Adsorbent as well as preparation method and application thereof

The reaction of phlogenetol and 2,6-dichloropyridine-3,5-dicarbonitrile to form porous organic hydrogen bonding materials, solving the problem of too low adsorption amount of existing uranyl adsorption materials and achieving efficient uranium Ion adsorption and stable seawater uranium recovery are suitable for the industrial production of seawater uranium extraction.

CN118978536AActive Publication Date: 2024-11-19NORTHEAST NORMAL UNIVERSITY

Patent Information

Application Number
CN202411048900.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The adsorption amount of existing uranyl adsorbent materials is too low to effectively extract uranium ions from seawater, especially in cases where ultra-low concentrations and coexistence interfere with metal ions.

Method used

The reaction of phlogenetol and 2,6-dichloropyridine-3,5-dicarbonitrile under alkaline catalysis to form a cyano group-containing molecular cage, and react with hydroxylamine hydrochloride to form an amide oxime group, and prepare it Porous organic hydrogen bonding material with high selectivity and high adsorption.

Benefits of technology

The obtained porous organic hydrogen bonding material has an uranium ion adsorption rate of 1727mg·g-1 at room temperature, which has good selectivity and stability, and can maintain high uranium recovery capacity in natural seawater. It is suitable for the industrial production of seawater uranium extraction. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978536A_ABST
    Figure CN118978536A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of adsorption materials, and discloses an adsorbent as well as a preparation method and application thereof. The preparation method comprises the following steps: dissolving phloroglucinol, 2, 6-dichloropyridine-3, 5-dicarbonitrile and a basic catalyst, reacting for 1-1.5 hours, and extracting to obtain an organic layer which is a molecular cage containing a cyano group; and under an alkaline condition, dissolving the obtained molecular cage containing the cyano group and hydroxylamine hydrochloride, reacting for 24-48 hours under the condition of 58-65 DEG C, and filtering to obtain a solid, namely the adsorbent. The main structure of the adsorbent obtained by the invention is a molecular cage containing an amidoxime group, and the amidoxime functional group as a uranium absorbent shows huge potential due to selectivity and high chelating affinity to uranium. The organic structure unit also contains a lot of nitrogen and oxygen atoms with electronegativity, so that a synergistic effect on selective adsorption of uranium ions can be achieved; # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adsorption materials, and in particular relates to an adsorbent and a preparation method and application thereof. Background Art

[0002] With the growing demand for energy and the massive burning of fossil fuels, nuclear energy has long attracted much attention as a carbon-free energy source that can greatly alleviate the global energy crisis on a large scale. Among all radionuclides, uranium, as a key basic resource for sustainably enhancing the capacity of nuclear reactors, plays an indispensable role in the search for alternative energy sources. It is estimated that the global seawater contains an almost inexhaustible amount of uranium, about 4.5 tons, which is nearly 1,000 times that of terrestrial uranium mines, so the development of selective uranium extraction technology seems particularly important. However, the ultra-low concentration of soluble uranium, about 3.3 ppb, and the coexistence of a large amount of excessive interfering metal ions have brought unprecedented challenges to the recovery of uranium from the ocean. Therefore, how to obtain highly selective and high-adsorption materials for extracting uranium ions from seawater is a technical problem that needs to be solved urgently.

[0003] The prior art discloses a synthesis method and application of a uranyl adsorbent material, with reference to Chinese patent CN107349919 B. Preparation method: a) fiber, polymer, double bond monomer and water are mixed and irradiated with electron beam to obtain a gel; the polymer includes one or more of polyvinyl alcohol, polyvinyl pyrrolidone, polystyrene and polyacrylonitrile; the double bond monomer includes one or more of acrylonitrile, divinylbenzene, styrene, acrylic acid, acrylamide, butadiene, pentadiene and triallyl isocyanurate; b) the gel is mixed with acrylonitrile and irradiated with electron beam to obtain a graft cross-linked body; c) the graft cross-linked body is mixed with hydroxylamine and reacted to obtain a uranyl adsorbent material. The adsorption capacity of the adsorbent is too small. Summary of the invention

[0004] The invention provides an adsorbent and a preparation method and application thereof, which solve the problem that the adsorption amount of the uranyl adsorption material prepared in the prior art is too low.

[0005] An adsorbent, the structural formula of the adsorbent is as follows:

[0006]

[0007] The second object of the present invention is to protect a method for preparing the adsorbent, which specifically comprises the following steps:

[0008] After dissolving phloroglucinol, 2,6-dichloropyridine-3,5-dicarbonitrile and an alkaline catalyst, the mixture is reacted for 1 h to 1.5 h, and the organic layer after extraction is vacuum dried at 60° C. to 80° C. for 12 h to 48 h to obtain a molecular cage containing a cyano group;

[0009] Under alkaline conditions, the obtained molecular cage containing cyano groups and hydroxylamine hydrochloride are dissolved, reacted at 58° C. to 65° C. for 24 h to 48 h, and then the obtained solid is filtered and vacuum dried at 100° C. to 110° C. for 12 h to 48 h to obtain the adsorbent.

[0010] The molecular cage synthesized by using 2,6-dichloropyridine-3,5-dicarbonitrile as a raw material and reacting with phloroglucinol under the catalysis of an alkaline catalyst contains many cyano groups, which can be converted into amine oxime groups with specific adsorption to uranium ions. The adsorbent prepared by the present invention has a molecular cage with six amine oximes as structural units on one molecule.

[0011] The reaction temperature of 58°C to 65°C is selected because when the temperature is too high, the cyano group is easily converted into a carboxyl group, and the boiling point of the solvent is 65°C. Therefore, in order to increase the yield and the reaction can be completely converted into an amine oxime group, the temperature is set to this range.

[0012] Preferably, when preparing the adsorbent, the molar ratio of the molecular cage containing the cyano group to hydroxylamine hydrochloride is 1:12-24.

[0013] Preferably, the molar ratio of phloroglucinol, 2,6-dichloropyridine-3,5-dicarbonitrile and the alkaline catalyst is 2:3:4-8.

[0014] The molar ratio of the molecular cage containing cyano groups and hydroxylamine hydrochloride, and the molar ratio of phloroglucinol and 2,6-dichloropyridine-3,5-dicarbonitrile were all set according to the number of reactive groups.

[0015] Preferably, the alkaline catalyst is any one of cesium carbonate, potassium carbonate, sodium carbonate, sodium hydroxide and potassium hydroxide.

[0016] Preferably, the structural formula of the molecular cage containing a cyano group is as follows:

[0017]

[0018] Preferably, the adsorbent is crystallized at -5°C to 35°C to obtain a porous organic hydrogen bond material.

[0019] Preferably, when the adsorbent is crystallized at -5°C to 24°C, the prepared porous organic hydrogen-bonded material has an R-3C space group, and the unit cell parameters are: α=90°, β=90°, γ=120°.

[0020] Preferably, when the adsorbent is crystallized at 25°C to 35°C, the prepared porous organic hydrogen-bonded material has a P-1 space group, and the unit cell parameters are: α=98.1°, β=106.6°, γ=94.3°.

[0021] The third object of the present invention is to protect the adsorbent as the porous organic hydrogen bonding material, and the porous organic hydrogen bonding material is used for extracting uranium from seawater.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The main structure of the adsorbent obtained by the present invention is a molecular cage containing an amide oxime group. Compared with other groups, the amide oxime functional group shows great potential as a uranium absorbent due to its selectivity and high chelating affinity for uranium. At the same time, there are many electronegative nitrogen and oxygen atoms in the organic structural unit, which can play a synergistic role in the selective adsorption of uranium ions. The adsorbent obtained by the present invention is crystallized to obtain a porous organic hydrogen bond material, and the maximum uranium ion adsorption rate can reach 1727 mg·g at room temperature. -1 The porous organic hydrogen-bonded material obtained by the present invention has high crystallinity. Different from other different types of amine oxime-based adsorbents, such as nanofibers, resins, hydrogels, covalent organic frameworks and porous aromatic frameworks, the porous organic hydrogen-bonded material obtained by the present invention has orderly pores and clear structures, and contains a large number of available chelating active sites, which can allow uranium ions to enter the pores and be selectively adsorbed between layers, meeting the requirements for practical applications in seawater.

[0024] In addition, the porous organic hydrogen-bonded material obtained by the present invention has good U / V selectivity, and can maintain its structural stability even after 7 adsorption-desorption cycles, and the adsorption rate can still reach more than 90%. In natural seawater, the porous organic hydrogen-bonded material has reached 10.85 mg·g after 30 days of field testing. -1 Considering these advantages, the present invention has great potential for uranium immobilization and opens up a new concept for synthetic uranium recovery materials.

[0025] 2. After the prepared adsorbent of the present invention is crystallized at different temperatures, the obtained porous organic hydrogen bond material has different crystal forms. The adsorbent has a large adsorption capacity for the crystal structure formed at 25°C to 35°C, and a small adsorption capacity for the crystal structure formed at -5°C to 24°C. This is because the material formed at high temperature has pores through which uranium ions can pass, while the material formed at low temperature has no pores and can only be adsorbed on the surface of the adsorbent.

[0026] 3. The preparation method of the porous organic hydrogen-bonded material for extracting uranium from seawater of the present invention is simple, the raw materials are cheap, the instruments used are conventional, and it is easy to use. It has good application prospects in the field of extracting uranium from seawater and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1This is the infrared spectrum of the cyano-containing molecular cage and its amide oximation obtained in Example 1 of the present invention;

[0028] Figure 2 This is the H NMR spectrum of the amide oxime molecular cage obtained in Example 1 of the present invention;

[0029] Figure 3 This is the NMR carbon spectrum of the amidoxime molecular cage obtained in Example 1 of the present invention;

[0030] Figure 4 This is an X-ray single crystal diffraction pattern of the porous organic hydrogen-bonding material prepared in Example 1;

[0031] Figure 5 This is an X-ray single crystal diffraction pattern of the porous organic hydrogen-bonding material prepared in Example 2;

[0032] Figure 6 This is an isothermal adsorption performance diagram of the porous organic hydrogen-bonded material obtained in Example 1 of the present invention for adsorbing uranium ions;

[0033] Figure 7 This is a kinetic diagram of the porous organic hydrogen-bonding material obtained in Example 1 of the present invention adsorbing uranium ions;

[0034] Figure 8 Graph showing the effect of pH on the adsorption of uranyl ions by the porous organic hydrogen-bonding material obtained in Example 1 of the present invention;

[0035] Fig. 9 This is a test graph of uranyl ion adsorption selectivity of the porous organic hydrogen-bonding material obtained in Example 1 of the present invention;

[0036] Fig.10 This is a graph of uranium cyclic adsorption and desorption test of the porous organic hydrogen-bonding material obtained in Example 1 of the present invention;

[0037] Fig.11 This is a test diagram of the porous organic hydrogen-bonding material obtained in Example 1 of the present invention adsorbing uranyl ions in natural seawater. DETAILED DESCRIPTION

[0038] The technical solutions in the present invention will be described clearly and completely below in conjunction with the specific implementation of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] The methods described in the embodiments of the present invention are conventional methods unless otherwise specified. The materials, reagents, etc. used can be obtained from commercial sources unless otherwise specified.

[0040] The structure of the molecular cage containing a cyano group prepared in the embodiment of the present invention is as follows:

[0041]

[0042] Example 1

[0043] A method for preparing an adsorbent comprises the following steps:

[0044] (1) Under ambient atmosphere, 1.59mmol of phloroglucinol, i.e. 200mg, 2.38mmol of 2,6-dichloropyridine-3,5-dicarbonitrile, i.e. 472mg and 4mmol of cesium carbonate, i.e. 1.30g, were added to a round-bottom flask, and 50mL of anhydrous dimethyl sulfoxide was added. The mixture was stirred for 1h to obtain a mixed product. The mixed product was extracted with 100mL of ethyl acetate and 100mL of ultrapure water, separated, the aqueous layer was extracted twice with 40mL of ethyl acetate, and the organic layers were combined. The combined organic layers were washed with 100mL of saturated brine, dried with anhydrous sodium sulfate, filtered, and the liquid was evaporated to remove the solvent to obtain a mixed solid. The obtained mixed solid was then washed three times with anhydrous methanol, filtered, and the washed solid was vacuum dried at 60°C for 12h. The obtained solid was a molecular cage containing a cyano group.

[0045] (2) Under ambient atmosphere, 251 mg of the cyano group-containing molecular cage obtained in step (1), 333.3 mg of hydroxylamine hydrochloride and 192 mg of sodium hydroxide were placed in a round-bottom flask, 30 mL of methanol was added, and the product was filtered after reacting at 58° C. for 24 h. After washing with ultrapure water, the solid was vacuum dried at 110° C. for 12 h to obtain an amide oxime molecular cage, i.e., the adsorbent.

[0046] (3) At 25° C., 50 mg of the adsorbent prepared in step (2) was dissolved in 70 mL of methanol and evaporated at room temperature for 2 days under ambient atmosphere to obtain a porous organic hydrogen bond material.

[0047] The porous organic hydrogen-bonded material prepared in this embodiment has a P-1 space group, and the unit cell parameters are: α=98.1°, β=106.6°, γ=94.3°.

[0048] Example 2

[0049] A method for preparing an adsorbent comprises the following steps:

[0050] (1) Under ambient atmosphere, 1.59mmol of phloroglucinol, i.e. 200mg, 2.38mmol of 2,6-dichloropyridine-3,5-dicarbonitrile, i.e. 472mg and 4mmol of cesium carbonate, i.e. 1.30g, were added to a round-bottom flask, and 50mL of anhydrous dimethyl sulfoxide was added. The mixture was stirred for 1h to obtain a mixed product. The mixed product was extracted with 100mL of ethyl acetate and 100mL of ultrapure water, separated, the aqueous layer was extracted twice with 40mL of ethyl acetate, and the organic layers were combined. The combined organic layers were washed with 100mL of saturated brine, dried with anhydrous sodium sulfate, filtered, and the liquid was evaporated to remove the solvent to obtain a mixed solid. The obtained mixed solid was then washed three times with anhydrous methanol, filtered, and the washed solid was vacuum dried at 60°C for 12h. The obtained solid was a molecular cage containing a cyano group.

[0051] (4) Under ambient atmosphere, 251 mg of the cyano group-containing molecular cage obtained in step (1), 333.3 mg of hydroxylamine hydrochloride and 192 mg of sodium hydroxide were placed in a round-bottom flask, 30 mL of methanol was added, and the product was filtered after reacting at 58° C. for 24 h. After washing with ultrapure water, the solid was vacuum dried at 110° C. for 12 h to obtain an amide oxime molecular cage, i.e., the adsorbent.

[0052] (5) At 29° C., 50 mg of the adsorbent obtained in step (2) was dissolved in 70 mL of methanol and evaporated at room temperature for 2 days under ambient atmosphere to obtain a porous organic hydrogen bond material.

[0053] The porous organic hydrogen-bonded material prepared in this embodiment has a P-1 space group, and the unit cell parameters are: α=98.1°, β=106.6°, γ=94.3°.

[0054] Example 3

[0055] A method for preparing an adsorbent comprises the following steps:

[0056] (1) Under ambient atmosphere, 1.59mmol of phloroglucinol, i.e. 200mg, 2.38mmol of 2,6-dichloropyridine-3,5-dicarbonitrile, i.e. 472mg and 4mmol of cesium carbonate, i.e. 1.30g, were added to a round-bottom flask, and 50mL of anhydrous dimethyl sulfoxide was added. The mixture was stirred for 1h to obtain a mixed product. The mixed product was extracted with 100mL of ethyl acetate and 100mL of ultrapure water, separated, the aqueous layer was extracted twice with 40mL of ethyl acetate, and the organic layers were combined. The combined organic layers were washed with 100mL of saturated brine, dried with anhydrous sodium sulfate, filtered, and the liquid was evaporated to remove the solvent to obtain a mixed solid. The obtained mixed solid was then washed three times with anhydrous methanol, filtered, and the washed solid was vacuum dried at 60°C for 12h. The obtained solid was a molecular cage containing a cyano group.

[0057] (6) Under ambient atmosphere, 251 mg of the cyano group-containing molecular cage obtained in step (1), 333.3 mg of hydroxylamine hydrochloride and 192 mg of sodium hydroxide were placed in a round-bottom flask, 30 mL of methanol was added, and the product was filtered after reacting at 58° C. for 24 h. After washing with ultrapure water, the solid was vacuum dried at 110° C. for 12 h to obtain an amide oxime molecular cage, i.e., the adsorbent.

[0058] (7) At 35° C., 50 mg of the adsorbent obtained in step (2) was dissolved in 70 mL of methanol and evaporated at room temperature for 2 days under ambient atmosphere to obtain a porous organic hydrogen bond material.

[0059] The porous organic hydrogen-bonded material prepared in this embodiment has a P-1 space group, and the unit cell parameters are: α=98.1°, β=106.6°, γ=94.3°.

[0060] Example 4

[0061] A method for preparing an adsorbent comprises the following steps:

[0062] (1) Under ambient atmosphere, 1.59mmol of phloroglucinol, i.e. 200mg, 2.38mmol of 2,6-dichloropyridine-3,5-dicarbonitrile, i.e. 472mg, and 4mmol of cesium carbonate, i.e. 1.30g, were added to a round-bottom flask, and 50mL of anhydrous DMSO was added. The mixture was stirred for 1h to obtain a mixed product. The mixed product was extracted with 100mL of ethyl acetate and 100mL of ultrapure water, separated, the aqueous layer was extracted twice with 40mL of ethyl acetate, and the organic layers were combined. The combined organic layers were washed with 100mL of saturated brine, dried with anhydrous sodium sulfate, filtered, and the liquid was evaporated to remove the solvent to obtain a mixed solid. The obtained mixed solid was then washed three times with anhydrous methanol, filtered, and the washed solid was vacuum dried at 60°C for 12h. The obtained solid was a molecular cage containing a cyano group.

[0063] (2) Under ambient atmosphere, 251 mg of the cyano group-containing molecular cage obtained in step (1), 500 mg of hydroxylamine hydrochloride and 288 mg of sodium hydroxide were placed in a round-bottom flask, 30 mL of methanol was added, and the product was filtered after reacting at 58° C. for 24 h. After washing with ultrapure water, the solid was vacuum dried at 110° C. for 12 h to obtain an amide oxime molecular cage, i.e., the adsorbent.

[0064] (3) At 5° C., 50 mg of the adsorbent prepared in step (2) was dissolved in 70 mL of methanol and slowly evaporated for 2 days under ambient atmosphere to obtain a porous organic hydrogen bond material.

[0065] The porous organic hydrogen-bonded material prepared in this embodiment has an R-3C space group, and the unit cell parameters are: α=90°, β=90°, γ=120°.

[0066] Example 5

[0067] A method for preparing an adsorbent comprises the following steps:

[0068] (1) Under ambient atmosphere, 1.59mmol of phloroglucinol, i.e. 200mg, 2.38mmol of 2,6-dichloropyridine-3,5-dicarbonitrile, i.e. 472mg and 7mmol of cesium carbonate, i.e. 2.28g, were added to a round-bottom flask, and 50mL of anhydrous DMSO was added. The mixture was stirred for 1h to obtain a mixed product. The mixed product was extracted with 100mL of ethyl acetate and 100mL of ultrapure water, separated, the aqueous layer was extracted twice with 40mL of ethyl acetate, and the organic layers were combined. The combined organic layers were washed with 100mL of saturated brine, dried with anhydrous sodium sulfate, filtered, and the liquid was evaporated to remove the solvent to obtain a mixed solid. The obtained mixed solid was then washed three times with anhydrous methanol, filtered, and the washed solid was vacuum dried at 70°C for 36h. The obtained solid was a molecular cage containing a cyano group.

[0069] (2) Under ambient atmosphere, 251 mg of the cyano group-containing molecular cage obtained in step (1), 583.3 mg of hydroxylamine hydrochloride and 336 mg of sodium hydroxide were placed in a round-bottom flask, 30 mL of methanol was added, and the product was filtered after reacting at 63° C. for 40 h. After washing with ultrapure water, the solid was vacuum dried at 110° C. for 36 h to obtain an amide oxime molecular cage, i.e., the adsorbent.

[0070] (3) At -5°C, 50 mg of the adsorbent prepared in step (2) was dissolved in 70 mL of methanol and slowly evaporated for 2 days under ambient atmosphere to obtain a porous organic hydrogen bond material.

[0071] The porous organic hydrogen-bonded material prepared in this embodiment has an R-3C space group, and the unit cell parameters are: α=90°, β=90°, γ=120°.

[0072] Example 6

[0073] A method for preparing an adsorbent comprises the following steps:

[0074] (1) Under ambient atmosphere, 1.59mmol of phloroglucinol, i.e. 200mg, 2.38mmol of 2,6-dichloropyridine-3,5-dicarbonitrile, i.e. 472mg and 8mmol of cesium carbonate, i.e. 2.61g, were added to a round-bottom flask, and 50mL of anhydrous DMSO was added. The mixture was stirred for 1h to obtain a mixed product. The mixed product was extracted with 100mL of ethyl acetate and 100mL of ultrapure water, separated, the aqueous layer was extracted twice with 40mL of ethyl acetate, and the organic layers were combined. The combined organic layers were washed with 100mL of saturated brine, dried with anhydrous sodium sulfate, filtered, and the liquid was evaporated to remove the solvent to obtain a mixed solid. The obtained mixed solid was then washed three times with anhydrous methanol, filtered, and the washed solid was vacuum dried at 80°C for 48h. The obtained solid was a molecular cage containing a cyano group.

[0075] (2) Under ambient atmosphere, 251 mg of the cyano group-containing molecular cage obtained in step (1), 666.7 mg of hydroxylamine hydrochloride and 384 mg of sodium hydroxide were placed in a round-bottom flask, 30 mL of methanol was added, and the product was filtered after reacting at 65° C. for 48 h. After washing with ultrapure water, the solid was vacuum dried at 110° C. for 48 h to obtain an amide oxime molecular cage, i.e., the adsorbent.

[0076] (3) At 10° C., 50 mg of the adsorbent prepared in step (2) was dissolved in 70 mL of methanol and slowly evaporated for 2 days under ambient atmosphere to obtain a porous organic hydrogen bond material.

[0077] The porous organic hydrogen-bonded material prepared in this embodiment has an R-3C space group, and the unit cell parameters are: α=90°, β=90°, γ=120°.

[0078] Comparative Example 1

[0079] Refer to Example 3 of Chinese Patent CN 107349919 B.

[0080] A method for synthesizing uranyl adsorption material:

[0081] (1) 11 parts by weight of straw fiber with a fineness of ≥30 mesh and an ash content of ≤2wt% are put into a mixing tank, and 600 parts by weight of clean water, 130 parts by weight of polyvinyl alcohol (brand 1799), 20 parts by weight of styrene, 0.9 parts by weight of acrylonitrile, 0.5 parts by weight of fatty alcohol polyoxyethylene ether (brand AEO-3), and 12 parts by weight of isopropanol are added, and stirred evenly; the brand of polyvinyl alcohol is 1799, and the brand of fatty alcohol polyoxyethylene ether is AEO-3.

[0082] (2) The prepared slurry in (1) is irradiated under an electron beam so that the absorbed dose of the slurry reaches 100 kGy, thereby obtaining a gel sheet.

[0083] (3) The gel sheet obtained in (2) is cut into gel particles by a cutting machine.

[0084] (4) Add 1.8 parts by weight of acrylonitrile to 10 parts by weight of the particles obtained in (3), mix well, and irradiate with an electron beam at a dose of 60 kGy to obtain a graft cross-linked body.

[0085] (5) 4.8 parts by weight of hydroxylamine hydrochloride was added to the graft cross-linked product of (4), and the temperature was controlled to react at 80° C. for 6 hours to obtain a uranyl adsorption material.

[0086] In this embodiment, the particle size of the uranyl adsorption material finally obtained is controlled to be 30-80 meshes by controlling the size of the colloid particles in step (3).

[0087] Performance Testing

[0088] 1) The apparent density of the prepared adsorption material was tested, and the result was: 0.6g / cm 3 .

[0089] 2) Prepare a solution containing 0.9 mg / L uranium ions, use the prepared adsorption material to adsorb at room temperature for 2 weeks under static conditions, and after elution, the adsorption amount is measured to reach 4.7 mg / g.

[0090] 3) A solution containing 10 mg / L uranium ions was prepared, and the prepared adsorbent material was used for adsorption at room temperature for one day under static conditions. After elution, the adsorption amount was measured to reach 29 mg / g; the adsorption amount of the adsorbent material after the third elution was 85.3% of the original adsorption amount.

[0091] The maximum adsorption capacity of the porous organic hydrogen bond material prepared in Examples 2 and 3 is 1723±10 mg·g -1 Therefore, the following performance test only takes the porous organic hydrogen bond material prepared in Example 1 as an example. Since the maximum adsorption capacity of the porous organic hydrogen bond materials prepared in Examples 4, 5, and 6 is relatively low, all at 300 mg·g -1 Therefore, the subsequent equilibrium adsorption amount is only taken as an example of the porous organic hydrogen bond material prepared in Example 4.

[0092] The maximum adsorption capacity of uranium ions by the uranyl adsorbent material in Comparative Example 1 is 29 mg·g -1 The porous organic hydrogen-bonded material prepared in Example 1 of the present invention has a higher adsorption capacity of 1723 mg·g -1; and even after 7 adsorption-desorption cycles, the structural stability can still be maintained, and the adsorption rate can still reach more than 90%, and the cyclic adsorption performance is higher than that of the uranyl adsorption material prepared in Comparative Example 1. In addition, the adsorption amount of the adsorbent of Example 1 in natural seawater is also higher than that of the ion-crosslinked supramolecular hydrogel membrane prepared in Comparative Example 1. It shows that the present invention has great potential for uranium immobilization, meets the application of seawater in practical requirements, and opens up a new concept for the synthesis of uranium recovery materials.

[0093] Figure 1 The infrared spectrum of the cyano-containing molecular cage obtained in Example 1 of the present invention and its amide oximation is shown in Figure 1. The infrared spectrum of the molecular cage before and after amide oximation is tested. The test results are as follows: Figure 1 As shown in the figure, the peak of the typical bond representing the C≡N stretching vibration of the cyanide molecular cage is at 2238cm -1 , while the amide oxime molecular cage has no obvious signal. However, the C=N related characteristic signal area appears in the infrared peak of the amide oxime molecular cage. In summary, the cyano group has been completely converted into the amide oxime group. This shows that the molecular cage is successfully amined.

[0094] Figure 2 The following is the H NMR spectrum of the amidoxime molecular cage obtained in Example 1 of the present invention. 1 H nuclear magnetic test, the test results are as follows Figure 2 As shown in the figure, the two singlets correspond to the amidoxime groups, of which the chemical shift peak of 9.60ppm belongs to the hydroxyl group, while the singlet of 5.82ppm is attributed to the amino group, indicating that the molecular cage has been successfully amidoximated. In addition, we also observed that the chemical shifts of the two aromatic proton peaks were 7.96 and 6.79ppm, respectively, and both peaks were singlets.

[0095] Figure 3 The following is the NMR carbon spectrum of the amidoxime molecular cage obtained in Example 1 of the present invention. 13 C nuclear magnetic test, the test results are as follows Figure 3 As shown in the figure, there are six chemical shift peaks, corresponding to six carbon atoms in different environments in the amide oxime molecular cage.

[0096] Figure 4 This is an X-ray single crystal diffraction pattern of the porous organic hydrogen bonding material prepared in Example 1. The displacement ellipsoid is scaled to a probability level of 50%. Figure 5This is the X-ray single crystal diffraction pattern of the porous organic hydrogen-bonding material prepared in Example 4. The displacement ellipsoid is scaled to a probability level of 50%. The crystallization temperatures of Example 1 and Example 4 are different, and the crystal arrangements of the obtained porous organic hydrogen-bonding materials are different. The crystal structure formed by the adsorbent at 25°C to 35°C has a large adsorption capacity, while the crystal structure formed at -5°C to 24°C has a small adsorption capacity. This is because the material formed at high temperature has pores inside that allow uranium ions to pass through, while the material formed at low temperature has no pores and can only be adsorbed on the surface of the adsorbent.

[0097] Figure 6 The isothermal adsorption performance curve of the porous organic hydrogen bonding material for uranium ions obtained in Example 1 of the present invention is shown in HPOC-α; and the isothermal adsorption performance curve of the porous organic hydrogen bonding material for uranium ions obtained in Example 4 is shown in HPOC-β. Under the condition of pH 7.0, uranium simulation solutions with different initial concentrations, i.e., 1.0-80.0 mg·L -1 , used for equilibrium adsorption isotherm experiment. 1 mg of the adsorbent prepared in Example 1 was added to 80 mL of uranium solution to obtain a uranium solution after adsorption by the adsorbent. After stirring at room temperature for 24 hours, the uranium solution after adsorption by the adsorbent was taken out and analyzed according to the arsenazo III test. The equilibrium isotherm data were fitted with Langmuir and Freundlich adsorption isotherms, respectively, and the equations were as follows:

[0098]

[0099] Among them, C in formula (1) and formula (2) e is the equilibrium concentration, in mg·g -1 ;q m Indicates saturated adsorption capacity, unit: mg·g -1 ;q e Indicates the equilibrium adsorption capacity, unit: mg·g -1 ; k1 represents the Langmuir constant, which is related to the affinity of the binding site. It can be seen from the figure that Example 1 belongs to Langmuir monolayer chemical adsorption, and the maximum adsorption amount is 1727 mg·g -1 The porous organic hydrogen-bonding material prepared in Example 4 has a relatively small adsorption capacity for uranium ions. The following tests were conducted using the porous organic hydrogen-bonding material prepared in Example 1.

[0100] Figure 7The kinetic diagram of the adsorption of uranium ions by the porous organic hydrogen-bonding material obtained in Example 1 of the present invention. Under the condition of pH 7.0, the uranium capture kinetic experiment was measured at concentrations of 10ppm, 20ppm and 30ppm respectively. 3.0mg of the porous organic hydrogen-bonding material obtained in Example 1 was soaked and dispersed in 300mL of uranium simulated seawater, and then 0.5mL of the solution was taken out at 1h, 3h, 6h, 9h, 12h, 24h, 36h, 48h, 60h, 72h, 84h, 96h and 120h of reaction, and centrifuged for detection. In order to further study the adsorption kinetic mechanism, we list the pseudo-first-order model and the pseudo-second-order model as the following equations:

[0101]

[0102] ln(qE-qt)=lnqE-kt 式(4)

[0103] Wherein, qe in formula (3) and formula (4) represents the equilibrium adsorption amount, in units of mg·g- 1 ; k1 represents the rate constant, unit is g·h- 1 mg- 1 ; qt is the amount of uranium adsorbed after contact time t, in mg·g- 1 ; Ct is the uranium concentration at time t, in mg·g- 1 ; k3 is the kinetic rate constant, t is the reaction time, unit is h. When the adsorption equilibrium is reached, qt and Ct are replaced by qe and Ce respectively.

[0104] from Figure 7 It can be seen that the porous organic hydrogen-bonding material obtained in Example 1 reaches equilibrium with uranium simulation solutions of different concentrations in about 24 hours.

[0105] Figure 8 Graph showing the effect of pH on the adsorption of uranyl ions by the porous organic hydrogen-bonding material obtained in Example 1 of the present invention. To obtain the optimal pH for the adsorption of uranyl ions by the porous organic hydrogen-bonding material of Example 1, 1 mg of the porous organic hydrogen-bonding material sample was added to 80 mL of a 10 mg·L- 1 The uranium simulated solution contains 438.607×10- 3 M sodium chloride and 2.297×10- 3 The solution was divided into 7 portions and the pH was adjusted by hydrochloric acid and sodium hydroxide to 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, and 9.0, respectively. After shaking with a magnetic stirrer at room temperature for 36 h, the samples were separated and analyzed for the concentration of residual uranium by inductively coupled plasma optical emission spectroscopy, abbreviated as ICP-OES. The adsorption capacity is represented by qt and calculated by the following formula:

[0106]

[0107] Wherein, qt in formula (5) is the amount of uranium adsorbed after contact time t, in units of mg·g- 1 ; C0 is the initial uranium concentration, in mg·g- 1 ; Ct is the uranium concentration at time t, in mg·g- 1 ; V is the volume of the solution, in L; m is the mass of the adsorbent used, in g.

[0108] from Figure 8 It can be seen that the porous organic hydrogen bond material obtained in Example 1 has the largest adsorption capacity when the pH is 7, which is close to the real seawater pH ≈ 8, so the porous organic hydrogen bond material obtained in Example 1 can be used for uranium extraction from seawater.

[0109] Fig. 9 This is a test diagram of the uranyl ion adsorption selectivity of the porous organic hydrogen-bonding material obtained in Example 1 of the present invention. In order to accurately determine the affinity of the porous organic hydrogen-bonding material obtained in Example 1 for uranyl ions, the metal ion Fe 3+ , VO 2+ , Ni 2 + , Zn 2+ , Sr. 2+ , Pb 2+ ,Co 2+ ,Ba 2+ , Cu 2+ , Cd 2+ With uranyl ion, namely UO2 2+ Mixed with natural seawater concentrated 100 times to obtain a mixture; Na + Mg 2+ , Ca 2+ , K + The concentration remains at the original concentration, i.e., sodium ion: 10.716 g / L, magnesium ion: 1.287 g / L, calcium ion: 0.41 g / L, potassium ion: 0.397 g / L. The pH value of the mixture is adjusted to 6.0, and then 5.0 mg of the porous organic hydrogen-bonded material is immersed in 400 mL of the mixture and shaken for 72 hours, and then the residual uranium concentration in the solution is recorded and analyzed by inductively coupled plasma mass spectrometry, abbreviated as ICP-MS. It can be analyzed that the porous organic hydrogen-bonded material obtained in Example 1 exhibits a U / V selectivity of 1.51 times, which provides a potential application for uranium recovery in natural seawater.

[0110] Fig.10This is a graph showing the uranium cyclic adsorption and desorption test of the porous organic hydrogen-bonding material obtained in Example 1 of the present invention. In order to evaluate the reusability of the porous organic hydrogen-bonding material obtained in Example 1, 5.0 mg of the porous organic hydrogen-bonding material obtained in Example 1 was immersed in 400 mL of a 20.0 mg·L -1 The porous organic hydrogen bond material that adsorbed uranium ions was placed in simulated seawater and stirred continuously for 24 hours, and then the porous organic hydrogen bond material was separated and regenerated with 200 mL of a mixed eluent of 1 M sodium carbonate and 0.1 M hydrogen peroxide until the concentration of the elution solution could not be detected by ICP-MS; the molar ratio of sodium carbonate and 0.1 M hydrogen peroxide was 10:1. During the desorption process, we need to immerse the separated and regenerated porous organic hydrogen bond material in 500 mL of deionized water, wash it twice with circulating ultrapure water, and completely remove the eluent. As mentioned above, the uranium adsorption-desorption cycle experiment was repeated 7 times. From Fig. 9 It can be seen that after 7 cycles, the adsorption rate is still above 90%, indicating that the porous organic hydrogen bond material obtained in Example 1 has excellent stability.

[0111] Fig.11 This is a test diagram of the porous organic hydrogen-bonding material obtained in Example 1 of the present invention adsorbing uranyl ions in natural seawater. In order to detect the uranium absorption capacity of the porous organic hydrogen-bonding material obtained in Example 1 in natural seawater, a flow test platform for laboratory field testing was established. Natural seawater collected from the Bohai Sea near the coast of Qingdao City, Shandong Province, was filtered through a 0.22μm filter membrane to remove marine microorganisms and suspended solids. 10.0mg of the porous organic hydrogen-bonding material obtained in Example 1 was placed in the above-mentioned equipment, 50L of filtered natural seawater was added, and the mixture was stirred at room temperature at 1L·min -1 The flow rate was set at 100 °C for 3 parallel experiments. The concentration of uranium-based and other metal ions in seawater was analyzed by ICP-MS at certain intervals. The porous organic hydrogen-bonded material prepared by the present invention showed an extremely fast adsorption rate within the first 10 days and reached 10.85 mg·g after 30 days of testing. -1 It has strong uranium absorption capacity and extremely strong adsorption properties.

[0112] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0113] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. An adsorbent, characterized in that: The structural formula of the adsorbent is as follows:

2. The method for preparing an adsorbent according to claim 1, characterized in that: The specific steps include: After dissolving phloroglucinol, 2,6-dichloropyridine-3,5-dicarbonitrile and an alkaline catalyst, the reaction is carried out for 1 h to 1.5 h, and the organic layer after extraction is a molecular cage containing a cyano group; Under alkaline conditions, the obtained molecular cage containing cyano groups and hydroxylamine hydrochloride are dissolved, reacted at 58° C. to 65° C. for 24 h to 48 h, and then the solid obtained by filtering is used as the adsorbent.

3. The method for preparing an adsorbent according to claim 2, characterized in that: When preparing the adsorbent, the molar ratio of the molecular cage containing the cyano group to the hydroxylamine hydrochloride is 1:12-24.

4. The method for preparing an adsorbent according to claim 3, characterized in that: The molar ratio of phloroglucinol, 2,6-dichloropyridine-3,5-dicarbonitrile and the alkaline catalyst is 2:3:4-8.

5. The method for preparing an adsorbent according to claim 4, characterized in that: The alkaline catalyst is any one of cesium carbonate, potassium carbonate, sodium carbonate, sodium hydroxide and potassium hydroxide.

6. The method for preparing an adsorbent according to claim 5, characterized in that: The structural formula of the molecular cage containing the cyano group is as follows:

7. The method for preparing an adsorbent according to claim 2, characterized in that: The adsorbent is crystallized at -5°C to 35°C to obtain a porous organic hydrogen bond material.

8. The method for preparing an adsorbent according to claim 7, characterized in that: When the adsorbent is crystallized at -5°C to 24°C, the prepared porous organic hydrogen-bonded material has an R-3C space group, and the unit cell parameters are: α=90°, β=90°, γ=120°.

9. The method for preparing an adsorbent according to claim 8, characterized in that: When the adsorbent is crystallized at 25°C to 35°C, the prepared porous organic hydrogen-bonded material has a P-1 space group, and the unit cell parameters are: α=98.1°, β=106.6°, γ=94.3°.

10. An application of an adsorbent, characterized in that: The adsorbent is the porous organic hydrogen-bonding material according to claim 7, and the porous organic hydrogen-bonding material is used for extracting uranium from seawater.

Citation Information

Patent Citations

  • A method for synthesizing uranyl adsorbent materials and its application

    CN107349919B

  • Amino-amidoximino bifunctional super-crosslinked microporous uranium adsorbent and preparation method thereof

    CN111804285A

  • Amidoxime-based porous framework material and preparation method and application thereof in adsorbing and separating uranium ions