical platinum loading of 1 wt.%, and dried at 120° C. to obtain the porous nitrogen-doped carbon-loaded noble metal catalyst.
[0057] Example 5: Preparation method of porous nitrogen-doped carbon-supported noble metal catalyst and its application in the synthesis of o-chloroaniline
[0058] (1) Preparation of porous nitrogen-doped carbon
[0059] The carbon source ethylenediaminetetraacetic acid and the metal source MgCl2 are added to distilled water in a molar ratio of 1:2, stirred and dissolved, and NaOH solution is added dropwise under stirring. After sufficient mixing, stirring is continued for 3 hours, and then oil bath aging is performed at 100°C for 6 hours; then, the nitrogen source dinitrile amide is added in a mass ratio of carbon source to nitrogen source of 1:1, and stirring and aging are continued for 6 hours. After aging, the temperature is lowered to 40°C and stirred and dried to obtain a carrier precursor; the carrier precursor is calcined at 950°C under a nitrogen atmosphere, and after calcination, it is soaked and washed with hydrochloric acid, filtered and washed until the upper clear liquid is pH neutral, and dried to obtain a porous nitrogen-doped carbon carrier.
[0060] (2) Modification of porous nitrogen-doped carbon supports
[0061] The porous nitrogen-doped carbon prepared in step (1) was immersed in a 25 wt % citric acid aqueous solution for 48 hours, filtered, washed, and dried to obtain a modified porous nitrogen-doped carbon carrier.
[0062] (3) Catalyst loading
[0063] The modified porous nitrogen-doped carbon support described in step (2) is immersed in a palladium salt aqueous solution with a theoretical palladium loading of 1 wt.%, and dried at 120° C. to obtain the porous nitrogen-doped carbon-loaded noble metal catalyst.
[0064] Example 6: Preparation method of porous nitrogen-doped carbon-supported noble metal catalyst and its application in the synthesis of o-chloroaniline
[0065] (1) Preparation of porous nitrogen-doped carbon
[0066] The carbon source ethylenediaminetetraacetic acid and the metal source CaCl2 are added to distilled water in a molar ratio of 1:4, stirred and dissolved, and NaOH solution is added dropwise under stirring. After sufficient mixing, stirring is continued for 3 hours, and then oil bath aging is performed at 100°C for 6 hours; then, the nitrogen source dinitrile amide is added in a mass ratio of carbon source to nitrogen source of 1:1, and stirring and aging are continued for 6 hours. After aging, the temperature is lowered to 40°C and stirred and dried to obtain a carrier precursor; the carrier precursor is calcined at 950°C under a nitrogen atmosphere, and after calcination, it is soaked and washed with hydrochloric acid, filtered and washed until the upper clear liquid is pH neutral, and dried to obtain a porous nitrogen-doped carbon carrier.
[0067] (2) Modification of porous nitrogen-doped carbon supports
[0068] The porous nitrogen-doped carbon prepared in step (1) was immersed in a 12 wt% H2O2 aqueous solution for 48 hours, filtered, washed, and dried to obtain a modified porous nitrogen-doped carbon carrier.
[0069] (3) Catalyst loading
[0070] The modified porous nitrogen-doped carbon support described in step (2) is immersed in a platinum salt aqueous solution with a theoretical platinum loading of 2 wt.%, and dried at 120° C. to obtain the porous nitrogen-doped carbon-loaded noble metal catalyst.
[0071] Comparative Example 1:
[0072] (1) Preparation of porous nitrogen-doped carbon
[0073] The carbon source ethylenediaminetetraacetic acid and the metal source MgCl2 are added to distilled water in a molar ratio of 1:0.5, stirred and dissolved, and NaOH solution is added dropwise under stirring. After sufficient mixing, stirring is continued for 3 hours, and then oil bath aging is performed at 100°C for 6 hours; then, the nitrogen source dinitrile amide is added in a mass ratio of carbon source to nitrogen source of 1:1, and stirring and aging are continued for 6 hours. After aging, the temperature is lowered to 40°C and stirred and dried to obtain a carrier precursor; the carrier precursor is calcined at 950°C under a nitrogen atmosphere, and after calcination, it is soaked and washed with hydrochloric acid, filtered and washed until the upper clear liquid is pH neutral, and dried to obtain a porous nitrogen-doped carbon carrier.
[0074] (2) Modification of porous nitrogen-doped carbon supports
[0075] The porous nitrogen-doped carbon prepared in step (1) was immersed in a 12 wt% H2O2 aqueous solution for 48 hours, filtered, washed, and dried to obtain a modified porous nitrogen-doped carbon carrier.
[0076] (3) Catalyst loading
[0077] The modified porous nitrogen-doped carbon support described in step (2) is immersed in a platinum salt aqueous solution with a theoretical platinum loading of 1 wt.%, and dried at 120° C. to obtain the porous nitrogen-doped carbon-loaded noble metal catalyst.
[0078] Comparative Example 2:
[0079] (1) Preparation of porous nitrogen-doped carbon
[0080] The carbon source ethylenediaminetetraacetic acid and the metal source MgCl2 are added to distilled water in a molar ratio of 1:4, stirred and dissolved, and NaOH solution is added dropwise under stirring. After sufficient mixing, stirring is continued for 3 hours, and then oil bath aging is performed at 100°C for 6 hours; then, the nitrogen source dinitrile amide is added in a mass ratio of carbon source to nitrogen source of 1:1, and stirring and aging are continued for 6 hours. After aging, the temperature is lowered to 40°C and stirred and dried to obtain a carrier precursor; the carrier precursor is calcined at 650°C under a nitrogen atmosphere, and after calcination, it is soaked and washed with hydrochloric acid, filtered and washed until the upper clear liquid is pH neutral, and dried to obtain a porous nitrogen-doped carbon carrier.
[0081] (2) Modification of porous nitrogen-doped carbon supports
[0082] The porous nitrogen-doped carbon prepared in step (1) was immersed in a 12 wt% H2O2 aqueous solution for 48 hours, filtered, washed, and dried to obtain a modified porous nitrogen-doped carbon carrier.
[0083] (3) Catalyst loading
[0084] The modified porous nitrogen-doped carbon support described in step (2) is immersed in a platinum salt aqueous solution with a theoretical platinum loading of 1 wt.%, and dried at 120° C. to obtain the porous nitrogen-doped carbon-loaded noble metal catalyst.
[0085] Comparative Example 3:
[0086] (1) Preparation of porous nitrogen-doped carbon
[0087] The carbon source ethylenediaminetetraacetic acid and the metal source MgCl2 are added to distilled water in a molar ratio of 1:4, stirred and dissolved, and NaOH solution is added dropwise under stirring. After sufficient mixing, stirring is continued for 3 hours, and then oil bath aging is performed at 100°C for 6 hours; then, the nitrogen source dinitrile amide is added in a mass ratio of carbon source to nitrogen source of 1:1, and stirring and aging is continued for 6 hours. After aging, the temperature is lowered to 40°C and stirred and dried to obtain a carrier precursor; the carrier precursor is calcined at 1050°C under a nitrogen atmosphere, and after calcination, it is soaked and washed with hydrochloric acid, filtered and washed until the upper clear liquid is pH neutral, and dried to obtain a porous nitrogen-doped carbon carrier.
[0088] (2) Modification of porous nitrogen-doped carbon supports
[0089] The porous nitrogen-doped carbon prepared in step (1) was immersed in a 12 wt% H2O2 aqueous solution for 48 hours, filtered, washed, and dried to obtain a modified porous nitrogen-doped carbon carrier.
[0090] (3) Catalyst loading
[0091] The modified porous nitrogen-doped carbon support described in step (2) is immersed in a platinum salt aqueous solution with a theoretical platinum loading of 1 wt.%, and dried at 120° C. to obtain the porous nitrogen-doped carbon-loaded noble metal catalyst.
[0092] Comparative Example 4:
[0093] (1) Preparation of porous nitrogen-doped carbon
[0094] The carbon source ethylenediaminetetraacetic acid and the metal source MgCl2 are added to distilled water in a molar ratio of 1:4, stirred and dissolved, and NaOH solution is added dropwise under stirring. After sufficient mixing, stirring is continued for 3 hours, and then oil bath aging is performed at 100°C for 6 hours; then, the nitrogen source dinitrile amide is added in a mass ratio of carbon source to nitrogen source of 1:3, and stirring and aging is continued for 6 hours. After aging, the temperature is lowered to 40°C and stirred and dried to obtain a carrier precursor; the carrier precursor is calcined at 850°C under a nitrogen atmosphere, and after calcination, it is soaked and washed with hydrochloric acid, filtered and washed until the upper clear liquid is pH neutral, and dried to obtain a porous nitrogen-doped carbon carrier.
[0095] (2) Modification of porous nitrogen-doped carbon supports
[0096] The porous nitrogen-doped carbon prepared in step (1) was immersed in a 12 wt% H2O2 aqueous solution for 48 hours, filtered, washed, and dried to obtain a modified porous nitrogen-doped carbon carrier.
[0097] (3) Catalyst loading
[0098] The modified porous nitrogen-doped carbon support described in step (2) is immersed in a platinum salt aqueous solution with a theoretical platinum loading of 1 wt.%, and dried at 120° C. to obtain the porous nitrogen-doped carbon-loaded noble metal catalyst.
[0099] Comparative Example 5:
[0100] (1) Preparation of porous nitrogen-doped carbon
[0101] The carbon source ethylenediaminetetraacetic acid and the metal source MgCl2 are added to distilled water in a molar ratio of 1:2, stirred and dissolved, and NaOH solution is added dropwise under stirring. After sufficient mixing, stirring is continued for 3 hours, and then oil bath aging is performed at 100°C for 6 hours; then, the nitrogen source dinitrile amide is added in a mass ratio of carbon source to nitrogen source of 1:1, and stirring and aging are continued for 6 hours. After aging, the temperature is lowered to 40°C and stirred and dried to obtain a carrier precursor; the carrier precursor is calcined at 950°C under a nitrogen atmosphere, and after calcination, it is soaked and washed with hydrochloric acid, filtered and washed until the upper clear liquid is pH neutral, and dried to obtain a porous nitrogen-doped carbon carrier.
[0102] (2) Modification of porous nitrogen-doped carbon supports
[0103] The porous nitrogen-doped carbon prepared in step (1) is immersed in a 30 wt % H2O2 aqueous solution for 24 hours, filtered, washed, and dried to obtain a modified porous nitrogen-doped carbon carrier.
[0104] (3) Catalyst loading
[0105] The modified porous nitrogen-doped carbon support described in step (2) is immersed in a palladium salt aqueous solution with a theoretical palladium loading of 1 wt.%, and dried at 120° C. to obtain the porous nitrogen-doped carbon-loaded noble metal catalyst.
[0106] Comparative Example 6:
[0107] (1) Preparation of porous nitrogen-doped carbon
[0108] The carbon source ethylenediaminetetraacetic acid and the metal source MgCl2 are added to distilled water in a molar ratio of 1:4, stirred and dissolved, and NaOH solution is added dropwise under stirring. After sufficient mixing, stirring is continued for 3 hours, and then oil bath aging is performed at 100°C for 6 hours; then, the nitrogen source dinitrile amide is added in a mass ratio of carbon source to nitrogen source of 1:1, and stirring and aging are continued for 6 hours. After aging, the temperature is lowered to 40°C and stirred and dried to obtain a carrier precursor; the carrier precursor is calcined at 950°C under a nitrogen atmosphere, and after calcination, it is soaked and washed with hydrochloric acid, filtered and washed until the upper clear liquid is pH neutral, and dried to obtain a porous nitrogen-doped carbon carrier.
[0109] (2) Modification of porous nitrogen-doped carbon supports
[0110] The porous nitrogen-doped carbon prepared in step (1) was immersed in a 12 wt% H2O2 aqueous solution for 48 hours, filtered, washed, and dried to obtain a modified porous nitrogen-doped carbon carrier.
[0111] (3) Catalyst loading
[0112] The modified porous nitrogen-doped carbon support described in step (2) is immersed in a palladium salt aqueous solution with a theoretical palladium loading of 5 wt.%, and dried at 120° C. to obtain the porous nitrogen-doped carbon-loaded noble metal catalyst.
[0113] Embodiment 7:
[0114] The catalyst prepared in Example 1 was added to an ethanol solution of o-chloronitrobenzene at a molar ratio of 1:10 to o-chloronitrobenzene, and reacted with hydrogen at 60°C and 0.3 MPa for 120 min. After the catalytic reaction, the reactants and the yield of o-chloroaniline were detected by gas chromatography, and the conversion rate and selectivity were calculated.
[0115] Embodiment 8:
[0116] The catalyst prepared in Example 2 was added to an ethanol solution of o-chloronitrobenzene at a molar ratio of 1:10 to o-chloronitrobenzene, and reacted with hydrogen at 60°C and 0.3 MPa for 120 min. After the catalytic reaction, the reactants and the yield of o-chloroaniline were detected by gas chromatography, and the conversion rate and selectivity were calculated.
[0117] Embodiment 9:
[0118] The catalyst prepared in Example 3 was added to an ethanol solution of o-chloronitrobenzene at a molar ratio of 1:10 to o-chloronitrobenzene, and reacted with hydrogen at 60°C and 0.3 MPa for 120 min. After the catalytic reaction, the reactants and the yield of o-chloroaniline were detected by gas chromatography, and the conversion rate and selectivity were calculated.
[0119] Embodiment 10:
[0120] The catalyst prepared in Example 4 was added to an ethanol solution of o-chloronitrobenzene at a molar ratio of 1:10 to o-chloronitrobenzene, and reacted with hydrogen at 60°C and 0.3 MPa for 120 min. After the catalytic reaction, the reactants and the yield of o-chloroaniline were detected by gas chromatography, and the conversion rate and selectivity were calculated.
[0121] Embodiment 11:
[0122] The catalyst prepared in Example 5 was added to an ethanol solution of o-chloronitrobenzene at a molar ratio of 1:10 to o-chloronitrobenzene, and reacted with hydrogen at 100°C and a pressure of 1.0 MPa for 150 minutes. After the catalytic reaction, the reactants and the yield of o-chloroaniline were detected by gas chromatography, and the conversion rate and selectivity were calculated.
[0123] Embodiment 12:
[0124] The catalyst prepared in Example 6 was added to an ethanol solution of o-chloronitrobenzene at a molar ratio of 1:20 to o-chloronitrobenzene, and reacted with hydrogen at 60°C and 0.5 MPa for 240 min. After the catalytic reaction, the reactants and the yield of o-chloroaniline were detected by gas chromatography, and the conversion rate and selectivity were calculated.
[0125] Embodiment 13:
[0126] The catalyst prepared in Comparative Example 1 was added to an ethanol solution of o-chloronitrobenzene at a molar ratio of 1:10 to o-chloronitrobenzene, and reacted with hydrogen at 60°C and 0.3 MPa for 240 minutes. After the catalytic reaction, the reactants and the yield of o-chloroaniline were detected by gas chromatography, and the conversion rate and selectivity were calculated.
[0127] Embodiment 14:
[0128] The catalyst prepared in Comparative Example 2 was added to an ethanol solution of o-chloronitrobenzene at a molar ratio of 1:10 to o-chloronitrobenzene, and reacted with hydrogen at 70°C and a pressure of 1.0 MPa for 240 minutes. After the catalytic reaction, the reactants and the yield of o-chloroaniline were detected by gas chromatography, and the conversion rate and selectivity were calculated.
[0129] Embodiment 15:
[0130] The catalyst prepared in Comparative Example 3 was added to an ethanol solution of o-chloronitrobenzene at a molar ratio of 1:10 to o-chloronitrobenzene, and reacted with hydrogen at 60°C and 0.3 MPa for 120 min. After the catalytic reaction, the reactants and the yield of o-chloroaniline were detected by gas chromatography, and the conversion rate and selectivity were calculated.
[0131] Embodiment 16:
[0132] The catalyst prepared in Comparative Example 4 was added to an ethanol solution of o-chloronitrobenzene at a molar ratio of 1:10 to o-chloronitrobenzene, and reacted with hydrogen at 60°C and 0.3 MPa for 120 minutes. After the catalytic reaction, the reactants and the yield of o-chloroaniline were detected by gas chromatography, and the conversion rate and selectivity were calculated.
[0133] Embodiment 17:
[0134] The catalyst prepared in Comparative Example 5 was added to an ethanol solution of o-chloronitrobenzene at a molar ratio of 1:10 to o-chloronitrobenzene, and reacted with hydrogen at 60°C and 0.3 MPa for 120 min. After the catalytic reaction, the reactants and the yield of o-chloroaniline were detected by gas chromatography, and the conversion rate and selectivity were calculated.
[0135] Embodiment 18:
[0136] The catalyst prepared in Comparative Example 6 was added to an ethanol solution of o-chloronitrobenzene at a molar ratio of 1:20 to o-chloronitrobenzene, and reacted with hydrogen at 100°C and a pressure of 1.0 MPa for 120 minutes. After the catalytic reaction, the reactants and the yield of o-chloroaniline were detected by gas chromatography, and the conversion rate and selectivity were calculated.
[0137] The test results of the reactant yields and product conversion rates in the above Examples 7 to 18 are shown in Table 1 below.
[0138] Table 1
[0139] o-Chloronitrobenzene conversion rate / % o-Chloroaniline selectivity / % Example 7 100 100 Example 8 99.5 98.0 Example 9 99.8 97.6 Example 10 98.3 97.0 Embodiment 11 98.0 95.0 Example 12 97.3 96.0 Example 13 98.5 68.6 Embodiment 14 62.5 68.0 Embodiment 15 85.0 80.2 Example 16 92.3 96.8 Embodiment 17 86.0 90.3 Embodiment 18 90.0 89.2
[0140] As can be seen from Table 1, the catalyst prepared in the present application does not require the addition of a dechlorination inhibitor in the process of preparing o-chloroaniline by hydrogenation of o-chloronitrobenzene, the catalyst activity is stable, the hydrogenation process conditions are mild, and the dechlorination amount is low.
[0141] In summary, the catalyst preparation method is simple and easy to prepare in batches, and has a multi-level pore structure; the high specific surface area nitrogen-doped carbon catalyst carrier can be evenly dispersed in the precious metal nanoparticles after modification, and the doped nitrogen element in the carrier interacts strongly with the precious metal nanoparticles, which is beneficial to the dispersion of active components while regulating the surface electronic state of the precious metal. Nitrogen regulates the electronic structure of the precious metal active components and inhibits the catalytic hydrogenation dechlorination side reaction.
[0142] The above description is only used to explain the preferred embodiments of the present invention, and is not intended to limit the present invention in any form. Therefore, any modifications or changes made to the present invention under the same inventive spirit should still be included in the scope of protection intended by the present invention.
Claims
1. A method for preparing a porous nitrogen-doped carbon-supported noble metal catalyst, characterized in that: The following steps are involved: Step 1: Add a carbon source and a metal source to distilled water and stir to mix, add an alkaline solution under stirring, continue stirring for 2 to 3 hours after mixing, and then age in an oil bath at 80 to 120° C. for 5 to 8 hours; then add a nitrogen source, continue stirring and aging for 5 to 8 hours, cool to 30 to 50° C. after aging, stir and dry to obtain a carrier precursor; calcine the carrier precursor at 750 to 950° C. under a nitrogen atmosphere, soak it in an acidic liquid after calcination, filter and wash until the upper clear liquid is pH neutral, and dry to obtain a porous nitrogen-doped carbon carrier; Step 2: Immerse the porous nitrogen-doped carbon support obtained in step 1 in a H2O2 aqueous solution or a citric acid aqueous solution for 40 to 50 hours, filter, wash, and dry to obtain a modified porous nitrogen-doped carbon support; Step 3: The modified porous nitrogen-doped carbon support obtained in step 2 is impregnated into an aqueous solution containing at least one of palladium salt, platinum salt and ruthenium salt, and then dried at 100-140° C. to obtain a porous nitrogen-doped carbon-loaded precious metal catalyst.
2. The method for preparing a porous nitrogen-doped carbon-supported noble metal catalyst according to claim 1, characterized in that: The carbon source is at least one of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, gluconic acid and aminotriacetic acid.
3. The method for preparing a porous nitrogen-doped carbon-supported noble metal catalyst according to claim 1, characterized in that: The metal source is at least one of MgCl2, CaCl2 and ZnCl2.
4. The method for preparing a porous nitrogen-doped carbon-supported noble metal catalyst according to claim 1, characterized in that: The nitrogen source is at least one of dicyandiamide and melamine urea.
5. The method for preparing a porous nitrogen-doped carbon-supported noble metal catalyst according to claim 1, characterized in that: The molar ratio of the carbon source to the metal source is 1:1 to 1:4, and the mass ratio of the carbon source to the nitrogen source is 1:0.5 to 1:
2.
6. The method for preparing a porous nitrogen-doped carbon-supported noble metal catalyst according to claim 1, characterized in that: The mass percentage of the H2O2 aqueous solution is 10-15wt%; the mass percentage of the citric acid aqueous solution is 20-25wt%.
7. The method for preparing a porous nitrogen-doped carbon-supported noble metal catalyst according to claim 1, characterized in that: The alkaline solution is a NaOH aqueous solution or a KOH aqueous solution; the acidic liquid is hydrochloric acid or nitric acid.
8. Use of the porous nitrogen-doped carbon-supported noble metal catalyst according to any one of claims 1 to 7 in the synthesis of o-chloroaniline, characterized in that: A porous nitrogen-doped carbon-supported noble metal catalyst is added to an organic solvent containing o-chloronitrobenzene, and reacted with hydrogen at 60° C. to 120° C. and a pressure of 0.2 MPa to 2.0 MPa. After the catalytic reaction is completed, o-chloroaniline is obtained by treatment.
9. The use according to claim 8, characterized in that: The organic solvent is at least one of methanol, ethanol, isopropanol and n-propanol.
10. The use according to claim 8, characterized in that: The mass ratio of the porous nitrogen-doped carbon-supported noble metal catalyst to o-chloronitrobenzene is 1:10 to 1:20.
Citation Information
Patent Citations
Pt-Fe / C catalyst as well as preparation method and application thereof
CN109225258A
Platinum / carbon-bentonite catalyst as well as preparation method and application thereof
CN109331815A
Nitrogen-doped mesoporous carbon supported platinum catalyst as well as preparation method and application thereof
CN113509948A
Cited By
Nitrogen-doped carbon-coated catalyst as well as preparation method and application thereof
CN119733541A
Preparation method of nitrogen-doped juncus roemerianus spherical carbon material
CN121470486A
Preparation method of nitrogen-doped lamp wick grass spherical carbon material
CN121470486B