High-corrosion-resistance all-solid-waste-based maritime work cementing material as well as preparation method and application thereof

Through the coordinated preparation of high-speed iron phase precursor gelling materials and solid waste-based magnesium phosphate cementitious materials, the problems of low solid waste utilization rate and poor seawater corrosion resistance are solved, and high corrosion resistance and Low-cost marine gelling materials are suitable for marine engineering and reduce environmental pollution.

CN118978383AActive Publication Date: 2024-11-19SHANDONG HI SPEED GRP CO LTD +1

Patent Information

Application Number
CN202411071439.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The solid waste utilization rate of existing solid waste-based gelling materials is low and have poor resistance to seawater erosion, making it difficult to meet the durability needs of offshore materials in seawater environments.

Method used

The high-speed iron phase precursor gelling material and solid waste-based magnesium phosphate cement materials are used to prepare high-speed iron phase precursor precursor by the mixed calcination of calcium-based solid waste, silicon-based solid waste, aluminum-based solid waste and iron-based solid waste. The bulk gelling material is mixed with solid waste-based magnesium phosphate cement material in proportion, and a water reducer is added to prepare high corrosion-resistant all solid waste-based offshore gelling material.

Benefits of technology

It has achieved high resistance to seawater erosion, low cost and high solid waste utilization rate, meets the needs of marine engineering, and reduces pollution to the ecological environment and provides economic and scientific value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004980994490000051
    Figure BDA0004980994490000051
  • Figure BDA0004980994490000061
    Figure BDA0004980994490000061
  • Figure BDA0004980994490000111
    Figure BDA0004980994490000111
Patent Text Reader

Abstract

The invention discloses a high-corrosion-resistance all-solid-waste-based maritime work cementing material as well as a preparation method and application thereof, and belongs to the technical field of preparation of maritime work cementing materials. The high-corrosion-resistance all-solid-waste-based marine engineering cementing material provided by the invention is prepared from 40 to 50 parts of a high-iron-phase precursor cementing material, 35 to 45 parts of a solid-waste-based magnesium phosphate cement material, 2 to 4 parts of a water reducing agent and 30 to 50 parts of water, the high-iron-phase precursor cementing material is obtained by calcining a mixture of calcium-based solid waste, silicon-based solid waste, aluminum-based solid waste and iron-based solid waste; the solid waste-based magnesium phosphate cement material comprises 15-25 parts of calcium-based solid waste, 35-40 parts of iron-based solid waste, 30-40 parts of over-burnt magnesia powder, 20-25 parts of monopotassium phosphate and 5-8 parts of a retarder. The high-corrosion-resistance all-solid-waste-based maritime work cementing material has the advantages of being short in setting time, high in mechanical strength, high in corrosion and erosion resistance and low in price, and has considerable economic value, engineering value and ecological benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of preparation of marine engineering cementitious materials, and in particular to a highly corrosion-resistant all-solid waste-based marine engineering cementitious material and a preparation method thereof. Background Art

[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Marine engineering materials are exposed to erosion and scouring by seawater during their service, and the durability of marine engineering concrete has always been highly valued. In the existing technology, a large amount of sulphoaluminate cement and organic admixtures are used to improve the material's anti-erosion ability; or the problem of poor anti-abrasion ability of marine engineering concrete is solved by adding double-ash cement powder; there are also existing technologies that use high-iron phosphate aluminate cement clinker as the main material and add auxiliary cementitious materials to improve the resistance to chloride ion corrosion and sulfate corrosion; or add some solid waste to silicate cement clinker and aluminate cement clinker, and improve the comprehensive performance of marine engineering concrete through reasonable particle size grading to alleviate corrosion. However, the above methods all use cement as the main material, which is relatively expensive.

[0004] At present, some research has been conducted on the comprehensive utilization of solid waste to realize its resource utilization. For example, a large amount of slag and a small amount of fly ash are added to the silicate cement clinker to improve the resistance to seawater erosion; there are also existing technologies that use waste slag as the main raw material, and add fly ash and tailings to prepare materials with economic and environmental benefits. However, the solid waste utilization rate of existing solid waste-based cementitious materials is relatively low, and solid waste-based cementitious materials with higher solid waste utilization rates have poor resistance to seawater erosion. Therefore, how to provide a fully solid waste-based marine engineering cementitious material with high resistance to seawater erosion is an urgent problem to be solved. Summary of the invention

[0005] In view of this, the present invention provides a highly corrosion-resistant all-solid waste-based marine engineering cementitious material and a preparation method and application thereof, which solves the problems of low solid waste utilization rate or poor resistance to seawater erosion of existing solid waste-based cementitious materials.

[0006] In a first aspect, the present invention provides a highly corrosion-resistant all-solid waste-based marine engineering cementitious material, comprising 40 to 50 parts of a high-iron phase precursor cementitious material, 35 to 45 parts of a solid waste-based magnesium phosphate cement material, 2 to 4 parts of a water reducer and 30 to 50 parts of water;

[0007] The high iron phase precursor gelling material is obtained by calcining a mixture of calcium-based solid waste, silicon-based solid waste, aluminum-based solid waste and iron-based solid waste; the limestone saturation coefficient of the mixture is 0.87-0.96, the silicon ratio is 1.7-2.7, and the aluminum ratio is 0.9-1.9;

[0008] The solid waste-based magnesium phosphate cement material comprises 15 to 25 parts of calcium-based solid waste, 35 to 40 parts of iron-based solid waste, 30 to 40 parts of overburned magnesium oxide powder, 20 to 25 parts of potassium dihydrogen phosphate and 5 to 8 parts of retarder.

[0009] Preferably, the calcium-based solid waste of the high iron phase precursor cementitious material and the solid waste-based magnesium phosphate cement material is selected from one or more of carbide slag, blast furnace slag, fly ash, limestone tailings or shell powder, and has a specific surface area of ​​300 to 450 m 2 / kg.

[0010] Preferably, the iron-based solid waste of the high iron phase precursor cementitious material and the solid waste-based magnesium phosphate cement material is selected from one or more of red mud, steel slag, steelmaking dust mud or grinding wheel mud, and has a specific surface area of ​​300 to 450 m 2 / kg.

[0011] Preferably, the silicon-based solid waste is selected from one or more of coal gangue, silica fume or waste glass, and has a specific surface area of ​​300 to 450 m 2 / kg.

[0012] Preferably, the aluminum-based solid waste is selected from one or more of aluminum ash, red mud, waste aluminum foil or aluminum tailings, and has a specific surface area of ​​300 to 450 m 2 / kg.

[0013] Preferably, the retarder is selected from one or more of borax, malic acid, urea, lignosulfonic acid or triethanolamine.

[0014] Preferably, the water reducer is selected from one or more of a naphthalene-based water reducer, a fatty acid-based water reducer or an aminosulfonate-based water reducer.

[0015] Preferably, the mineral components of the high iron phase precursor gelling material include 35 to 40 parts of CaO, 20 to 23 parts of SiO2, 20 to 30 parts of Al2O3, and 25 to 35 parts of Fe2O3.

[0016] In a second aspect, the present invention provides a method for preparing the above-mentioned highly corrosion-resistant all-solid waste-based marine engineering cementitious material, comprising the following steps:

[0017] Calcium-based solid waste, silicon-based solid waste, aluminum-based solid waste and iron-based solid waste are mixed, and then calcined to obtain a high-iron phase precursor gelling material;

[0018] Mixing calcium-based solid waste, iron-based solid waste, overburned magnesium oxide powder, potassium dihydrogen phosphate and a retarder to obtain a solid waste-based magnesium phosphate cement material;

[0019] Mixing high iron phase precursor cementitious material and solid waste-based magnesium phosphate cement material in proportion to obtain a dry mix;

[0020] Dissolve the water reducing agent in water to obtain an admixture solution;

[0021] Add the admixture solution into the dry mix and stir evenly to obtain the product.

[0022] Preferably, the calcination temperature is 1300-1400° C., the heating rate is controlled at 5-10° C. / min, and the calcination time is 3-4.5 h.

[0023] In a third aspect, the present invention provides the use of the above-mentioned highly corrosion-resistant all-solid waste-based marine engineering cementitious material or the highly corrosion-resistant all-solid waste-based marine engineering cementitious material prepared by the above-mentioned preparation method in the field of marine engineering grouting materials.

[0024] Compared with the prior art, the present invention has achieved the following beneficial effects:

[0025] (1) The highly corrosion-resistant all-solid waste-based marine engineering cementitious material of the present invention is prepared by synergistically using a solid waste-based magnesium phosphate cement material with high early strength and controllable setting time and a high-iron phase precursor cementitious material with high late strength and excellent corrosion resistance. It has the advantages of short setting time, high mechanical strength, strong resistance to dissolution and erosion, and low price. It meets the needs of marine engineering construction and has considerable economic and engineering value.

[0026] (2) The present invention not only consumes a large amount of solid waste and realizes the resource utilization of solid waste, but also solves the problem of large amounts of solid waste storage occupying arable land, reduces the pollution and damage to the ecological environment including soil and groundwater, and avoids the use of traditional cement, with lower costs and good scientific value and ecological benefits. DETAILED DESCRIPTION

[0027] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0028] The present invention provides a highly corrosion-resistant all-solid waste-based marine engineering cementitious material, comprising 40 to 50 parts of a high-iron phase precursor cementitious material, 35 to 45 parts of a solid waste-based magnesium phosphate cement material, 2 to 4 parts of a water reducer and 30 to 50 parts of water;

[0029] The high iron phase precursor gelling material is obtained by calcining a mixture of calcium-based solid waste, silicon-based solid waste, aluminum-based solid waste and iron-based solid waste; the limestone saturation coefficient of the mixture is 0.87-0.96, the silicon ratio is 1.7-2.7, and the aluminum ratio is 0.9-1.9;

[0030] The solid waste-based magnesium phosphate cement material comprises 15 to 25 parts of calcium-based solid waste, 35 to 40 parts of iron-based solid waste, 30 to 40 parts of overburned magnesium oxide powder, 20 to 25 parts of potassium dihydrogen phosphate and 5 to 8 parts of retarder.

[0031] In the present invention, a highly corrosion-resistant high-iron phase precursor cementitious material and a solid waste-based magnesium phosphate cement material with high early strength performance are developed in a balanced manner, wherein the hydration product gel of the high-iron phase precursor cementitious material can adsorb corrosive ions, has a small microstructure porosity, is difficult for seawater to penetrate, and can effectively block the diffusion of chloride ions and other corrosive ions; the solid waste-based magnesium phosphate cement material hydrates and coagulates quickly, can improve the pore structure, increase the density, can contribute to early strength, make up for the problem of low early strength of the high-iron phase precursor cementitious material, and further enhance the corrosion resistance.

[0032] The present invention makes full use of various solid wastes, and has excellent properties such as better corrosion resistance compared to traditional cement and cementitious materials using materials such as fly ash. At the same time, compared with the existing technical solutions for preparing cementitious materials using solid waste, the present invention has a higher utilization rate of solid waste and better effects, and has the characteristics of full resource utilization of solid waste and environmental protection.

[0033] The combination of various solid waste components in the high-iron phase precursor cementitious material of the cementitious material of the present invention realizes the control of the content of the main components CaO, SiO2, Al2O3, and Fe2O3 within a certain range. Each main component affects the rate value design of the high-iron phase precursor cementitious material (limestone saturation coefficient, silicon rate, aluminum rate). The silicon and calcium contents affect the strength contribution of the high-iron phase precursor cementitious material. The aluminum and iron contents affect the high-iron phase precursor cementitious material's resistance to ion erosion and scouring, and affect the coagulation time.

[0034] In the present invention, the limestone saturation coefficient (KH) of the raw material of the high iron phase precursor cementitious material (i.e., calcium-based solid waste, silicon-based solid waste, aluminum-based solid waste and iron-based solid waste material before calcination) is in the range of 0.87 to 0.96, the silicon ratio (SM) is in the range of 1.7 to 2.7, and the aluminum ratio (IM) is in the range of 0.9 to 1.9. The chemical composition of the raw material is calculated by setting key parameters (KH, SM, IM), and then the theoretical mineral composition of the high iron phase precursor cementitious material is calculated by chemical method, and the calculation formula is shown in formulas (1) to (11):

[0035]

[0036]

[0037] Among them, ∑ is taken as 97.5%, w CaO , Respectively represent the mass percentage of CaO, SiO2, Al2O3, and Fe2O3; They represent the mass percentages of tricalcium silicate, dicalcium silicate, tricalcium aluminate and tetracalcium aluminoferrite respectively.

[0038] The limestone saturation coefficient (KH) indicates the degree to which the silicon dioxide in the high iron phase precursor cementitious material is saturated with calcium oxide to form tricalcium silicate. When the KH value is greater than 1, there will be free calcium oxide in the precursor; when the KH value is close to 1, there is too much free calcium oxide in the mineral system, resulting in poor volume stability of the precursor and decreased performance of the precursor. In order to make the precursor mineral composition reach the theoretical set value and control the content of free calcium oxide at the same time, the KH value is controlled between 0.87 and 0.96.

[0039] The silicon ratio (SM) reflects the relative content of silicate minerals (C3S, C2S) and flux minerals (C3A, C4AF) in the high-iron phase precursor cementitious material. If the SM value is too high, there will be more silicate minerals and less flux minerals, which is beneficial to the strength of the precursor, but it is difficult to achieve with the existing synthesis process; if the SM value is too low, there are too many flux minerals in the precursor, and it is easy to form large lumps and rings during calcination, and it is easy to cause the strength of the precursor to be too low. Therefore, the SM value is controlled between 1.7 and 2.7.

[0040] The aluminum ratio (IM) reflects the relative mass fraction of C3A and C4AF in the high iron phase precursor cementitious material. When the IM value is too high, the C3A content is too high, the C4AF content is relatively low, the liquid phase viscosity increases, which is not conducive to the formation of C3S, and excessive C3A content will cause rapid solidification of the material; when the IM value is too low, the relative mass fraction of C3A is small, the C4AF content is high, the liquid phase viscosity is small, which is conducive to the formation of C3S, but it is easy to cause large lumps in the kiln. Therefore, 0.9 to 1.9 is selected as the control parameter of the IM value.

[0041] In the present invention, the calcium-based solid waste of the high iron phase precursor cementitious material and the solid waste-based magnesium phosphate cement material is selected from one or more of carbide slag, blast furnace slag, fly ash, limestone tailings or shell powder, and the specific surface area is 300-450m 2 The iron-based solid waste of the high iron phase precursor cementitious material and the solid waste-based magnesium phosphate cement material is selected from one or more of red mud, steel slag, steelmaking dust mud or grinding wheel mud, and has a specific surface area of ​​300-450m 2 / kg.

[0042] In the present invention, the silicon-based solid waste is selected from one or more of coal gangue, silica fume or waste glass, and has a specific surface area of ​​300 to 450 m 2 The aluminum-based solid waste is selected from one or more of aluminum ash, red mud, waste aluminum foil or aluminum tailings, and has a specific surface area of ​​300 to 450 m 2 / kg.

[0043] In the present invention, the retarder is selected from one or more of borax, malic acid, urea, lignosulfonic acid or triethanolamine. The retarder can slow down the coagulation and hardening of the cementitious material, and avoid the inconvenience of construction caused by too fast coagulation rate.

[0044] In the present invention, the water reducer is selected from one or more of naphthalene water reducer, fatty acid water reducer or aminosulfonate water reducer. The water reducer is combined with the high iron phase precursor gelling material to adjust the stability of the setting time, early strength and late strength within a certain range.

[0045] The present invention also provides a method for preparing the above-mentioned highly corrosion-resistant all-solid waste-based marine engineering cementitious material, comprising the following steps:

[0046] Calcium-based solid waste, silicon-based solid waste, aluminum-based solid waste and iron-based solid waste are mixed, and then calcined to obtain a high-iron phase precursor gelling material;

[0047] Mixing calcium-based solid waste, iron-based solid waste, overburned magnesium oxide powder, potassium dihydrogen phosphate and a retarder to obtain a solid waste-based magnesium phosphate cement material;

[0048] Mixing high iron phase precursor cementitious material and solid waste-based magnesium phosphate cement material in proportion to obtain a dry mix;

[0049] Dissolve the water reducing agent in water to obtain an admixture solution;

[0050] Add the admixture solution into the dry mix and stir evenly to obtain the product.

[0051] In the present invention, before calcium-based solid waste, silicon-based solid waste, aluminum-based solid waste and iron-based solid waste are mixed and calcined, each solid waste raw material needs to be dried to make the moisture content of each solid waste raw material less than 25%, so as to avoid the influence of moisture on the overall structure formed by the combination of various raw materials during the calcination process. In addition, each solid waste raw material is preferably ground and sieved before calcination, and the size of the sieve is 50 to 150 mesh, more preferably 100 mesh. Sieving before calcination can improve the uniformity of calcination.

[0052] In the present invention, the calcination temperature is 1300-1400°C, more preferably 1300-1360°C; the heating rate is controlled to be 5-10°C / min, and the calcination time is 3-4.5h. High temperature calcination can promote chemical reactions between raw material molecules to form new substances, such as silicate minerals and ferroaluminate minerals, which have an important influence on the mechanical properties and corrosion resistance of the high iron phase precursor cementitious material.

[0053] After the calcination is completed, the present invention further comprises a cooling step, which specifically comprises: first water cooling and then natural cooling, water cooling for 5 to 15 minutes and then natural cooling for 2 to 4 hours; more preferably, water cooling for 5 to 10 minutes and then natural cooling for 2 to 3 hours.

[0054] In the present invention, after cooling to obtain the calcined product, the process further comprises the steps of crushing, grinding and sieving, wherein the sieve has a size of 150 to 250 mesh, preferably 200 mesh. Particles with uniform particle size are beneficial to the subsequent mixing and hydration process.

[0055] In the present invention, the specific surface area of ​​the dry mixture of the high iron phase precursor cementitious material and the solid waste-based magnesium phosphate cement material is 350 to 450 m 2 / kg, more preferably 380 to 420 m 2 / kg.

[0056] The present invention also provides the application of the above-mentioned highly corrosion-resistant all-solid waste-based marine engineering cementitious material in the field of marine engineering grouting materials.

[0057] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0058] Example 1

[0059] (1) Red mud, carbide slag, silica fume, limestone tailings and aluminum ash are dried to a moisture content of no more than 25% and passed through a 100-mesh sieve; various dried materials are mixed, based on solid mass, to obtain a mixture of 40 g red mud, 30 g carbide slag, 10 g silica fume, 15 g limestone tailings and 5 g aluminum ash; the mixture has a limestone saturation coefficient (KH) of 0.89, a silicon content (SM) of 1.74 and an aluminum content (IM) of 0.93.

[0060] (2) The mixture was heated to 1300°C at a heating rate of 10°C / min and calcined at high temperature for 3.16 hours. The calcined product was first water-cooled for 5 minutes and then naturally cooled for 2 hours. The cooled calcined product was crushed, ground, and sieved through a 200-mesh sieve to obtain a high-iron phase precursor gel material.

[0061] (3) 40 g of red mud, 20 g of blast furnace slag, 35 g of overburned magnesium oxide powder, 20 g of potassium dihydrogen phosphate and 6 g of borax were mixed to obtain a solid waste-based magnesium phosphate cement material.

[0062] (4) Mix 90 g of high iron phase precursor cementitious material and 80 g of solid waste-based magnesium phosphate cement material to obtain a dry mixture; dissolve 6 g of naphthalene-based water reducer in 90 g of water to obtain an admixture solution for later use; add the admixture solution to the dry mixture and stir evenly to prepare a highly corrosion-resistant all-solid waste-based marine engineering cementitious material.

[0063] Example 2

[0064] (1) Red mud, carbide slag, silica fume, limestone tailings and aluminum ash are dried to a moisture content of no more than 25% and passed through a 100-mesh sieve; various dried materials are mixed, based on solid mass, to obtain a mixture of 40 g red mud, 30 g carbide slag, 10 g silica fume, 15 g limestone tailings and 5 g aluminum ash; the mixture has a limestone saturation coefficient (KH) of 0.89, a silicon content (SM) of 1.74 and an aluminum content (IM) of 0.93.

[0065] (2) The mixture was heated to 1330°C at a rate of 10°C / min and calcined for 3.22 hours. The calcined product was first water-cooled for 5 minutes and then naturally cooled for 2 hours. The cooled calcined product was crushed, ground, and sieved through a 200-mesh sieve to obtain a high-iron phase precursor gel material.

[0066] (3) 40 g of red mud, 20 g of blast furnace slag, 35 g of overburned magnesium oxide powder, 20 g of potassium dihydrogen phosphate and 6 g of borax were mixed to obtain a solid waste-based magnesium phosphate cement material.

[0067] (4) Mix 90 g of high iron phase precursor cementitious material and 85 g of solid waste-based magnesium phosphate cement material to obtain a dry mixture; dissolve 6 g of naphthalene-based water reducer in 95 g of water to obtain an admixture solution for later use; add the admixture solution to the dry mixture and stir evenly to prepare a highly corrosion-resistant all-solid waste-based marine cementitious material.

[0068] Example 3

[0069] (1) Red mud, carbide slag, silica fume, limestone tailings and aluminum ash are dried to a moisture content of no more than 25% and passed through a 100-mesh sieve; various dried materials are mixed, based on solid mass, to obtain a mixture of 40 g red mud, 30 g carbide slag, 10 g silica fume, 15 g limestone tailings and 5 g aluminum ash; the mixture has a limestone saturation coefficient (KH) of 0.89, a silicon content (SM) of 1.74 and an aluminum content (IM) of 0.93.

[0070] (2) The temperature was raised to 1300°C at a heating rate of 10°C / min for high temperature calcination for 3.16 hours. The calcined product was first water-cooled for 5 minutes and then naturally cooled for 2 hours. The cooled calcined product was crushed, ground, and sieved through a 200-mesh sieve to obtain a high-iron phase precursor gel material.

[0071] (3) 35 g of red mud, 20 g of blast furnace slag, 35 g of overburned magnesium oxide powder, 25 g of potassium dihydrogen phosphate and 6 g of urea were mixed to obtain a solid waste-based magnesium phosphate cement material.

[0072] (4) Mix 90 g of high iron phase precursor cementitious material and 80 g of solid waste-based magnesium phosphate cement material to obtain a dry mixture; dissolve 6 g of naphthalene-based water reducer in 90 g of water to obtain an admixture solution for later use; add the admixture solution to the dry mixture and stir evenly to prepare a highly corrosion-resistant all-solid waste-based marine engineering cementitious material.

[0073] Comparative Example 1

[0074] Compared with Example 1, the difference is that this comparative example does not add solid waste-based magnesium phosphate cement materials.

[0075] (1) Red mud, carbide slag, silica fume, limestone tailings and aluminum ash are dried to a moisture content of no more than 25% and passed through a 100-mesh sieve; various dried materials are mixed, based on solid mass, to obtain a mixture of 40 g red mud, 30 g carbide slag, 10 g silica fume, 15 g limestone tailings and 5 g aluminum ash; the mixture has a limestone saturation coefficient (KH) of 0.89, a silicon content (SM) of 1.74 and an aluminum content (IM) of 0.93.

[0076] (2) The mixture was heated to 1300°C at a heating rate of 10°C / min and calcined at high temperature for 3.16 hours. The calcined product was first water-cooled for 5 minutes and then naturally cooled for 2 hours. The cooled calcined product was crushed, ground, and sieved through a 200-mesh sieve to obtain a high-iron phase precursor gel material.

[0077] (3) 6 g of a naphthalene-based water reducer was dissolved in 90 g of water to obtain an admixture solution, and the admixture solution was added to 90 g of a high iron phase precursor gelling material, and the mixture was stirred evenly to prepare a gelling material.

[0078] Comparative Example 2

[0079] Compared with Example 1, the difference is that this comparative example does not add a high iron phase precursor gelling material.

[0080] (1) 40 g of red mud, 20 g of blast furnace slag, 35 g of overburned magnesium oxide powder, 20 g of potassium dihydrogen phosphate and 6 g of borax are mixed to obtain a solid waste-based magnesium phosphate cement material.

[0081] (2) dissolving 6 g of a naphthalene-based water reducer in 90 g of water to obtain an admixture solution; adding the admixture solution to 80 g of a solid waste-based magnesium phosphate cement material, and uniformly stirring to prepare a cementitious material.

[0082] Test example

[0083] Concrete was prepared using the highly corrosion-resistant all-solid waste-based marine engineering cementitious materials prepared in Examples 1 to 3 and the cementitious materials of Comparative Examples 1 to 2. The concrete was prepared in accordance with the "Code for Design of Ordinary Concrete Mix Ratio" JGJ 55-2011. The properties of the concrete prepared in Examples 1 to 3 and Comparative Examples 1 to 2 are shown in Table 1.

[0084] Table 1 Performance test results of concrete of embodiment and comparative example

[0085]

[0086]

[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A highly corrosion-resistant all-solid waste-based marine engineering cementitious material, characterized in that: It includes 40 to 50 parts of high iron phase precursor cementitious material, 35 to 45 parts of solid waste-based magnesium phosphate cement material, 2 to 4 parts of water reducing agent and 30 to 50 parts of water; The high iron phase precursor gelling material is obtained by calcining a mixture of calcium-based solid waste, silicon-based solid waste, aluminum-based solid waste and iron-based solid waste; the limestone saturation coefficient of the mixture is 0.87-0.96, the silicon ratio is 1.7-2.7, and the aluminum ratio is 0.9-1.9; The solid waste-based magnesium phosphate cement material comprises 15 to 25 parts of calcium-based solid waste, 35 to 40 parts of iron-based solid waste, 30 to 40 parts of overburned magnesium oxide powder, 20 to 25 parts of potassium dihydrogen phosphate and 5 to 8 parts of retarder.

2. The highly corrosion-resistant all-solid waste-based marine engineering cementitious material according to claim 1, characterized in that: The calcium-based solid waste of the high iron phase precursor cementitious material and the solid waste-based magnesium phosphate cement material is selected from one or more of carbide slag, blast furnace slag, fly ash, limestone tailings or shell powder, and has a specific surface area of ​​300-450m 2 / kg.

3. The highly corrosion-resistant all-solid waste-based marine cementitious material according to claim 1, characterized in that: The iron-based solid waste of the high iron phase precursor cementitious material and the solid waste-based magnesium phosphate cement material is selected from one or more of red mud, steel slag, steelmaking dust mud or grinding wheel mud, and has a specific surface area of ​​300-450m 2 / kg.

4. The highly corrosion-resistant all-solid waste-based marine engineering cementitious material according to claim 1, characterized in that: The silicon-based solid waste is selected from one or more of coal gangue, silica fume or waste glass, and has a specific surface area of ​​300 to 450 m 2 / kg.

5. The highly corrosion-resistant all-solid waste-based marine engineering cementitious material according to claim 1, characterized in that: The aluminum-based solid waste is selected from one or more of aluminum ash, red mud, waste aluminum foil or aluminum tailings, and has a specific surface area of ​​300 to 450 m 2 / kg.

6. The highly corrosion-resistant all-solid waste-based marine engineering cementitious material according to claim 1, characterized in that: The retarder is selected from one or more of borax, malic acid, urea, lignosulfonic acid or triethanolamine.

7. The highly corrosion-resistant all-solid waste-based marine engineering cementitious material according to claim 1, characterized in that: The water reducer is selected from one or more of a naphthalene-based water reducer, a fatty acid-based water reducer or an aminosulfonate-based water reducer.

8. The method for preparing a highly corrosion-resistant all-solid waste-based marine engineering cementitious material according to any one of claims 1 to 7, characterized in that: The steps include: Calcium-based solid waste, silicon-based solid waste, aluminum-based solid waste and iron-based solid waste are mixed, and then calcined to obtain a high-iron phase precursor gelling material; Mixing calcium-based solid waste, iron-based solid waste, overburned magnesium oxide powder, potassium dihydrogen phosphate and a retarder to obtain a solid waste-based magnesium phosphate cement material; Mixing high iron phase precursor cementitious material and solid waste-based magnesium phosphate cement-like material in proportion to obtain a dry mix; Dissolve the water reducing agent in water to obtain an admixture solution; Add the admixture solution into the dry mix and stir evenly to obtain the product.

9. The preparation method according to claim 8, characterized in that: The calcination temperature is 1300-1400° C., the heating rate is controlled at 5-10° C. / min, and the calcination time is 3-4.5 hours.

10. Application of the highly corrosion-resistant all-solid waste-based marine cementitious material as described in any one of claims 1 to 7 or the highly corrosion-resistant all-solid waste-based marine cementitious material prepared by the preparation method as described in any one of claims 8 to 9 in the field of marine engineering grouting materials.

Citation Information

Patent Citations

  • Anti-erosion phosphoaluminate cement based cementing material applicable to ocean engineering

    CN108069632A

  • High-corrosion-resistance maritime work cementing material as well as preparation method and application thereof

    CN111704419A

  • Solid-waste-based high-iron sulphoaluminate maritime work cementing material as well as preparation method and application thereof

    CN113698117A

Cited By

  • Solid-waste-based grouting material suitable for subsea tunnel lining repair and preparation method of solid-waste-based grouting material

    CN120441281A

  • A solid waste-based grouting material suitable for submarine tunnel lining repair and its preparation method

    CN120441281B