Environment-friendly base digital printing plate and preparation method thereof

By setting a back coating on the back surface of the base material of the digital printing board and using environmentally friendly resin, warping and environmental protection problems are solved, production efficiency and durability are improved, and high-quality digital printing board production is achieved.

CN118978822AActive Publication Date: 2024-11-19ANHUI SENTAI WPC TECH FLOOR CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410935211.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-19
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

Existing digital printed boards are prone to warping problems during use, and traditional PVC substrates have environmental protection and safety risks, making it difficult to control reverse warping, resulting in low production efficiency and reduced yield.

Method used

The back coating is provided on the back surface of the substrate, and the base resin is replaced with a biodegradable resin or polyolefin resin. Each layer is formed by photocuring the resin, balance the shrinkage stress of the coating, and optimize the process flow to improve flatness and durability .

Benefits of technology

It effectively solves the problem of floor warpage, improves production efficiency and yield, reduces the risk of environmental pollution, and enhances the durability and flatness of the board.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978822A_ABST
    Figure CN118978822A_ABST
Patent Text Reader

Abstract

The invention relates to an environment-friendly digital printing plate and a preparation method thereof. Belongs to the technical field of digital printing boards. The environment-friendly digital printing plate comprises a base material, a primer layer, a pattern layer, a three-dimensional effect layer and a finish paint layer, a back coating is also arranged on the back surface of the base material; basic resin of the base material is biodegradable resin or polyolefin resin; the primer layer, the pattern layer, the three-dimensional effect layer, the finishing coat layer and the back coating layer are all formed by light-cured resin. Relatively environment-friendly resin is adopted, so that the potential safety hazard of a PVC base material is solved; the bottom of the base material is subjected to back coating, the back coating layer is formed after curing, and therefore the problem that the floor is prone to warping is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a digital printing plate, in particular to an environmentally friendly digital printing plate and a preparation method thereof, belonging to the technical field of digital printing plates. Background Art

[0002] Digital printing board is an upgraded product of traditional SPC stone plastic floor. With its unique technical advantages, it has a broad market prospect. The production of traditional SPC stone plastic floor requires hot pressing and laminating PVC color film on the stone plastic substrate. PVC color film needs to be ordered. When producing different styles of floor, different types of color film need to be purchased. In order to ensure the production of floor, more color film is often ordered, which results in a large amount of inventory. Digital printing board can directly print the required pattern on the floor, so there will be no inventory problem of color film.

[0003] The relevant prior art is introduced as follows.

[0004] CN112739463A discloses a method and apparatus for producing a surface structure, comprising the following steps: A) applying resin A to the surface of a material; B) when the resin A is in a liquid state or partially solidified, applying liquid B to at least a portion of the resin A; C) polymerizing the resin A and the liquid B separately; D) removing the polymerized liquid B to produce a three-dimensional structure.

[0005] CN110773403A discloses a 3D printing plate with a surface brushing effect, the structure of which is a base layer, a UV primer layer, a UV white paint layer, a UV transition paint layer, a color pattern layer, a UV wear-resistant paint, a 3D texture layer, and a UV topcoat layer from bottom to top. A flatbed inkjet printer is used to spray varnish on the uncured UV wear-resistant paint surface, and the position of the varnish corresponds to the pattern texture position of the color pattern layer; after printing is completed, the printer is dried and cured by the LED built into the printer; at this time, the cured part is limited to the part not covered by the varnish, and the wear-resistant paint of the part covered by the varnish is not cured; then a wood grain drawing machine is used to draw the uncured printed parts in the 3D texture, so as to obtain a 3D texture layer.

[0006] The floor made by the above method is prone to warping during use.

[0007] In the prior art, in order to solve the problem of floor warping, the substrate is pre-made with a certain reverse warping degree, thereby solving the problem of floor warping in the later stage. However, the technical window of reverse warping degree is narrow, and it must be sufficiently precise, otherwise it is easy to cause problems such as large floor tiles and back tiles exceeding the limit, resulting in a decrease in the yield rate. Moreover, the reverse warping degree of the substrate is also difficult to control, resulting in low production efficiency.

[0008] In addition, the digital printing sheets in the existing technology usually use polyvinyl chloride resin (PVC) as the main resin of the base material, in which the PVC content is usually above 90%. Although PVC has advantages such as good mechanical properties and low cost, it also has some problems. 1. Environmental issues: PVC materials contain halogens, which may release harmful substances during their production and use, causing pollution to the environment; 2. Application restrictions: PVC sheets are easy to deform at high temperatures, which limits their application in certain scenarios; 3. Risk of combustion toxic gas: PVC will produce toxic gases and thick smoke when burning, posing a safety hazard. Summary of the invention

[0009] The present invention aims to solve the above problems, thereby providing an environmentally friendly digital printing plate; the digital printing plate of the present invention solves the problem of easy warping by providing a back coating on the back surface of the substrate.

[0010] The technical solution of the present invention to solve the above problems is as follows: An environmentally friendly digital printing plate material comprises at least a substrate, a primer layer, a pattern layer, a three-dimensional effect layer and a topcoat layer in order from bottom to top; a back coating layer is also provided on the back surface of the substrate; the substrate is mainly composed of a base resin and a filler, the base resin is a biodegradable resin or a polyolefin resin; the filler is at least one of a mineral filler or a plant filler; the primer layer, the pattern layer, the three-dimensional effect layer, the topcoat layer and the back coating layer are all formed by a photocurable resin; the primer layer comprises a first adhesion layer covering the surface of the substrate and a first primer layer covering the surface of the first adhesion layer; the back coating layer covers a second adhesion layer on the back surface of the substrate and a second primer layer covering the surface of the second adhesion layer.

[0011] In the above technical solution of the present invention, by providing a back coating on the back surface of the substrate, the shrinkage stress formed by the coatings on both sides of the substrate during the curing process is balanced to a certain extent, thereby effectively solving the problem of warping of the floor during use.

[0012] In the above technical solution of the present invention, the base resin of the substrate is also replaced with a biodegradable resin or a polyolefin resin, such as polylactic acid, etc., thereby eliminating the potential risks of polyvinyl chloride.

[0013] As a preferred embodiment of the above technical solution, the surface hardness of the plate is not less than Shore hardness 90HD.

[0014] As a preferred embodiment of the above technical solution, the thickness of the three-dimensional effect layer is 100~300μm; the thickness of the primer layer is 10~50μm; the thickness of the pattern layer is 8~30μm; and the thickness of the back coating layer is 20~100μm.

[0015] Another object of the present invention is to provide a method for preparing the digital printing plate.

[0016] A method for preparing an environmentally friendly digital printing plate comprises the following steps: S1. providing a substrate; S2, pre-treating the surface to be decorated and the back surface of the substrate; S3, coating an adhesion primer on one surface of the substrate, and curing it under light to form a first adhesion layer; S4, coating a primer on the surface of the first adhesion layer, and curing the primer by light to form a primer layer; S5, using an industrial printer to print ink on the surface of the primer layer, and curing it under light to form a pattern layer; S6, coating a light-curing resin on the surface of the pattern layer; S7, spray-printing an inhibitor containing a polymerization inhibitor and / or a UV absorbing agent using a 3D printer; S8, light curing; S9. Treat the surface with a metal brush roller to remove the paste that has not been completely cured; S10, cleaning the surface and then drying; S11, applying topcoat and curing by light; S12, turning the substrate over, applying an adhesive primer to the back surface of the substrate, and curing the substrate under light to form a second adhesive layer; S13, coating a primer on the surface of the second adhesion layer, and curing the primer under light to form a back coating layer; S14. Press the coated sheet flat at 80-90°C for 8-20 hours to enhance the flatness and durability of the sheet; S15. Place flat at room temperature for 16 to 48 hours.

[0017] In the above technical scheme of the present invention, firstly, by pre-treating the substrate, the surface flatness is ensured and the dimensional accuracy and quality consistency are improved; secondly, the entire process flow is optimized, including extrusion, grinding, printing, back coating, tempering and other processes, thereby improving production efficiency and yield rate.

[0018] In the above technical solution of the present invention, durability refers to the ability of the floor to maintain its flatness during long-term use or placement.

[0019] As a preferred embodiment of the above technical solution, in step S14, the pressure of the flattening is controlled at 2.0-8.0 MPa.

[0020] As a preferred embodiment of the above technical solution, in step S14, the pressure of the flattening is controlled at 2.0-5.0 MPa.

[0021] As a preferred embodiment of the above technical solution, the base resin of the substrate is polyolefin and the filler is calcium carbonate.

[0022] As a preferred embodiment of the above technical solution, the pretreatment is a grinding treatment. Furthermore, the grinding treatment is performed by using a sanding machine. Furthermore, the grinding roller of the sanding machine is elastically set so that the sanding belt and the substrate maintain a contact pressure of 0.05-0.2 MPa.

[0023] As a preferred embodiment of the above technical solution, in step S3, the adhesion primer includes the following components in parts by weight: Multifunctional acrylate monomer 35~55 Pure acrylate 10~15 Talc 10~20 Fumed silica 0.1~0.5 Photoinitiator 0.5~0.8 Reactive diluent 15~25.

[0024] In the above technical solution of the present invention, the adhesion primer is transparent and has a certain filling effect, which not only improves the adhesion of the subsequent coating, but also fills the pitted surface of the substrate under the microscopic after grinding, making the substrate surface smoother, thereby improving the accuracy of the subsequent coating.

[0025] As a preferred embodiment of the above technical solution, in steps S4 and S13, the primer includes the following components in parts by weight: Epoxy acrylate 45~55 Polyurethane acrylate 10~15 Titanium dioxide 25~35 Photoinitiator 0.3~0.8 Reactive diluent 15~25.

[0026] In the above technical solution of the present invention, the addition of titanium dioxide can improve the whiteness of the primer and the hiding power, thereby covering the color of the substrate and avoiding the influence of the apparent quality of the product due to the change of the color saturation of the substrate color.

[0027] As a preferred embodiment of the above technical solution, in step S5, the ink used by the industrial printer is a photocurable color paste.

[0028] As a preferred embodiment of the above technical solution, in step S6, the photocurable resin includes the following components in parts by weight: Epoxy acrylate 70~90 Photoinitiator 0.3~0.8 Reactive diluent 10~15.

[0029] In the above technical solution of the present invention, the film-forming substance is epoxy acrylate, which has the advantage of high surface hardness after light curing and is suitable for use as the surface layer of the board.

[0030] As a further preferred embodiment of the above technical solution, in step S6, the photocurable resin further includes 5 to 15 parts by mass of nano α-aluminum oxide.

[0031] In the above technical solution of the present invention, the addition of nano α-alumina can further improve the wear resistance of the plate.

[0032] In summary, the present invention has the following beneficial effects: 1. The present invention adopts relatively environmentally friendly resin to solve the potential safety hazards of PVC substrate; 2. The present invention performs back coating on the bottom of the substrate, and forms a back coating after curing, thereby solving the problem of the floor being easy to warp; 3. After printing, back coating and curing, the present invention also performs a tempering treatment on the plate, and appropriately flattens the plate at 85°C, thereby further dissolving the internal stress of the plate, improving the flatness of the plate and the performance of maintaining the flatness; 4. The present invention rationally designs the formula of each coating layer. The film-forming substance of the adhesion primer is multifunctional acrylate monomer and pure acrylate, and the filler is talcum powder; the film-forming substance of the primer is epoxy acrylate and polyurethane acrylate, and the filler is titanium dioxide; the ink used in the industrial printer is a photocurable color paste; the film-forming substance of the three-dimensional effect layer is epoxy acrylate; thereby each layer meets its own functional requirements and significantly improves the paint film quality of the digital printing plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a structural schematic diagram of the environmentally friendly digital printing plate of the present invention; In the figure, 01-substrate, 02-primer layer, 03-pattern layer, 04-three-dimensional effect layer, 05-topcoat layer, 06-back coating layer, 02-1-first adhesion layer, 02-2-first primer layer, 06-1-second adhesion layer, 06-2-second primer layer. DETAILED DESCRIPTION

[0034] The present invention is further explained below in conjunction with the accompanying drawings.

[0035] This specific implementation is only an explanation of the present invention, not a limitation of the present invention. Any changes made by those skilled in the art after reading the specification of the present invention, as long as they are within the scope of the claims, will be protected by the patent law.

[0036] Embodiment 1 An environmentally friendly digital printing plate, such as Figure 1 As shown, from bottom to top, it includes a substrate 01, a primer layer 02, a pattern layer 03, a three-dimensional effect layer 04 and a topcoat layer 05; wherein the back surface of the substrate 01 is also provided with a back coating layer 06. The back coating layer 06 is similar to the primer layer 02, and both include two layers. For example, the primer layer 02 includes a first adhesion layer 02-1 covering the surface of the substrate and a first primer layer 02-2 covering the surface of the first adhesion layer 02-1; the back coating layer 06 includes a second adhesion layer 06-1 covering the back surface of the substrate and a second primer layer 06-2 covering the surface of the second adhesion layer 06-1. The primer layer 02 and the back coating layer 06 are coated and cured using similar formulas, but their respective thicknesses may be different. Generally, the thickness of the primer layer 02 is 10~50μm, while the thickness of the back coating layer 06 is 20~100μm. This is achieved by controlling the respective coating amounts during the process.

[0037] The above-mentioned various coatings, such as primer layer 02, three-dimensional effect layer 04 and topcoat layer 05, are all formed by roller coating of light-curing resin and then light curing. However, the formulas of the respective coatings are different. For example, primer layer 02 mainly considers adhesion, filling and covering, so the formula is divided into two parts, namely, the adhesion primer formula and the covering primer formula. In the adhesion primer formula: the film-forming substance is mainly a combination of multifunctional acrylate monomers and pure acrylates, among which multifunctional acrylate monomers account for the majority; and among the multifunctional acrylate monomers, difunctional is the main one, and a small amount of trifunctional, tetrafunctional and hexafunctional can be contained. The filler is 1250 mesh talcum powder. In the covering primer formula: the film-forming substance is mainly a combination of epoxy acrylate and polyurethane acrylate, among which epoxy acrylate accounts for the majority, and a small amount of UV monomer can also be added; the filler is 600 mesh titanium dioxide. The reactive diluents in each formula can be universal, and hydroxyethyl (meth)acrylate is usually selected. Photoinitiators can also be used universally, and are usually selected with absorption peaks in the UV-A band, such as initiator 184 and TPO.

[0038] Different from the above coating, the pattern layer 03 is formed by inkjet printing with an industrial printer and then solidified. The ink used in the industrial printer is a photocurable color paste, and the film-forming substance is mainly polyurethane acrylate.

[0039] It should be noted that although the 3D effect layer 04 is applied by roller coating, the 3D effect layer 04 is not formed immediately after roller coating. Instead, an industrial printer (3D printer) is required to spray 3D ink containing an inhibitor and / or an ultraviolet absorber on specific parts, so that the parts sprayed with 3D ink are not cured or not completely cured, thus distinguishing them from the cured parts. Then, the uncured or incompletely cured substances can be removed by a wire roller, so as to create a 3D concave-convex effect on the layer, which is the 3D effect layer 04. Figure 1As shown, the surface of the three-dimensional effect layer 04 is uneven.

[0040] The topcoat layer 05 is covered on the three-dimensional effect layer 04. Ideally, Figure 1 As shown; however, in actual operation, there may be inconsistent thickness of the topcoat, which is due to the uneven surface of the three-dimensional effect layer 04.

[0041] In order to improve the environmental friendliness of the product, the substrate 01 adopts an environmentally friendly substrate. Specifically, the substrate 01 is mainly composed of a base resin and a filler. The base resin is a biodegradable resin or a polyolefin resin; the filler is at least one of a mineral filler or a plant filler; in this embodiment, the thickness of the substrate is 5 mm; the base resin of the substrate 01 is HDPE, and the filler is ultrafine calcium carbonate. In this embodiment, the mass ratio of HDPE to ultrafine calcium carbonate is about 1:2.

[0042] The method for preparing the above-mentioned environmentally friendly digital printing plate comprises the following steps: S1, providing a substrate 01; S2, using a sanding machine to grind the surface to be decorated and the back surface of the substrate; the grinding roller of the sanding machine is elastic, so that the sanding belt and the substrate always maintain a contact pressure of 0.05-0.1MPa; S3. Roll-coat the adhesion primer on the upper surface of the substrate in an amount of 8.0 g / ㎡; then cure it with a 395nm UV light to form a first adhesion layer 02-1; the adhesion primer formula is as follows: 35 parts by mass of a difunctional acrylate monomer (1,4-butanediol acrylate), 5 parts by mass of a trifunctional acrylate monomer (pentaerythritol triacrylate), 10 parts by mass of a monofunctional methacrylate monomer (methacrylate), 15 parts by mass of 1250 mesh talc, 5.0 parts by mass of a photoinitiator TPO, 15 parts by mass of a reactive diluent (hydroxyethyl methacrylate), and 0.2 parts by mass of a defoamer; S4, apply a covering primer on the surface of the first adhesion layer 02-1, with a coating amount of 25.0 g / ㎡; then use 395nm UV light to cure to form a first primer layer 02-2; the covering primer formula is as follows: 45 parts by mass of epoxy acrylate, 10 parts by mass of polyurethane acrylate, 15 parts by mass of difunctional acrylate monomer (1,4-butanediol acrylate), 30 parts by mass of 600 mesh titanium dioxide, 5.0 parts by mass of photoinitiator TPO, 20 parts by mass of reactive diluent (hydroxyethyl methacrylate), and 0.2 parts by mass of defoamer; S5, inkjet printing is performed on the surface of the primer layer 02 using an industrial printer, with a spraying amount of 6.0 g / ㎡; light curing is performed to form a pattern layer 03; the ink uses a light-curing color paste, and the film-forming substance is mainly polyurethane acrylate; S6, coating the surface of the pattern layer with a photocurable resin; coating in batches, coating twice; the first coating amount is 80 g / ㎡; then curing with a 395nm UV light; the second coating amount is 150 g / ㎡; in this step, the photocurable resin formula is as follows: 90 parts by mass of epoxy acrylate, 5.0 parts by mass of photoinitiator TPO, 10 parts by mass of reactive diluent (hydroxyethyl methacrylate), and 0.2 parts by mass of defoamer; S7, spray-printing an inhibitor containing a polymerization inhibitor and / or a UV absorbing agent using a 3D printer; S8, then use 395nm UV light to cure; S9. Treat the surface with a wire roller to remove the paste that has not been completely cured; S10, cleaning the surface and then drying; S12, turn over the substrate 01, apply an adhesion primer on the back surface of the substrate 01, and apply a coating amount of 8.0 g / ㎡; then use 395nm UV light to cure to form a second adhesion layer 02-1; the adhesion primer formula is the same as step S3; S13, coating the surface of the second adhesion layer 02-1 with a primer, and curing it with a 395nm UV light to form a back coating layer 06; in this step, the primer formula is as follows: 45 parts by mass of epoxy acrylate, 10 parts by mass of polyurethane acrylate, 15 parts by mass of a difunctional acrylate monomer (1,4-butanediol acrylate), 5.0 parts by mass of a photoinitiator TPO, 10 parts by mass of a reactive diluent (hydroxyethyl methacrylate), and 0.2 parts by mass of a defoamer; S14, flatten the coated sheet at 85°C with a pressure of 2.0 MPa for 12 hours to enhance the flatness and durability of the sheet; S15. Place flat at room temperature for 16 hours.

[0043] Comparative Example 1 An environmentally friendly digital printing plate includes, from bottom to top, a substrate, a primer layer, a pattern layer, a three-dimensional effect layer and a topcoat layer. The primer layer includes a first adhesion layer covering the surface of the substrate and a first primer layer covering the surface of the first adhesion layer. The substrate adopts an environmentally friendly substrate, specifically, the substrate is mainly composed of a base resin and a filler; in this embodiment, the thickness of the substrate is 5 mm; the base resin of the substrate is HDPE, and the filler is ultrafine calcium carbonate. In this embodiment, the mass ratio of HDPE to ultrafine calcium carbonate is about 1:2.

[0044] The method for preparing the above-mentioned environmentally friendly digital printing plate comprises the following steps: S1. Provide a substrate; the thickness of the substrate is 5 mm; S2, using a sanding machine to grind the surface to be decorated and the back surface of the substrate; the grinding roller of the sanding machine is elastic, so that the sanding belt and the substrate always maintain a contact pressure of 0.05-0.1MPa; S3. Roll-coat the adhesion primer on the upper surface of the substrate in an amount of 8.0 g / ㎡; then cure it with a 395nm UV light to form a first adhesion layer 02-1; the adhesion primer formula is as follows: 35 parts by mass of a difunctional acrylate monomer (1,4-butanediol acrylate), 5 parts by mass of a trifunctional acrylate monomer (pentaerythritol triacrylate), 10 parts by mass of a monofunctional methacrylate monomer (methacrylate), 15 parts by mass of 1250 mesh talc, 5.0 parts by mass of a photoinitiator TPO, 15 parts by mass of a reactive diluent (hydroxyethyl methacrylate), and 0.2 parts by mass of a defoamer; S4, apply a covering primer on the surface of the first adhesion layer 02-1, with a coating amount of 25.0 g / ㎡; then use 395nm UV light to cure to form a first primer layer 02-2; the covering primer formula is as follows: 45 parts by mass of epoxy acrylate, 10 parts by mass of polyurethane acrylate, 15 parts by mass of difunctional acrylate monomer (1,4-butanediol acrylate), 30 parts by mass of 600 mesh titanium dioxide, 5.0 parts by mass of photoinitiator TPO, 20 parts by mass of reactive diluent (hydroxyethyl methacrylate), and 0.2 parts by mass of defoamer; S5, inkjet printing is performed on the surface of the primer layer 02 using an industrial printer, with a spraying amount of 6.0 g / ㎡; light curing is performed to form a pattern layer 03; the ink uses a light-curing color paste, and the film-forming substance is mainly polyurethane acrylate; S6, coating the surface of the pattern layer with a photocurable resin; coating in batches, coating twice; the first coating amount is 80 g / ㎡; then curing with a 395nm UV light; the second coating amount is 150 g / ㎡; in this step, the photocurable resin formula is as follows: 90 parts by mass of epoxy acrylate, 5.0 parts by mass of photoinitiator TPO, 10 parts by mass of reactive diluent (hydroxyethyl methacrylate), and 0.2 parts by mass of defoamer; S7, spray-printing an inhibitor containing a polymerization inhibitor and / or a UV absorbing agent using a 3D printer; S8, then use 395nm UV light to cure; S9. Treat the surface with a wire roller to remove the paste that has not been completely cured; S10. Clean the surface and then dry it.

[0045] Comparative Example 2 An environmentally friendly digital printing plate includes, from bottom to top, a substrate, a primer layer, a pattern layer, a three-dimensional effect layer and a topcoat layer. The primer layer includes a first adhesion layer covering the surface of the substrate and a first primer layer covering the surface of the first adhesion layer. The substrate adopts an environmentally friendly substrate, specifically, the substrate is mainly composed of a base resin and a filler; in this embodiment, the thickness of the substrate is 5 mm; the base resin of the substrate is HDPE, and the filler is ultrafine calcium carbonate. In this embodiment, the mass ratio of HDPE to ultrafine calcium carbonate is about 1:2.

[0046] The method for preparing the above-mentioned environmentally friendly digital printing plate comprises the following steps: S1. Provide a substrate; the thickness of the substrate is 5 mm; S2, using a sanding machine to grind the surface to be decorated and the back surface of the substrate; the grinding roller of the sanding machine is elastic, so that the sanding belt and the substrate always maintain a contact pressure of 0.05-0.1MPa; S3. Roll-coat the adhesion primer on the upper surface of the substrate in an amount of 8.0 g / ㎡; then cure it with a 395nm UV light to form a first adhesion layer 02-1; the adhesion primer formula is as follows: 35 parts by mass of a difunctional acrylate monomer (1,4-butanediol acrylate), 5 parts by mass of a trifunctional acrylate monomer (pentaerythritol triacrylate), 10 parts by mass of a monofunctional methacrylate monomer (methacrylate), 15 parts by mass of 1250 mesh talc, 5.0 parts by mass of a photoinitiator TPO, 15 parts by mass of a reactive diluent (hydroxyethyl methacrylate), and 0.2 parts by mass of a defoamer; S4, apply a covering primer on the surface of the first adhesion layer 02-1, with a coating amount of 25.0 g / ㎡; then use 395nm UV light to cure to form a first primer layer 02-2; the covering primer formula is as follows: 45 parts by mass of epoxy acrylate, 10 parts by mass of polyurethane acrylate, 15 parts by mass of difunctional acrylate monomer (1,4-butanediol acrylate), 30 parts by mass of 600 mesh titanium dioxide, 5.0 parts by mass of photoinitiator TPO, 20 parts by mass of reactive diluent (hydroxyethyl methacrylate), and 0.2 parts by mass of defoamer; S5, inkjet printing is performed on the surface of the primer layer 02 using an industrial printer, with a spraying amount of 6.0 g / ㎡; light curing is performed to form a pattern layer 03; the ink uses a light-curing color paste, and the film-forming substance is mainly polyurethane acrylate; S6, coating the surface of the pattern layer with a photocurable resin; coating in batches, coating twice; the first coating amount is 80 g / ㎡; then curing with a 395nm UV light; the second coating amount is 150 g / ㎡; in this step, the photocurable resin formula is as follows: 90 parts by mass of epoxy acrylate, 5.0 parts by mass of photoinitiator TPO, 10 parts by mass of reactive diluent (hydroxyethyl methacrylate), and 0.2 parts by mass of defoamer; S7, spray-printing an inhibitor containing a polymerization inhibitor and / or a UV absorbing agent using a 3D printer; S8, then use 395nm UV light to cure; S9. Treat the surface with a wire roller to remove the paste that has not been completely cured; S10, cleaning the surface and then drying; S11. Press the coated sheet flat at 85°C with a pressure of 2.0 MPa for 12 hours to enhance the flatness and durability of the sheet; S12. Place flat at room temperature for 16 hours.

[0047] In accordance with relevant standards, performance tests were performed on Example 1, Comparative Example 1 and Comparative Example 2, and the results are shown in the following table.

Claims

1. An environmentally friendly digital printing plate, comprising at least a substrate (01), a primer layer (02), a pattern layer (03), a three-dimensional effect layer (04) and a topcoat layer (05) in order from bottom to top; characterized in that: The back surface of the substrate (01) is also provided with a back coating layer (06); the substrate (01) is mainly composed of a base resin and a filler, the base resin is a biodegradable resin or a polyolefin resin; the filler is at least one of a mineral filler or a plant filler; the primer layer (02), the pattern layer (03), the three-dimensional effect layer (04), the topcoat layer (05) and the back coating layer (06) are all formed of a light-curing resin; the primer layer (02) comprises a first adhesion layer (02-1) covering the surface of the substrate and a first primer layer (02-2) covering the surface of the first adhesion layer; the back coating layer (06) comprises a second adhesion layer (06-1) covering the back surface of the substrate and a second primer layer (06-2) covering the surface of the second adhesion layer.

2. The environmentally friendly digital printing plate according to claim 1, characterized in that: The surface hardness of the plate is not less than Shore hardness 90HD.

3. The environmentally friendly digital printing plate according to claim 1, characterized in that: The thickness of the three-dimensional effect layer (04) is 100-300 μm; the thickness of the primer layer (02) is 10-50 μm; the thickness of the pattern layer (03) is 8-30 μm; and the thickness of the back coating layer (06) is 20-100 μm.

4. The method for preparing an environmentally friendly digital printing plate according to any one of claims 1 to 3, comprising the following steps: S1. providing a substrate (01); S2, pre-treating the surface to be decorated and the back surface of the substrate; S3, coating an adhesion primer on one surface of the substrate, and curing it under light to form a first adhesion layer; S4, coating a primer on the surface of the first adhesion layer, and curing the primer layer under light to form a primer layer (02); S5, using an industrial printer to print ink on the surface of the primer layer, and curing it under light to form a pattern layer (03); S6, coating a light-curing resin on the surface of the pattern layer; S7, spray-printing an inhibitor containing a polymerization inhibitor and / or a UV absorbing auxiliary agent using a 3D printer; S8, light curing; S9. Treat the surface with a metal brush roller to remove the paste that has not been completely cured; S10, cleaning the surface and then drying; S11, applying topcoat and curing by light; S12, turning the substrate over, applying an adhesive primer to the back surface of the substrate, and curing the substrate under light to form a second adhesive layer; S13, coating a primer on the surface of the second adhesion layer, and curing it under light to form a back coating layer (06); S14. Press the coated sheet flat at 80-90°C for 8-20 hours to enhance the flatness and durability of the sheet; S15. Place flat at room temperature for 16 to 48 hours.

5. The method for preparing an environmentally friendly digital printing plate according to claim 4, characterized in that: The base resin of the substrate is polyolefin, and the filler is calcium carbonate.

6. The method for preparing an environmentally friendly digital printing plate according to claim 4, characterized in that: The pretreatment is grinding.

7. The method for preparing an environmentally friendly digital printing plate according to claim 4, characterized in that: In step S3, the adhesion primer includes the following components in parts by weight: Multifunctional acrylate monomer 35~55 Pure acrylate 10~15 Talc 10~20 Fumed silica 0.1~0.5 Photoinitiator 0.5~0.8 Reactive diluent 15~25.

8. The method for preparing an environmentally friendly digital printing plate according to claim 4, characterized in that: In steps S4 and S13, the primer includes the following components in parts by mass: Epoxy acrylate 45~55 Polyurethane acrylate 10~15 Titanium dioxide 25~35 Photoinitiator 0.3~0.8 Reactive diluent 15~25.

9. The method for preparing an environmentally friendly digital printing plate according to claim 4, characterized in that: In step S5, the ink used by the industrial printer is a photocurable color paste.

10. The method for preparing an environmentally friendly digital printing plate according to claim 4, characterized in that: In step S6, the photocurable resin includes the following components in parts by weight: Epoxy acrylate 70~90 Photoinitiator 0.3~0.8 Reactive diluent 10~15.

Citation Information

Patent Citations

  • 3D printing plate with surface drawing effect

    CN110773403A

  • Method and apparatus for generating a superficial structure

    CN112739463A

  • Base material for digital printing, digital printing plate and preparation method of digital printing plate

    CN114179465A

  • Preparation method of highlight PET wallboard and wallboard

    CN118002447A