High-efficiency composite flame retardant for thermosetting polymer foaming resin and application of high-efficiency composite flame retardant
By using low-temperature gas phase, medium-temperature expansion, high-temperature skeleton flame retardant and fluorosiloxane modification treatment, the problem of uneven dispersion and migration of flame retardants in thermosetting polymer foam materials was solved, achieving gradient synergistic flame retardancy across the entire temperature range and improving the fire resistance and stability of the material.
Patent Information
- Application Number
- CN202411122533.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing flame retardants for thermosetting polymer foam materials suffer from uneven dispersion, migration of liquid flame retardants, and a decline in flame retardant effect over time, making it difficult to achieve effective flame retardancy within the full decomposition temperature range, thus affecting the fire resistance and stability of the materials.
By employing a composite of low-temperature gas-phase, medium-temperature expansion, and high-temperature skeleton flame retardants, as well as flame retardants containing active hydrogen, combined with fluorosiloxane surface modification treatment, a gradient synergistic flame retardant mechanism is formed, ensuring that the flame retardants are uniformly dispersed and stably exist in different temperature ranges.
It achieves gradient synergistic flame retardancy of polymer materials in the range of 150-800℃, improves the A2 fire rating of the materials, maintains the stability, strength and water resistance of the foam, and extends the flame retardant life.
Smart Images

Figure BDA0004995490970000021 
Figure BDA0004995490970000031 
Figure BDA0004995490970000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new materials, and in particular relates to a high-efficiency composite flame retardant for thermosetting polymer foaming resin and application thereof. Background Art
[0002] Thermosetting polymer foam materials such as phenolic foam, polyurethane foam and other thermosetting polymer resin foams are not only light in weight, but also have low thermal conductivity and excellent thermal insulation performance. However, their fire resistance is difficult to meet the A-level requirements, and their fire resistance must be improved. Generally, flame retardants are added to polymer foam materials to improve the flame retardancy of polymer foam materials. There are many types of flame retardants, such as halogen flame retardants, phosphorus flame retardants, nitrogen flame retardants and inorganic flame retardants. To achieve A-level flame retardancy, the method of adding inorganic and organic composite flame retardants is often used. Patent CN112679938A uses polyvinyl alcohol and sodium dodecylbenzene sulfonate to modify inorganic fillers such as copper oxide, lead dioxide and molybdenum oxide, etc., and smoke suppression flame retardants such as isophthalic acid, FR808, antimony trioxide and ferrocene to make polyurethane foam achieve A-level fire resistance, but the surface modifier used is hydrophilic, which is not conducive to the waterproofing of the foam material. Patent CN113585504A discloses that low-viscosity flame-retardant polyester and polyether are combined with silane coupling agent or titanate coupling agent to activate inorganic materials such as quartz sand, vitrified microspheres and calcium carbonate to achieve flame retardancy. This surface modification solves the reaction between hydroxyl groups on the surface of inorganic materials and black materials, reduces the formation of a large number of hydrogen bonds between polar groups on the surface of inorganic materials and combined white materials, and improves the compatibility of inorganic materials with rigid foam polyurethane, but low-viscosity flame-retardant polyester and polyether are expensive. Patent CN118005882A also uses bromine-containing highly flame-retardant polyether polyols, and also uses liquid flame retardants and solid flame retardants to achieve flame retardancy. Patent CN116656005A discloses a composite flame retardant, which uses a catalytic flame retardant and an endothermic flame retardant for composite flame retardancy. Although these patents claim to achieve Class A flame retardancy, they all have the problem of uneven dispersion of solid flame retardants, and do not solve the problem of migration of liquid flame retardants, which will lead to poor flame retardant effect and the problem of decreased flame retardant effect over time. At the same time, the decomposition and combustion temperature characteristics of the foam substrate are not considered to design the temperature gradient flame retardant, which may lead to deterioration of flame retardancy in practical applications. Patent CN117467104A announced the use of low decomposition temperature flame retardants and high decomposition temperature flame retardants for flame retardancy. Although the patent does not solve the problem of migration of liquid flame retardants and dispersion of solid flame retardants, it has taken into account the problem of temperature gradient flame retardancy, but it ignores the flame retardancy of the material in the middle of combustion. In summary, the current design and preparation of flame retardants are still mainly limited to physical mixing of traditional flame retardant compounds, lack of consideration of synergistic flame retardancy in the full decomposition temperature range of the material, and thus it is difficult to achieve true flame retardancy. In the real environment, the flame retardant performance often decreases with the extension of time, and the performance of the material deteriorates, such as foam and dimensional instability, and the strength, waterproofness and thermal insulation of the material deteriorate. Summary of the invention
[0003] The purpose of the present invention is to overcome the defects of the above-mentioned prior art, and to provide a high-efficiency composite flame retardant for thermosetting polymer foaming resin, and a preparation method and application thereof. The flame retardant prepared by the present invention takes into account low temperature, medium temperature and high temperature full-time flame retardancy, and realizes the flame retardancy of polymer materials to reach A2 level. At the same time, the flame retardant and the resin have good compatibility, are evenly dispersed in the material, the liquid flame retardant is not easy to migrate in the molding material, and the solid flame retardant has stable performance, thereby being able to extend the flame retardant life. In addition, the molding material has stable foam and size, and excellent material strength, waterproofness and thermal insulation.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0005] A high-efficiency composite flame retardant for thermosetting polymer foaming resin, the flame retardant includes component A and component B, by weight percentage, the component A is a low-temperature gas phase flame retardant, the component B includes a medium-temperature expansion flame retardant, a high-temperature skeleton flame retardant, an active hydrogen-containing flame retardant, and fluorosilicone, and the proportions of each component by weight percentage are as follows:
[0006]
[0007] Preferably, the low-temperature gas phase flame retardant includes one or more of chlorinated paraffin, tris(2-chloropropyl) phosphate, tris(β-chloroethyl) phosphate, dimethyl methylphosphonate and diethyl ethylphosphonate. The low-temperature gas phase flame retardant has a decomposition temperature below 250°C and is a liquid flame retardant that is compounded into a polymer resin.
[0008] Preferably, the medium-temperature intumescent flame retardant includes one or more of expandable graphite, graphene oxide, aluminum hydroxide, magnesium hydroxide, ammonium polyphosphate, melamine, melamine cyanurate, melamine phosphate, aluminum diethylphosphinate, poly-2,6-dibromophenyl ether, decabromodiphenyl ether, decabromodiphenyl ethane, brominated polyethylene, borax decahydrate, and zinc borate. The expansion and decomposition temperature of the medium-temperature intumescent flame retardant is 250°C-550°C, and it is a solid flame retardant.
[0009] Preferably, the high-temperature skeleton-type flame retardant includes one or more of silicon dioxide, lead dioxide, antimony trioxide, ferric oxide, calcium carbonate, barium borate, barium sulfate, low-temperature glass powder, low-temperature ceramic powder, and machine-made sand; the high-temperature skeleton-type flame retardant has a temperature tolerance of above 550°C and is a solid flame retardant.
[0010] Preferably, the active hydrogen-containing flame retardant is one or two selected from hexa(4-DOPOhydroxymethylphenoxy)-cyclotriphosphazene and hexa(4-aminophenoxy)cyclotriphosphazene.
[0011] Preferably, the fluorosilicone is a hydroxyl-terminated fluorosilicone, and its structure is as follows:
[0012]
[0013] Wherein, the degree of polymerization n is greater than 5000.
[0014] Preferably, the preparation method of component B is as follows:
[0015] Add medium-temperature expansion flame retardant and high-temperature skeleton flame retardant according to weight percentage in a mixing tank with double-layer stirring, stir and mix at room temperature for 30-60 minutes, and then spray the mixture containing active hydrogen flame retardant, alcohol and fluorosilicone at a uniform speed under stirring for 30-60 minutes. After the spraying is completed, continue stirring for 30-60 minutes, and then recover the alcohol by reduced pressure distillation. When 90-95% of the alcohol is recovered, the material is discharged to obtain the component B.
[0016] Preferably, the mass proportions of the components of the mixed solution are as follows:
[0017] Fluorosilicone 0.3-2%, industrial alcohol 90-97.7%, active hydrogen flame retardant 2-8%.
[0018] The high-efficiency composite flame retardant of the invention is applied to thermosetting polymer resin foaming, including phenolic resin foaming, polyurethane resin foaming and synthetic resin foaming.
[0019] Compared with the prior art, the present invention has the following advantages and effects:
[0020] The high-efficiency composite flame retardant provided by the present invention includes a low-temperature gas phase flame retardant, a medium-temperature expansion flame retardant, a high-temperature skeleton flame retardant, an active hydrogen-containing flame retardant and fluorosilicone. The effective decomposition range of the decomposition product of the flame retardant is 150-800°C, wherein the decomposition temperature of the low-temperature gas phase flame retardant is below 250°C, the decomposition temperature of the medium-temperature expansion flame retardant is 250-550°C, and the tolerance temperature of the high-temperature skeleton flame retardant is above 550°C, thereby achieving the gradient synergistic flame retardancy of various flame retardants in different temperature zones. During the combustion process of the thermosetting polymer foam material, its flame retardant mechanism is as follows: ① The gas phase flame retardant in the low-temperature zone decomposes when heated, and absorbs a large amount of heat released by the free radical chain reaction of the foam material during the decomposition process, and produces a large amount of inert gas and water vapor, which reduces the temperature of the combustion surface of the material and dilutes the concentration of the combustible gas, making it difficult for the temperature of the combustion surface of the material and the concentration of the combustible gas to meet the requirements of the ignition point. ② The expansion flame retardant in the medium temperature zone works synergistically, expands when exposed to fire, and continuously forms a porous isolation layer that is difficult to burn, which can insulate heat and oxygen, inhibit smoke, weaken and gradually terminate the free radical chain reaction. ③ The skeleton flame retardant in the high temperature zone is mostly an inorganic filler with a large specific heat capacity. Through its heat storage and heat conduction effects, the material is not easy to reach the decomposition temperature when exposed to fire. At the same time, it condenses with the decomposition residues of the flame retardant in the medium and low temperature zones to form a material skeleton, enhancing the fire resistance of the material.
[0021] (2) The high-efficiency composite flame retardant provided by the present invention, wherein the temperature expansion type flame retardant and the high-temperature skeleton type flame retardant are surface-modified by terminal hydroxyl fluorosilicone. Since the terminal hydroxyl fluorosilicone has a flexible terminal hydroxyl structure, the fluorosilicone will be uniformly adsorbed on the surface of the flame retardant and is not easy to migrate. At the same time, the fluorosilicone also gives the solid flame retardant low surface free energy. This can achieve the following properties: ① Improve the compatibility of solid flame retardants and polymer materials, so that solid flame retardants are evenly dispersed in polymer materials, and at the same time, liquid flame retardants can slowly migrate to fluorosilicone, preventing its migration and loss, and improving the stability and life of flame retardants; ② Fluorosilicone maintains the stability of the foaming material, improving its water resistance and mechanical properties; ③ Fluorosilicone encapsulation greatly reduces the decomposition rate of flame retardants, increases the amount of carbon deposits in foam materials after heating, and improves the flame retardant time of flame retardants; ④ After high-temperature decomposition of fluorosilicone, a layer of flaky silicon dioxide is covered on the surface of the residual carbon, hindering the transfer of substances and heat; ⑤ Solid flame retardants modified with fluorosilicone are easy to migrate to the surface of foam materials at high temperatures, thereby improving the flame retardant effect of flame retardants. ⑥ Fluorosilicone encapsulation of solid flame retardants can prevent powder flame retardants such as polyphosphates, aluminum hydroxide, etc. from reacting with acidic or alkaline substances in the environment, thereby improving the life of flame retardants.
[0022] (3) Phosphate-type flame retardants containing active hydrogen are used, such as hexa(4-DOPO hydroxymethylphenoxy)-cyclotriphosphazene and hexa(4-aminophenoxy)cyclotriphosphazene. This type of flame retardant reacts during the mixing process with the thermosetting polymer resin, preventing the migration of liquid gas-phase flame retardant in the molding material and ensuring the long-term fire resistance. At the same time, a continuous, uniform and dense expanded carbon layer can be formed during the heating process, thereby improving the flame retardant effect.
[0023] (4) The high-efficiency composite flame retardant of the present invention is applied to thermosetting polymer foam materials to achieve temperature gradient synergistic flame retardancy, thereby improving the fire resistance grade of the foam materials from Class B to Class A without substantially affecting the original excellent performance of the materials. Both the energy-saving effect and the fire resistance performance can meet the current urgent needs of the industry, and have broad prospects for promotion and application. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] A high-efficiency composite flame retardant for thermosetting polymer foaming resin, comprising component A and component B, wherein component A is a low-temperature gas phase flame retardant, and a preparation method of component B comprises the following steps:
[0027] 9 g of expandable graphite, 1 g of graphene oxide, 10 g of melamine, 10 g of ammonium polyphosphate, 10 g of decabromodiphenylethane, 60 g of lead dioxide and 60 g of barium sulfate were added to a mixing tank with double-layer stirring, and the mixture was stirred at room temperature for 30 min. Then, a mixed solution of 8 g of hexa(4-DOPOhydroxymethylphenoxy)-cyclotriphosphazene, 90 g of industrial alcohol and 2 g of hydroxy-terminated fluorosilicone was uniformly sprayed into the mixture under stirring. The spraying time was 30 min. After the spraying was completed, stirring was continued for 30 min. After that, the material was discharged to obtain component B when 90% of the alcohol was recovered by reduced pressure distillation.
[0028] Example 2
[0029] A high-efficiency composite flame retardant for thermosetting polymer foaming resin, comprising component A and component B, wherein component A is a low-temperature gas phase flame retardant, and a preparation method of component B comprises the following steps:
[0030] 9 g of expandable graphite, 1 g of graphene oxide, 10 g of aluminum hydroxide, 10 g of melamine phosphate, 10 g of decabromodiphenyl ether, 60 g of antimony trioxide and 60 g of ferric oxide were added to a mixing tank with double-layer stirring, and the mixture was stirred for 60 min at room temperature. Then, under stirring, a mixed solution of 3.4 g of hexa(4-aminophenoxy)cyclotriphosphazene, 96.09 g of industrial alcohol and 0.51 g of hydroxy-terminated fluorosilicone was uniformly sprayed into the mixture for 30 min. After the spraying was completed, stirring was continued for 60 min. After that, the B component was obtained by discharging the material when 95% of the alcohol was recovered by reduced pressure distillation.
[0031] Example 3
[0032] A high-efficiency composite flame retardant for thermosetting polymer foaming resin, comprising component A and component B, wherein component A is a low-temperature gas phase flame retardant, and a preparation method of component B comprises the following steps:
[0033] In a mixing tank with a double-layer stirrer, 10 g of magnesium hydroxide, 10 g of ammonium polyphosphate, 10 g of melamine cyanurate, 10 g of polyethylene bromide and 120 g of silicon dioxide were added and stirred at room temperature for 30 min. Then, under stirring, a mixture of 8 g of hexa(4-DOPOhydroxymethylphenoxy)-cyclotriphosphazene, 90 g of industrial alcohol and 2 g of hydroxy-terminated fluorosilicone was uniformly sprayed into the mixture for 30 min. After the spraying, stirring was continued for 30 min. After that, the B component was obtained by discharging the material when 90% of the alcohol was recovered by reduced pressure distillation.
[0034] Example 4
[0035] A high-efficiency composite flame retardant for thermosetting polymer foaming resin, comprising component A and component B, wherein component A is a low-temperature gas phase flame retardant, and a preparation method of component B comprises the following steps:
[0036] 9 g of expandable graphite, 1 g of graphene oxide, 10 g of melamine phosphate, 10 g of poly-2,6-dibromophenyl ether, 10 g of aluminum diethylphosphinate and 120 g of silicon dioxide were added to a mixing tank with double-layer stirring, and the mixture was stirred and mixed at room temperature for 30 min. Then, under stirring, a mixed solution of 8 g of hexa(4-DOPOhydroxymethylphenoxy)-cyclotriphosphazene, 90 g of industrial alcohol and 2 g of hydroxy-terminated fluorosilicone was uniformly sprayed into the mixture for 30 min. After the spraying was completed, stirring was continued for 30 min. After that, the B component was obtained by discharging the material when 90% of the alcohol was recovered by reduced pressure distillation.
[0037] Example 5
[0038] A high-efficiency composite flame retardant for thermosetting polymer foaming resin, comprising component A and component B, wherein component A is a low-temperature gas phase flame retardant, and a preparation method of component B comprises the following steps:
[0039] In a mixing tank with a double-layer stirrer, 10 g of melamine cyanurate, 10 g of ammonium polyphosphate, 10 g of decabromodiphenyl ether, 10 g of aluminum hydroxide, 60 g of ferric oxide and 60 g of calcium carbonate were added and stirred at room temperature for 30 min. Then, a mixed solution of 4 g of hexa(4-DOPO hydroxymethylphenoxy)-cyclotriphosphazene and 2 g of hexa(4-aminophenoxy)cyclotriphosphazene, 93 g of industrial alcohol and 1 g of hydroxy-terminated fluorosilicone was uniformly sprayed into the mixture under stirring. The spraying time was 30 min. After the spraying was completed, stirring was continued for 30 min. After that, the B component was obtained when 90% of the alcohol was recovered by reduced pressure distillation.
[0040] Example 6
[0041] A high-efficiency composite flame retardant for thermosetting polymer foaming resin, comprising component A and component B, wherein component A is a low-temperature gas phase flame retardant, and a preparation method of component B comprises the following steps:
[0042] 9 g of expandable graphite, 1 g of graphene oxide, 10 g of magnesium hydroxide, 10 g of polyethylene bromide, 10 g of melamine, 60 g of lead dioxide and 60 g of barium sulfate were added to a mixing tank with double-layer stirring, and the mixture was stirred at room temperature for 30 min. Then, a mixed solution of 8 g of hexa(4-DOPOhydroxymethylphenoxy)-cyclotriphosphazene, 90 g of industrial alcohol and 2 g of hydroxy-terminated fluorosilicone was uniformly sprayed into the mixture under stirring. The spraying time was 30 min. After the spraying was completed, stirring was continued for 30 min. After that, the B component was obtained by discharging the material when 90% of the alcohol was recovered by reduced pressure distillation.
[0043] The following are examples of the application of the flame retardant in the above embodiment:
[0044] Application Example 1
[0045] A polymer composite foam material comprises a polymer foam material and a composite flame retardant, wherein the polymer foam material is a polyurethane foam material, component B in the composite flame retardant is the high-efficiency flame retardant of Example 1, and component A is chlorinated paraffin. The mass ratio of the polyurethane foam material, the flame retardant component A and the component B is 30:2:68.
[0046] The polyurethane foam material is prepared from the following raw materials in a mass ratio: 100 parts of polyether polyol, 4 parts of triethylenediamine A33, 22 parts of foaming agent 141b, 4 parts of silicone oil 6950, and 160 parts of isocyanate MDI.
[0047] The preparation of the polyurethane composite foam material is as follows: polyether polyol, triethylene diamine, foaming agent 141b, silicone oil, flame retardant component A and 2 / 5 of composite flame retardant component B are mixed evenly, and isocyanate MDI and 3 / 5 of composite flame retardant component B are mixed evenly. Then the two mixtures are stirred for 15 seconds under a high-speed disperser, poured into a mold, and after closing the mold for 10 minutes, the polyurethane foam is aged at 50°C for 4 hours.
[0048] Application Example 2
[0049] A polymer composite foam material, comprising a polymer foam material and a composite flame retardant, wherein the polymer foam material is a polyurethane foam material, component B in the composite flame retardant is the high-efficiency flame retardant of Example 2, and component A is tris(2-chloropropyl) phosphate. The mass ratio of the polyurethane foam material, the flame retardant component A, and the component B is 26.5:1.5:72.
[0050] The composition and preparation of the polyurethane composite foam material are the same as those in Application Example 1.
[0051] Application Example 3
[0052] A polymer composite foam material comprises a polymer foam material and a composite flame retardant, wherein the polymer foam material is a polyurethane foam material, component B in the composite flame retardant is the high-efficiency flame retardant of Example 3, and component A is tris(β-chloroethyl) phosphate. The mass ratio of the polyurethane foam material, the flame retardant component A and the component B is 23:1:76.
[0053] The composition and preparation of the polyurethane composite foam material are the same as those in Application Example 1.
[0054] Application Example 4
[0055] A polymer composite foam material comprises a polymer foam material and a composite flame retardant, wherein the polymer foam material is a phenolic foam material, component B in the composite flame retardant is the high-efficiency flame retardant of Example 4, and component A is dimethyl methylphosphonate. The mass ratio of the phenolic foam material, the flame retardant component A and the component B is 30:2:68.
[0056] The phenolic foam material is prepared from the following raw materials in a mass ratio: 100 parts of resol phenolic resin, 4 parts of silicone oil, 8 parts of n-pentane and 8 parts of p-toluenesulfonic acid.
[0057] The preparation of the polymer composite foam material is as follows: weigh the raw materials according to the above weight ratio, mix the phenolic resin, silicone oil, n-pentane, p-toluenesulfonic acid, flame retardant component A and flame retardant component B evenly under high-speed stirring, inject them into the mold, expand and foam at 60°C, and solidify and demold to obtain the composite foam material.
[0058] Application Example 5
[0059] A polymer composite foam material comprises a polymer foam material and a composite flame retardant, wherein the polymer foam material is a phenolic foam material, component B in the composite flame retardant is the high-efficiency flame retardant of Example 5, and component A is diethyl ethylphosphonate. The mass ratio of the phenolic foam material, the flame retardant component A and the component B is 26.5:1.5:72.
[0060] The composition and preparation of the phenolic composite foam material are the same as those in Application Example 4.
[0061] Application Example 6
[0062] A polymer composite foam material, comprising a polymer foam material and a composite flame retardant, wherein the polymer foam material is a phenolic foam material, component B in the composite flame retardant is the high-efficiency flame retardant of Example 6, and component A is chlorinated paraffin, tris(2-chloropropyl) phosphate and dimethyl methylphosphonate (mass ratio 1:2:2). The mass ratio of the phenolic foam material, the flame retardant component A and the component B is 23:1:76.
[0063] The composition and preparation of the phenolic composite foam material are the same as those in Application Example 4.
[0064] Performance evaluation experiment: The polymer composite foam materials obtained in the above application examples 1 to 6 were subjected to performance tests, and the test results are shown in the following table. As can be seen from the table, the flame retardant grade of all polymer composite foam materials can reach A2 level, and other indicators meet the requirements.
[0065] Table 1 Performance evaluation table of two materials
[0066]
[0067]
[0068] Note: * Flame retardancy testing is based on the method specified in the national standard GB8624-2012. The A2 level of non-flammability test is determined by mass loss ≤ 50%, temperature rise in the furnace ≤ 50°C, and continuous burning time ≤ 20s.
[0069] It can be seen from the table that the overall density of the polyurethane and phenolic composite foam materials made of the flame retardant prepared by the present invention is ≥90kg / m 3 , compression strength ≥ 0.1MPa, good mechanical strength, can pass the non-combustibility test of GB 8624-2012 "Classification of Combustion Performance of Building Materials and Products", the mass loss is less than 50%, the temperature rise in the furnace is less than 50℃, and the open flame time is less than 20 seconds.
[0070] This technology can also be applied to flame retardant applications of other thermosetting composite resins.
[0071] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modification or improvement made without departing from the spirit of the present invention belongs to the scope of protection claimed in the present invention.
Claims
1. A high-efficiency composite flame retardant for thermosetting polymer foaming resin, characterized in that: The flame retardant includes component A and component B, wherein component A is a low-temperature gas phase flame retardant, and component B includes a medium-temperature expansion flame retardant, a high-temperature skeleton flame retardant, an active hydrogen-containing flame retardant and fluorosilicone, and the weight percentage of each component is as follows:
2. The high-efficiency composite flame retardant according to claim 1, characterized in that: The low-temperature gas phase flame retardant is one or more of chlorinated paraffin, tris(2-chloropropyl) phosphate, tris(β-chloroethyl) phosphate, dimethyl methylphosphonate and diethyl ethylphosphonate.
3. The high-efficiency composite flame retardant according to claim 1, characterized in that: The medium-temperature intumescent flame retardant is one or more of expandable graphite, graphene oxide, aluminum hydroxide, magnesium hydroxide, ammonium polyphosphate, melamine, melamine cyanurate, melamine phosphate, aluminum diethylphosphinate, poly-2,6-dibromophenyl ether, decabromodiphenyl ether, decabromodiphenyl ethane, brominated polyethylene, borax decahydrate and zinc borate.
4. The high-efficiency composite flame retardant according to claim 1, characterized in that: The high-temperature skeleton-type flame retardant is one or more of silicon dioxide, lead dioxide, antimony trioxide, ferric oxide, calcium carbonate, barium borate, barium sulfate, low-temperature glass powder, low-temperature ceramic powder, and machine-made sand.
5. The high-efficiency composite flame retardant according to claim 1, characterized in that: The active hydrogen-containing flame retardant is one or two of hexa(4-DOPO hydroxymethylphenoxy)-cyclotriphosphazene and hexa(4-aminophenoxy)cyclotriphosphazene.
6. The high-efficiency composite flame retardant according to claim 1, characterized in that: The fluorosilicone is a hydroxyl-terminated fluorosilicone, and its structure is as follows: Wherein, the degree of polymerization n is greater than 5000.
7. The high-efficiency composite flame retardant according to claim 1, characterized in that: The preparation method of the component B is as follows: adding a medium-temperature expansion flame retardant and a high-temperature skeleton flame retardant according to weight percentage into a mixing tank with a double-layer stirrer, stirring and mixing at room temperature for 30-60 minutes, and then spraying a mixed liquid containing an active hydrogen flame retardant, alcohol, and fluorosilicone at a uniform speed under stirring for 30-60 minutes. After the spraying is completed, stirring is continued for 30-60 minutes, and then the alcohol is recovered by reduced pressure distillation. When 90-95% of the alcohol is recovered, the material is discharged to obtain the component B.
8. The high-efficiency composite flame retardant according to claim 7, characterized in that: The mass proportions of the components of the mixed liquid are as follows: 0.3-2% fluorosilicone, 90-97.7% industrial alcohol, and 2-8% active hydrogen-containing flame retardant.
9. The use of the high-efficiency composite flame retardant according to claim 1, characterized in that: It is used in thermosetting polymer resin foaming, including phenolic resin foaming, polyurethane resin foaming, melamine resin foaming and synthetic resin foaming.
Citation Information
Patent Citations
Preparation method of ammonium polyphosphate wrapped with fluorine-containing silicone oil on surface
CN104479172A
Preparation method of flame-retardant and anti-smelting dripping polyester material and flame-retardant and anti-smelting dripping polyester
CN107245228A
Fluorine-containing silicone oil and fluorine-containing flame retardant prepared from fluorine-containing silicone oil
CN115850707A
Hard flame-retardant polyurethane foam and preparation method thereof
CN116515070A
Composite flame retardant and polymer composite foam material
CN116656005A
Cited By
Fireproof fiber composite board and preparation method thereof
CN120840167A