Preparation method and application of CuS / SnS2 composite heterogeneous negative electrode material

Through the preparation of CuS/SnS2 composite heterostructure, the poor conductivity and volume expansion problems of the negative electrode material of sodium ion battery are solved, the electrochemical performance and cyclic stability are improved, and high capacity and good reversibility are achieved.

CN118978178AActive Publication Date: 2024-11-19HARBIN UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411049809.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The existing sodium ion battery negative electrode materials have poor conductivity and large volume expansion. The first time Coulomb efficiency is low, the sodium ion transmission speed is slow, and CuS is used as the negative electrode of lithium ion battery, resulting in rapid battery capacity due to poor conductivity and severe volume expansion. It is difficult to maintain high specific capacity.

Method used

Using the preparation method of CuS/SnS2 composite heterogeneous anode material, CuS microspheres and SnS2 composite heterogeneous structures are prepared through hydrothermal reactions, and hollowed-shaped heterostructures are constructed to improve the specific surface area and charge transfer paths, and reduce mechanical stress caused by charging and discharging. .

Benefits of technology

It significantly improved the electrochemical performance of sodium ion batteries, with a capacity of 379.5mAhg-1 at 0.1Ag-1, and maintained 281.2mAhg-1 after 350 cycles at high current density, demonstrating good reversibility and cycle stability sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978178A_ABST
    Figure CN118978178A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a CuS / SnS2 composite heterogeneous negative electrode material, and relates to a preparation method and application of a negative electrode material. The invention aims to solve the problems of poor conductivity, large volume expansion, low first coulombic efficiency and slow sodium ion transmission speed of the negative electrode material of the existing sodium ion battery, and the problems of rapid reduction of the capacity of the battery in the first few circles and high cost caused by poor conductivity and serious volume expansion of the CuS material when the CuS material is used as the negative electrode of the lithium ion battery. And finally, the high specific capacity is difficult to maintain. The method comprises the following steps: 1, preparing CuS microspheres; and 2, preparing the CuS / SnS2 composite heterostructure. The CuS / SnS2 composite heterogeneous negative electrode material is used as a sodium ion battery negative electrode material. By constructing the CuS / SnS2 hollow heterostructure, a large specific surface area is provided, ion transmission is more facilitated, and the capacity is improved. The method is simple to operate and suitable for large-scale popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a negative electrode material. Background Art

[0002] Energy is the material basis for the progress of human civilization. With the rapid development of social economy, human society's dependence on energy is increasing. At present, traditional fossil energy such as coal, oil and natural gas provide the main energy for human society. Fossil energy is becoming increasingly exhausted and has a significant impact on the environment. Therefore, changing the existing unreasonable energy structure has become the primary issue facing the sustainable development of human society. At present, the vigorously developed wind energy, solar energy, tidal energy and geothermal energy are all renewable clean energy. However, due to the randomness and intermittency of clean energy, if the electricity generated by it is directly input into the power grid, it will have a great impact on the power grid. Under this situation, the development of efficient and convenient energy storage technology to meet human energy needs has become a research hotspot worldwide. In recent years, secondary batteries such as lithium-ion batteries, aluminum-ion batteries, and sodium-ion batteries (Sodium Ion Batteries, SIBs) have gradually come into people's view. Among them, SIBs are considered to be the most likely energy storage devices to replace LIBs because of their abundant reserves, low cost and similar charging and discharging mechanism to LIBs (because lithium and sodium are both in the first main group and have similar physical and chemical properties).

[0003] At present, sodium-ion battery technology is developing rapidly and has achieved some results, but there are still some problems that need to be solved. Metal sulfides can be used in sodium-ion batteries due to their rich variety, high specific capacity and high specific energy. However, due to a series of problems such as their poor conductivity, large volume expansion, low first coulombic efficiency, and slow sodium ion transmission, it is necessary to systematically carry out structural regulation and mechanism research to further improve their electrochemical performance.

[0004] In recent years, more and more research has been done on copper sulfide (CuS). When CuS is used as the negative electrode of lithium-ion batteries, it is studied because of its high theoretical specific capacity and flat lithium insertion and extraction platform. However, the poor conductivity and severe volume expansion of CuS materials lead to a rapid decrease in the capacity of the battery in the first few cycles, and ultimately it is difficult to maintain a high specific capacity, which is also the main reason hindering its further application. Summary of the invention

[0005] The purpose of the present invention is to solve the problems that the negative electrode materials of existing sodium ion batteries have poor conductivity, large volume expansion, low first coulomb efficiency, slow sodium ion transmission speed, and when CuS is used as the negative electrode of lithium ion batteries, the capacity of the battery drops rapidly in the first few cycles, and it is ultimately difficult to maintain a high specific capacity due to the poor conductivity and severe volume expansion of the CuS material, and to provide a preparation method and application of a CuS / SnS2 composite heterogeneous negative electrode material.

[0006] A method for preparing a CuS / SnS2 composite heterogeneous negative electrode material is specifically completed by the following steps:

[0007] 1. Preparation of CuS microspheres:

[0008] ① Dissolve Cu(NO3)2·3H2O and polyvinyl pyrrolidone in ethylene glycol, then add thiourea and stir to obtain a clear solution;

[0009] ②, placing the clarified solution in a stainless steel reactor lined with polytetrafluoroethylene, and then placing the stainless steel reactor in an oven, hydrothermally reacting at 150°C to 170°C for a period of time, and then naturally cooling to room temperature to obtain reaction product I;

[0010] ③, centrifuging the reaction product I, washing the solid product obtained after centrifugation, and vacuum drying to obtain CuS microspheres;

[0011] 2. Preparation of CuS / SnS2 composite heterostructure:

[0012] ①, add SnCl4·5H2O and thioacetamide to anhydrous ethanol, ultrasonicate for a period of time, then add CuS microspheres, stir to obtain a mixture;

[0013] ②, placing the mixture in a stainless steel reactor lined with polytetrafluoroethylene, and then placing the stainless steel reactor in an oven, hydrothermally reacting at 150°C to 170°C for a period of time, and then naturally cooling to room temperature to obtain reaction product II;

[0014] ③. Centrifuge the reaction product II, wash the solid product obtained after centrifugation, and vacuum dry it to obtain a CuS / SnS2 composite heterogeneous negative electrode material.

[0015] A CuS / SnS2 composite heterogeneous negative electrode material is used as a negative electrode material for a sodium ion battery.

[0016] Principles and beneficial effects of the present invention:

[0017] 1. The present invention effectively shortens the charge transfer path in the battery by designing and constructing a heterogeneous structure, reducing the mechanical stress caused by volume fluctuations caused by repeated charge and discharge. For other transition metal sulfides, Zhao et al. used kapok petal biomass to grow MoS2 nanosheets in situ by a simple one-step hydrothermal method, and further coated the surface with a conductive polypyrrole layer to construct a ternary sandwich structure PC / MoS2@PPy composite electrode, which also alleviated the volume effect of the material during the charge and discharge cycle. -1 Can reach 216.4mAhg -1 The present invention provides a large specific surface area by constructing a CuS / SnS2 hollow heterostructure, which is more conducive to the transmission of ions and improves the capacity; the electrochemical performance is tested and the -1 The capacity can reach 379.5mAhg -1 , at 5A·g -1 After 350 cycles, the current density can reach 281.2 mAh g -1 ; This test result shows that the negative electrode material provided by the present invention still has a considerable capacity even under large current, and the prepared composite material has good reversibility, making it very useful in the research of negative electrode materials for sodium ion batteries and electrode materials in other energy storage fields;

[0018] 2. The present invention provides a method for preparing a CuS / SnS2 composite heterogeneous negative electrode material. The prepared CuS / SnS2 composite heterogeneous negative electrode material is used in sodium ion battery negative electrode materials. The preparation method of the present invention is simple to operate and is suitable for large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 A schematic diagram of the process for preparing the CuS / SnS2 composite heterogeneous negative electrode material according to Example 1;

[0020] Figure 2 are scanning electron microscope images, in which ab is a scanning electron microscope image of the CuS microspheres prepared in step 1 of Example 1, cd is a scanning electron microscope image of the CuS / SnS2 composite heterogeneous negative electrode material prepared in step 2 of Example 2, and ef is a scanning electron microscope image of the CuS / SnS2 electrode grown on carbon cloth prepared in comparative example 1;

[0021] Figure 3 XRD spectra of CuS microspheres, SnS2, CuS / SnS2=2:1, CuS / SnS2=3:1, and CuS / SnS2=5:1 prepared in step 1 of Example 1;

[0022] Figure 4The Raman spectra of CuS microspheres, SnS2, CuS / SnS2=2:1, CuS / SnS2=3:1, and CuS / SnS2=5:1 prepared in step 1 of Example 1;

[0023] Figure 5 The CuS microspheres prepared in step 1 of Example 1, SnS2, CC / CuS / SnS2, CuS / SnS2=2:1, CuS / SnS2=3:1, and CuS / SnS2=5:1 prepared in Comparative Example 1 were heated to a current density of 0.1A g -1 Cycle performance under

[0024] Figure 6 CuS / SnS2=3:1 at 5A g -1 Cycle performance under

[0025] Figure 7 These are the magnification diagrams of the CuS microspheres, SnS2, CuS / SnS2=2:1, CuS / SnS2=3:1, and CuS / SnS2=5:1 prepared in step 1 of Example 1. DETAILED DESCRIPTION

[0026] Specific implementation method 1: This implementation method is a method for preparing a CuS / SnS2 composite heterogeneous negative electrode material, which is specifically completed by the following steps:

[0027] 1. Preparation of CuS microspheres:

[0028] ① Dissolve Cu(NO3)2·3H2O and polyvinyl pyrrolidone in ethylene glycol, then add thiourea and stir to obtain a clear solution;

[0029] ②, placing the clarified solution in a stainless steel reactor lined with polytetrafluoroethylene, and then placing the stainless steel reactor in an oven, hydrothermally reacting at 150°C to 170°C for a period of time, and then naturally cooling to room temperature to obtain reaction product I;

[0030] ③, centrifuging the reaction product I, washing the solid product obtained after centrifugation, and vacuum drying to obtain CuS microspheres;

[0031] 2. Preparation of CuS / SnS2 composite heterostructure:

[0032] ①, add SnCl4·5H2O and thioacetamide to anhydrous ethanol, ultrasonicate for a period of time, then add CuS microspheres, stir to obtain a mixture;

[0033] ②, placing the mixture in a stainless steel reactor lined with polytetrafluoroethylene, and then placing the stainless steel reactor in an oven, hydrothermally reacting at 150°C to 170°C for a period of time, and then naturally cooling to room temperature to obtain reaction product II;

[0034] ③. Centrifuge the reaction product II, wash the solid product obtained after centrifugation, and vacuum dry it to obtain a CuS / SnS2 composite heterogeneous negative electrode material.

[0035] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: the volume ratio of the amount of Cu(NO3)2·3H2O described in step 1① to ethylene glycol is (2mmol-4mmol):60mL; the volume ratio of the mass of polyvinyl pyrrolidone described in step 1① to ethylene glycol is (0.3g-1g):60mL. The other steps are the same as those in specific embodiment 1.

[0036] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the volume ratio of the amount of thiourea and ethylene glycol described in step 1① is (7mmol-11mmol):60mL. The other steps are the same as those of specific embodiment 1 or 2.

[0037] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the time of the hydrothermal reaction in step 1② is 10 h to 14 h. The other steps are the same as those of specific embodiments 1 to 3.

[0038] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: the centrifugal speed in step 1 ③ is 10000 rpm, and the centrifugal time is 5 min to 9 min; in step 1 ③, the solid product obtained after centrifugation is first washed 3 to 5 times with anhydrous ethanol, and then washed 3 to 5 times with deionized water; the vacuum drying temperature in step 1 ③ is 60°C to 80°C, and the vacuum drying time is 8h to 12h. The other steps are the same as those in specific embodiments 1 to 4.

[0039] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the molar ratio of CuS microspheres to SnCl4·5H2O in step 2① is (2 to 5):1; the molar ratio of thioacetamide to SnCl4·5H2O in step 2① is (3 to 5):1. The other steps are the same as those in specific embodiments 1 to 5.

[0040] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the volume ratio of the amount of the CuS microspheres described in step 2① to anhydrous ethanol is (2mol~5mol):(30mL~50mL); the ultrasonic time described in step 2① is 20min~40min; the stirring time described in step 2① is 10min~20min. The other steps are the same as specific embodiments 1 to 6.

[0041] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that: the time of the hydrothermal reaction in step 2 ② is 10h to 14h; the speed of the centrifugation in step 2 ③ is 10000rpm, and the time of the centrifugation is 5min to 9min. The other steps are the same as those in specific embodiments 1 to 7.

[0042] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: in step 2 ③, the solid product obtained after centrifugation is first washed 3 to 5 times with anhydrous ethanol, and then washed 3 to 5 times with deionized water; the vacuum drying temperature in step 2 ③ is 60°C to 80°C, and the vacuum drying time is 8h to 12h. The other steps are the same as those in specific embodiments 1 to 8.

[0043] Specific embodiment ten: This embodiment is a CuS / SnS2 composite heterogeneous negative electrode material used as a negative electrode material for a sodium ion battery.

[0044] The following examples are used to verify the beneficial effects of the present invention:

[0045] Example 1: A method for preparing a CuS / SnS2 composite heterogeneous negative electrode material is specifically completed by the following steps:

[0046] 1. Preparation of CuS microspheres:

[0047] ① Dissolve 3mmol Cu(NO3)2·3H2O and 0.5g polyvinylpyrrolidone in 60mL ethylene glycol, then add 9mmol thiourea and stir to obtain a clear solution;

[0048] ②, place the clarified solution in a stainless steel reactor lined with polytetrafluoroethylene, then place the stainless steel reactor in an oven, perform hydrothermal reaction at 160°C for 12 hours, and then naturally cool to room temperature to obtain reaction product I;

[0049] ③, centrifuging the reaction product I, then washing the solid product obtained after centrifugation with anhydrous ethanol for 5 times, and then washing the solid product obtained after centrifugation with deionized water for 5 times; finally, vacuum drying at 60°C for 10 hours to obtain CuS microspheres;

[0050] The centrifugal speed in step 1 (3) is 10000 rpm and the centrifugal time is 7 min;

[0051] 2. Preparation of CuS / SnS2 composite heterostructure:

[0052] ①, SnCl4·5H2O and thioacetamide were added to anhydrous ethanol, ultrasonicated for 30 min, and then CuS microspheres were added and stirred for 10 min to obtain a mixture;

[0053] The molar ratio of CuS microspheres to SnCl4·5H2O described in step 2① is 2:1;

[0054] The molar ratio of thioacetamide to SnCl4·5H2O described in step 2① is 4:1;

[0055] The volume ratio of the amount of the CuS microspheres described in step 2① to anhydrous ethanol is 2 mol:40 mL;

[0056] ②, placing the mixture in a stainless steel reactor lined with polytetrafluoroethylene, and then placing the stainless steel reactor in an oven, hydrothermally reacting at 160°C for 12 hours, and then naturally cooling to room temperature to obtain reaction product II;

[0057] ③, centrifuging the reaction product II, then washing the solid product obtained after centrifugation with anhydrous ethanol for 5 times, then washing the solid product obtained after centrifugation with deionized water for 5 times, and finally vacuum drying at 60°C for 10h to obtain a CuS / SnS2 composite heterogeneous negative electrode material (CuS / SnS2=2:1);

[0058] The centrifugal speed described in step 2③ is 10000 rpm and the centrifugal time is 7 min.

[0059] Example 2: The difference between this example and Example 1 is that the molar ratio of CuS microspheres to SnCl4·5H2O in step 2① is 3:1; and step 2③ obtains CuS / SnS2 composite heterogeneous negative electrode material (CuS / SnS2=3:1). The other steps and parameters are the same as those in Example 1.

[0060] Example 3: The difference between this example and Example 1 is that the molar ratio of CuS microspheres to SnCl4·5H2O in step 2① is 5:1; and in step 2③, a CuS / SnS2 composite heterogeneous negative electrode material (CuS / SnS2=5:1) is obtained. The other steps and parameters are the same as those in Example 1.

[0061] Comparative Example 1: A method for preparing an electrode of CuS / SnS2 grown on carbon cloth is specifically completed in the following steps:

[0062] 1. Preparation of CuS microspheres:

[0063] ① Dissolve 3mmol Cu(NO3)2·3H2O and 0.5g polyvinylpyrrolidone in 60mL ethylene glycol, then add 9mmol thiourea and stir to obtain a clear solution;

[0064] ②, place the clarified solution in a stainless steel reactor lined with polytetrafluoroethylene, then place the stainless steel reactor in an oven, perform hydrothermal reaction at 160°C for 12 hours, and then naturally cool to room temperature to obtain reaction product I;

[0065] ③, centrifuging the reaction product I, then washing the solid product obtained after centrifugation with anhydrous ethanol for 5 times, and then washing the solid product obtained after centrifugation with deionized water for 5 times; finally, vacuum drying at 60°C for 10 hours to obtain CuS microspheres;

[0066] The centrifugal speed in step 1 (3) is 10000 rpm and the centrifugal time is 7 min;

[0067] 2. Put CuS microspheres, carbon cloth, SnCl4·5H2O, thioacetamide and anhydrous ethanol into a stainless steel reactor for hydrothermal synthesis, heat at 160°C for 12h, wait for it to cool naturally after the hydrothermal process, wash it with anhydrous ethanol and deionized water for 5 times respectively, and then vacuum dry it at 60°C for 10h to obtain CuS / SnS2 electrodes vertically grown on carbon cloth (CC / CuS / SnS2);

[0068] The molar ratio of the CuS microspheres to SnCl4·5H2O is 2:1;

[0069] The molar ratio of thioacetamide to SnCl4·5H2O is 4:1;

[0070] The volume ratio of the amount of the CuS microspheres to anhydrous ethanol is 2 mol:40 mL.

[0071] Figure 2 are scanning electron microscope images, in which ab is a scanning electron microscope image of the CuS microspheres prepared in step 1 of Example 1, cd is a scanning electron microscope image of the CuS / SnS2 composite heterogeneous negative electrode material prepared in step 2 of Example 2, and ef is a scanning electron microscope image of the CuS / SnS2 electrode grown on carbon cloth prepared in comparative example 1;

[0072] from Figure 2 It can be seen that: during the composite process, the CuS / SnS2 composite heterostructure is gradually transformed into a hollow sheet, the gaps between the nanosheets are gradually connected, and the thickness of the sheet becomes thinner. This morphology greatly increases the specific surface area of ​​the entire structure and will provide more sodium ion attachment sites, allowing the material to maintain a more stable structure, which helps to stabilize the structure of the material and is beneficial to maintaining the cycle stability of the electrode material.

[0073] Figure 3XRD spectra of CuS microspheres, SnS2, CuS / SnS2=2:1, CuS / SnS2=3:1, and CuS / SnS2=5:1 prepared in step 1 of Example 1;

[0074] from Figure 3 It can be seen that the main diffraction peaks of the CuS / SnS2=3:1 composite heterogeneous electrode material can all correspond to the standard spectrum of CuS. Compared with the results of pure CuS microspheres, the intensity of each diffraction peak of the CuS / SnS2=3:1 sample prepared in Example 2 is significantly reduced, and the half-peak width is also widened.

[0075] Figure 4 The Raman spectra of CuS microspheres, SnS2, CuS / SnS2=2:1, CuS / SnS2=3:1, and CuS / SnS2=5:1 prepared in step 1 of Example 1;

[0076] from Figure 4 It can be seen that the Raman spectrum of the CuS / SnS2=3:1 composite heterogeneous electrode material prepared in Example 2 is at 461 cm -1 The characteristic peak of Cu-S bond in copper sulfide is shown at 314 cm -1 There is a strong peak at the SnS2, which is the S stretching vibration (A 1g mode). Raman test results confirmed the existence of CuS / SnS2 in the composite heterostructure.

[0077] Figure 5 The CuS microspheres prepared in step 1 of Example 1, SnS2, CC / CuS / SnS2, CuS / SnS2=2:1, CuS / SnS2=3:1, and CuS / SnS2=5:1 prepared in Comparative Example 1 were heated to a current density of 0.1A g -1 Cycle performance under

[0078] Figure 5 The test results show that the discharge capacity of the composite heterogeneous electrode material with CuS / SnS2=3:1 prepared in Example 2 reaches the highest, and the first discharge capacity of the pure CuS electrode is 423.7 mAh g -1 and 565.5mAh g -1 The results show that the cycle performance is significantly improved after modification. The discharge capacity of the composite heteroelectrode of CuS / SnS2=3:1 can reach 376.1 mAh g after 50 cycles. -1 By comparison, it can be found that the initial capacity of the CC / CuS / SnS2 heterogeneous electrode material prepared in Comparative Example 1 is 325.8 mAhg -1 After 50 cycles, the capacity is 55.5 mAh g -1The above test results show that the formation of the CuS / SnS2=3:1 heterostructure prepared in Example 2 enhances its reaction kinetics, thereby greatly improving the rate performance of the electrode.

[0079] Figure 6 CuS / SnS2=3:1 at 5A g -1 Cycle performance under

[0080] Figure 6 The CuS / SnS2=3:1 composite heterogeneous electrode material prepared in Example 2 is 5Ag -1 Cyclic performance test under high current density, after 350 cycles, it can still maintain 281.2mAhg -1 The discharge specific capacity (the first 30 cycles are activation cycles) and the capacity decay rate is low.

[0081] Figure 7 The magnification diagrams are of CuS microspheres, SnS2, CuS / SnS2=2:1, CuS / SnS2=3:1, and CuS / SnS2=5:1 prepared in step 1 of Example 1;

[0082] from Figure 7 It can be seen that the composite material of CuS / SnS2=3:1 has a -1 Still has 281.8mAh g -1 The discharge capacity is restored to 100 mA g -1 The capacity can reach 379.5mAh g -1 This test result shows that the prepared composite material has good reversibility.

Claims

1. A method for preparing a CuS / SnS2 composite heterogeneous negative electrode material, characterized in that The preparation method is specifically completed according to the following steps:

1. Preparation of CuS microspheres: ① Dissolve Cu(NO3)2·3H2O and polyvinyl pyrrolidone in ethylene glycol, then add thiourea and stir to obtain a clear solution; ②, placing the clarified solution in a stainless steel reactor lined with polytetrafluoroethylene, and then placing the stainless steel reactor in an oven, hydrothermally reacting at 150°C to 170°C for a period of time, and then naturally cooling to room temperature to obtain reaction product I; ③, centrifuging the reaction product I, washing the solid product obtained after centrifugation, and vacuum drying to obtain CuS microspheres; 2. Preparation of CuS / SnS2 composite heterostructure: ①, add SnCl4·5H2O and thioacetamide to anhydrous ethanol, ultrasonicate for a period of time, then add CuS microspheres, stir to obtain a mixture; ②, placing the mixture in a stainless steel reactor lined with polytetrafluoroethylene, and then placing the stainless steel reactor in an oven, hydrothermally reacting at 150°C to 170°C for a period of time, and then naturally cooling to room temperature to obtain reaction product II; ③. Centrifuge the reaction product II, wash the solid product obtained after centrifugation, and vacuum dry it to obtain a CuS / SnS2 composite heterogeneous negative electrode material.

2. The method for preparing a CuS / SnS2 composite heterogeneous negative electrode material according to claim 1, characterized in that The volume ratio of the amount of Cu(NO3)2·3H2O described in step 1① to ethylene glycol is (2mmol~4mmol):60mL; the volume ratio of the mass of polyvinyl pyrrolidone described in step 1① to ethylene glycol is (0.3g~1g):60mL.

3. The method for preparing a CuS / SnS2 composite heterogeneous negative electrode material according to claim 1, characterized in that The volume ratio of the amount of thiourea described in step 1① to ethylene glycol is (7mmol~11mmol):60mL.

4. The method for preparing a CuS / SnS2 composite heterogeneous negative electrode material according to claim 1, characterized in that The time of the hydrothermal reaction described in step 1② is 10h to 14h.

5. The method for preparing a CuS / SnS2 composite heterogeneous negative electrode material according to claim 1, characterized in that The centrifugal speed described in step 1③ is 10000rpm, and the centrifugal time is 5min~9min; in step 1③, the solid product obtained after centrifugation is first washed 3 times to 5 times with anhydrous ethanol, and then the solid product obtained after centrifugation is washed 3 times to 5 times with deionized water; the vacuum drying temperature described in step 1③ is 60℃~80℃, and the vacuum drying time is 8h~12h.

6. The method for preparing a CuS / SnS2 composite heterogeneous negative electrode material according to claim 1, characterized in that The molar ratio of the CuS microspheres to SnCl4·5H2O in step 2① is (2-5):1; the molar ratio of the thioacetamide to SnCl4·5H2O in step 2① is (3-5):

1.

7. The method for preparing a CuS / SnS2 composite heterogeneous negative electrode material according to claim 1, characterized in that The volume ratio of the amount of CuS microspheres described in step 2① to anhydrous ethanol is (2mol~5mol):(30mL~50mL); the ultrasonic time described in step 2① is 20min~40min; the stirring time described in step 2① is 10min~20min.

8. The method for preparing a CuS / SnS2 composite heterogeneous negative electrode material according to claim 1, characterized in that The time of the hydrothermal reaction described in step 2② is 10h to 14h; the speed of the centrifugation described in step 2③ is 10000rpm, and the time of the centrifugation is 5min to 9min.

9. The method for preparing a CuS / SnS2 composite heterogeneous negative electrode material according to claim 1, characterized in that In step 2③, the solid product obtained after centrifugation is first washed 3 to 5 times with anhydrous ethanol, and then washed 3 to 5 times with deionized water; the vacuum drying temperature described in step 2③ is 60°C to 80°C, and the vacuum drying time is 8h to 12h.

10. Application of a CuS / SnS2 composite heterogeneous negative electrode material prepared by the preparation method according to claim 1, characterized in that A CuS / SnS2 composite heterogeneous negative electrode material is used as a negative electrode material for a sodium ion battery.

Citation Information

Patent Citations

  • Preparation method of interlayer spacing and pore volume adjustable layered copper sulfide microsphere material for sodium ion battery

    CN108423705A

  • Electrode material for negative electrode of lithium ion battery and preparation method of electrode material

    CN114242964A

  • Heterostructure composite material and preparation method and application thereof

    CN114620780A

  • Preparation method and application of iron selenide / molybdenum selenide heterostructure electrode material

    CN115911286A

  • Preparation of heterojunction-containing sulfide composite negative electrode of sodium battery

    CN117393715A